Self-repairing microcapsule, coating, chip and preparation method thereof

By combining modified silica nanoparticles with hydroxy polyether and silane modifiers, self-healing microcapsules with dual repair mechanisms were prepared, which solved the problems of limited loading of repair agents and uneven dispersion in the prior art. , realizes efficient self-repair and good dispersion of the coating, and improves the acid and alkali corrosion resistance and self-repair performance of the chip.

CN119034636AInactive Publication Date: 2024-11-29XIANGFU LABORATORY

Patent Information

Application Number
CN202411514158.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the coating preparation process, the existing self-healing coatings have problems such as limited loading of repair agents and uneven dispersion, which leads to limited self-healing capabilities and affects the performance and uniformity of the coating.

Method used

The modified silica nanoparticles were used to mix with hydroxy polyether, silane modifier and catalyst to prepare microcapsules by adjusting pH and heating reaction, and combined with self-healing polyurethane to form a dual synergistic repair mechanism to achieve self-healing of the coating.

Benefits of technology

It improves the stability, uniformity and dispersion of self-healing microcapsules, enhances the acid and alkali corrosion resistance and self-healing properties of the coating, shortens the crack healing time, and achieves long-term self-healing of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034636A_ABST
    Figure CN119034636A_ABST
Patent Text Reader

Abstract

The invention provides a self-repairing microcapsule, a self-repairing coating, a self-repairing chip and a preparation method of the self-repairing microcapsule. The self-repairing microcapsule prepared by the method provided by the invention has good stability, uniformity, affinity, environmental tolerance and dispersity, and can effectively prevent the agglomeration phenomenon. The coating and the chip provided by the invention comprise the self-repairing polyurethane and the self-repairing microcapsule, and have good acid and alkali corrosion resistance and self-repairing performance, and the self-repairing condition is mild.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material technology, and in particular to a self-repairing microcapsule, a coating and a chip and a preparation method thereof. Background Art

[0002] Optimizing the surface properties of biochips, such as hydrophilicity, adhesion, antibacterial properties, corrosion resistance, self-cleaning properties, etc., can greatly improve their value in practical applications. Coating technology uses physical or chemical techniques to coat special functional materials on the surface, which can not only maintain the inherent characteristics of the base material, but also give the various properties required by the surface, thereby adapting to the special requirements of practical applications. It is a very effective way to modify the surface of the chip. However, during the storage and use of biochips, the coating may be damaged or cracked due to the external environment, which may lead to the decline or even loss of certain functions of the coating, affecting the use of the chip.

[0003] The development of self-healing coatings provides an effective solution to this problem. Self-healing coatings can automatically repair surface cracks without human intervention and restore coating performance, thereby greatly extending the service life of the chip. Since the self-healing coating was proposed, it has received a lot of attention. According to the self-healing mechanism, self-healing coatings are divided into two categories: intrinsic self-healing and external self-healing. Intrinsic self-healing uses the inherent properties of the coating material to achieve self-healing based on the breaking and recombination of covalent bonds. Although multiple repairs can be achieved without the need for additional repair agents, special conditions such as heating, specific frequency light, and specific pH environment are often required to trigger, which is not easy to meet in actual use. External self-healing uses a carrier to carry a repair agent or corrosion inhibitor. When the coating is damaged, the repair agent or corrosion inhibitor is released to repair the damaged area. Among them, self-healing coatings based on microcapsule technology have been widely studied. Microcapsules use chemical or physical methods to encapsulate the repair agent as the core material into tiny capsules. When the coating is damaged, the microcapsule wall material senses external stimuli (external force, corrosive media, pH changes, thermal effects, light effects, etc.) and the shell breaks, releasing the repair agent to repair the cracks. This method relies on the repair agent, which has a limited storage capacity of the repair agent, resulting in limited self-repair ability, and is prone to problems such as uneven dispersion of the repair agent during the coating preparation process, resulting in poor effectiveness and uniformity of the self-repair performance. Summary of the invention

[0004] The present invention provides a method for preparing a self-repairing microcapsule, the preparation method comprising the following steps: (1) Preparing modified silica nanoparticles: mixing silica nanoparticles with hydroxy polyether, silane modifier and catalyst, adjusting the pH to 8-9, heating for reaction; separating the reaction liquid to obtain modified silica nanoparticles; (2) Preparing a prepolymer: reacting an isocyanate solution with 1,4-butanediol to obtain the prepolymer; (3) Preparing microcapsules: dispersing the modified silica nanoparticles prepared in step (1) in water to prepare a modified silica nanoparticle suspension; mixing the prepolymer prepared in step (2) with ethyl acetate and hexamethylene diisocyanate to form an oil phase; adding the oil phase to the modified silica nanoparticle suspension, and then adding 1,4-butanediol to react to obtain microcapsules.

[0005] According to an embodiment of the present invention, in step (1), the hydroxy polyether is selected from one, two or more of polyethylene glycol, polyethylene glycol octylphenyl ether, polytetramethylene glycol ether, etc.

[0006] According to an embodiment of the present invention, in step (1), the silane modifier is selected from one, two or more of isocyanatepropyltriethoxysilane, isocyanatepropyltrimethoxysilane, vinyltriethoxysilane and γ-glycidyloxypropyltrimethoxysilane.

[0007] According to an embodiment of the present invention, in step (1), the catalyst is selected from one, two or more of dibutyltin dilaurate, triphenylbismuth and N,N-dimethylbenzylamine.

[0008] According to an embodiment of the present invention, in step (1), the molar ratio of the silane modifier to the hydroxy polyether is 1:1-1:4, for example, 1:1, 1:2, 1:3, 1:4.

[0009] According to an embodiment of the present invention, in step (1), the molar amount of the catalyst is 0.05%-0.3% of the molar amount of the silane modifier, for example, 0.08%, 0.1%, 0.15%, 0.2%.

[0010] According to an embodiment of the present invention, step (1) is specifically: firstly, hydroxy polyether, silane modifier and catalyst are mixed and reacted, then silicon dioxide nanoparticle solution is added, pH is adjusted to 8-9, and heated to react; the reaction liquid is separated to obtain modified silicon dioxide nanoparticles. Preferably, after the hydroxy polyether, silane modifier and catalyst are mixed, they are heated to react overnight at 40°C. Preferably, the silicon dioxide nanoparticle solution is an ethanol aqueous solution of silicon dioxide nanoparticles; preferably, the volume ratio of ethanol to water in the ethanol aqueous solution is 1:10-10:1, preferably 5:1-10:1, for example 9:1. Preferably, the preparation method of the silicon dioxide nanoparticle solution is: ultrasonically disperse the silicon dioxide nanoparticles into the ethanol aqueous solution. Preferably, the mass volume ratio of the silicon dioxide nanoparticles to the ethanol aqueous solution is 1g:10-30mL, for example 1g:10mL, 1g:15mL, 1g:20mL, 1g:25mL. Preferably, the mass ratio of the mixed reaction liquid of the hydroxy polyether, the silane modifier and the catalyst to the silicon dioxide nanoparticles is 1:5-5:1, for example, 1:3, 1:2, 1:1, 2:1, 3:1.

[0011] According to an embodiment of the present invention, in step (1), aqueous ammonia can be used to adjust the pH to 8-9.

[0012] According to an embodiment of the present invention, in step (1), the temperature of the heating reaction is 60° C.; preferably, the heating reaction time is overnight.

[0013] According to an embodiment of the present invention, after the reaction in step (1) is completed, the reaction solution is centrifuged, and the separated solid is washed with an ethanol aqueous solution and dried to obtain modified silica nanoparticles. Preferably, the volume ratio of ethanol to water in the ethanol aqueous solution is 1:10-10:1, preferably 5:1-10:1, for example 9:1. Preferably, the mixture is dried in an oven at 80°C.

[0014] According to the embodiment of the present invention, step (1) is specifically as follows: hydroxy polyether, silane modifier and catalyst are stirred and mixed uniformly, heated and stirred at 40°C overnight to obtain a mixture; the mixture is added to the silica nanoparticle solution, the pH is adjusted to 8-9 with ammonia water, and heated at 60°C overnight to react; the reaction liquid is centrifuged, the solid is washed with ethanol aqueous solution, and dried in an oven at 80°C to obtain modified silica nanoparticles. Preferably, the mass ratio of the mixture to the silica nanoparticle solution is 1:20-30.

[0015] According to an embodiment of the present invention, in step (2), the isocyanate is selected from one, two or more of toluene diisocyanate, methylene diphenyl diisocyanate, p-phenylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate and the like.

[0016] According to an embodiment of the present invention, in step (2), the isocyanate solution is a solution formed by dissolving isocyanate in cyclohexane. Preferably, the concentration of the isocyanate solution is 0.5 mol / L-5 mol / L, for example, 2 mol / L. Preferably, the volume of the isocyanate solution is 20 mL.

[0017] According to an embodiment of the present invention, in step (2), the molar ratio of isocyanate to 1,4-butanediol is 1:0.1-0.5, for example, 1:0.2, 1:0.3.

[0018] According to an embodiment of the present invention, in step (2), the reaction temperature is 60° C.; preferably, the reaction time is overnight.

[0019] According to an embodiment of the present invention, after the reaction in step (2) is completed, the reaction mixture is distilled under reduced pressure to remove the solvent, thereby obtaining the prepolymer.

[0020] According to an embodiment of the present invention, step (2) is specifically as follows: adding 1,4-butanediol dropwise to the isocyanate solution under stirring, and reacting at 60° C. overnight; after the reaction is completed, distilling the reaction mixture under reduced pressure to remove the solvent, thereby obtaining the prepolymer.

[0021] According to an embodiment of the present invention, in step (3), the mass concentration of the modified silica nanoparticle suspension is 0.5-5%, such as 1%, 2%, 3%, etc.

[0022] According to an embodiment of the present invention, in step (3), the mixing ratio of the prepolymer prepared in step (2) to ethyl acetate and hexamethylene diisocyanate is 1-5:1-5:1-5, for example, 1:1:1 (volume ratio).

[0023] According to an embodiment of the present invention, the amount of 1,4-butanediol used in step (3) is the same as the amount of 1,4-butanediol used in step (2).

[0024] According to an embodiment of the present invention, in step (3), the volume ratio of the oil phase to the modified silica nanoparticle suspension is 1:5-5:1, for example, 1:3, 1:2, 1:1, 2:1, 3:1.

[0025] According to an embodiment of the present invention, in step (3), the reaction temperature is 60° C.; preferably, the reaction time is 2 h.

[0026] According to an embodiment of the present invention, after the reaction in step (3) is completed, the reaction solution is filtered, washed with water, and dried to obtain microcapsules. Preferably, the drying is carried out in an oven at 60°C.

[0027] According to the embodiment of the present invention, step (3) is specifically as follows: dispersing the modified silica nanoparticles prepared in step (1) in water to prepare a modified silica nanoparticle suspension with a mass fraction of 1%; mixing the prepolymer prepared in step (2), ethyl acetate and hexamethylene diisocyanate in a ratio of 1:1:1 to serve as an oil phase; adding the oil phase to the modified silica nanoparticle suspension while stirring, then dropping 1,4-butanediol, heating to 60°C and reacting for 2h; after the reaction is completed, filtering, washing with water, and drying in an oven at 60°C to obtain microcapsules.

[0028] The present invention also provides self-repairing microcapsules prepared by the above preparation method.

[0029] The present invention also provides a self-repairing coating, which comprises the self-repairing microcapsules.

[0030] According to an embodiment of the present invention, the self-repairing coating further comprises self-repairing polyurethane. According to an embodiment of the present invention, the preparation method of the self-repairing polyurethane is: hydroxy polyether and isocyanate are mixed, and then disulfide, catalyst and cross-linking agent are added, and the mixture is mixed and stirred to obtain the self-repairing polyurethane.

[0031] According to an embodiment of the present invention, the hydroxy polyether is selected from one, two or more of polyethylene glycol, polyethylene glycol octylphenyl ether, polytetramethylene ether glycol, etc. According to an embodiment of the present invention, the isocyanate is selected from one, two or more of toluene diisocyanate, methylene diphenyl diisocyanate, p-phenylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, etc. According to an embodiment of the present invention, the mixing ratio of the hydroxy polyether to the isocyanate is 1:5-5:1, for example, 1:1.

[0032] According to an embodiment of the present invention, the disulfide is selected from one, two or more of 4,4-diaminodiphenyl disulfide, 2,2-diaminodiphenyl disulfide and bis(2-hydroxyethyl) disulfide. Preferably, the amount of the disulfide is 30-70%, such as 50%. According to an embodiment of the present invention, the catalyst is selected from one, two or more of dibutyltin dilaurate, triphenylbismuth and N,N-dimethylbenzylamine. Preferably, the amount of the catalyst is 0.05%-0.3%, such as 0.8%, 0.1%, 0.15%, 0.2%. According to an embodiment of the present invention, the crosslinking agent is selected from trimethylolpropane or triethanolamine; preferably, the amount of the crosslinking agent is 2%-5%, such as 3%.

[0033] According to an embodiment of the present invention, the mixing ratio (mass ratio) of hydroxy polyether, isocyanate, disulfide, catalyst and crosslinking agent is 80-120: 80-120:30-60:0.01-0.2:1-10, for example, 100:100:50:0.1:3.

[0034] According to an embodiment of the present invention, the self-repairing coating comprises the self-repairing microcapsules and the self-repairing polyurethane. According to an embodiment of the present invention, the mass ratio of the self-repairing microcapsules to the self-repairing polyurethane is 1-20:100, for example, 3:100, 4:100, 5:100, 10:100, 20:100.

[0035] According to an embodiment of the present invention, the self-repairing coating further comprises a pore-forming agent. According to an embodiment of the present invention, the pore-forming agent is selected from one, two or more of ammonium bicarbonate, ammonium chloride, sodium bicarbonate and ammonium nitrate. Preferably, the pore-forming agent is a 25% ammonium chloride solution. Preferably, the amount of the pore-forming agent is 0.01%-0.05% of the total mass of the self-repairing microcapsules and the self-repairing polyurethane, for example, 0.02%, 0.03%.

[0036] The present invention also provides a method for preparing the self-repairing coating, the method comprising: The self-repairing microcapsules, optional self-repairing polyurethane, and optional pore-forming agent are mixed to obtain the self-repairing coating.

[0037] The present invention also provides a chip comprising the self-repairing coating.

[0038] The present invention also provides a method for preparing the above chip, the method comprising: The self-repairing coating is coated on the surface of the chip and cured to obtain the chip.

[0039] According to an embodiment of the present invention, the curing temperature is 50° C.-100° C., such as 80° C.; preferably, the curing time is 2 h-8 h, such as 5 h.

[0040] The present invention also provides the use of the self-repairing microcapsules and the self-repairing coatings in preparing chips.

[0041] Beneficial Effects The invention provides a method for preparing a self-repairing microcapsule, and a coating and a chip comprising the self-repairing microcapsule.

[0042] The self-repairing microcapsules prepared by the method of the present application have good stability, uniformity, affinity, environmental tolerance and dispersibility, and can effectively prevent agglomeration.

[0043] The coating and chip provided by the present application include self-repairing polyurethane and self-repairing microcapsules. When the coating is damaged, the microcapsules are damaged and the core material is released to achieve self-repair of the cracks. At the same time, the self-repairing polyurethane also plays a self-repairing function. The double synergistic repair shortens the crack healing time. When the coating is damaged multiple times and the repair agent is used up, the self-repairing polyurethane still works to achieve long-term self-repair of the coating. The chip surface provided by the present application has good acid and alkali corrosion resistance and self-repairing performance, and the self-repairing conditions are mild. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is the distribution morphology of the microcapsules in Example 1.

[0045] Figure 2 This is the distribution morphology of the microcapsules in Comparative Example 1.

[0046] Figure 3 This is the distribution morphology of the microcapsules in Comparative Example 2.

[0047] Figure 4 Schematic diagram of the three-phase contact angle of silica nanoparticles before and after modification.

[0048] Figure 5 This is a diagram showing the chip self-repair effect of Example 1.

[0049] Figure 6 The chip contact angle change curves of Example 1 and Comparative Example 1 in the acid and alkali corrosion test. DETAILED DESCRIPTION

[0050] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0051] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0052] Example 1 1. Preparation of modified silica nanoparticles: Propyl triethoxysilane, polyethylene glycol octylphenyl ether, and dibutyltin dilaurate were mixed and stirred in a ratio of 1:2:0.1% (molar ratio), and heated at 40°C overnight to obtain a mixture. 1g of silica nanoparticles was ultrasonically dispersed in 20mL of ethanol aqueous solution (ethanol: water = 90:10 / v:v), and then 1g of the above mixture was added (with a mass ratio of 1:20-30 to the dispersion), and the pH of the mixture was adjusted to about 8-9 with ammonia water, and heated at 60°C overnight. The suspension obtained by the reaction was centrifuged, and the solid was ultrasonically cleaned with ethanol aqueous solution (ethanol: water = 90:10 / v:v), and dried in an oven at 80°C.

[0053] 2. Preparation of prepolymer: Prepare 20 mL of 2M toluene diisocyanate cyclohexane solution, add 30% equivalent of 1,4-butanediol (0.6 M) dropwise while stirring, continue stirring after the addition is complete, and heat to 60°C to react overnight. The reaction mixture is distilled under reduced pressure to remove the solvent to obtain a prepolymer.

[0054] 3. Preparation of microcapsules: Ultrasonic dispersion of the modified silica nanoparticles prepared in step 1 in deionized water to form a suspension with a mass fraction of 1%. Mix the prepolymer prepared in step 2, ethyl acetate, and hexamethylene diisocyanate in a ratio of 1:1:1 as the oil phase, add it to the modified silica nanoparticle suspension (oil phase to water phase volume ratio 1:1) while stirring, then slowly drop 0.3 equivalents of 1,4-butanediol (0.6M), heat to 60°C and react for 2h. After the reaction is completed, filter, wash with deionized water, and dry in an oven at 60°C.

[0055] 4. Prepare a self-healing coating on the chip surface: Mix polyethylene glycol octylphenyl ether and hexamethylene diisocyanate in a ratio of 1:1, add 50% equivalent of 4,4-diaminodiphenyl disulfide, 0.1% equivalent of dibutyltin dilaurate, and 3% equivalent of triethanolamine, and stir for 30 minutes to obtain a mixed solution. Ultrasonic mix the microcapsules prepared in step 3 with the mixed solution in a mass ratio of 4:100, add 25% ammonium chloride solution with a mixed mass ratio of 0.02, and mix again. Coat the mixed solution on the chip surface and cure it at 80°C for 5 hours to obtain a chip with a self-healing coating.

[0056] Comparative Example 1 The proportions of the reagents in the coating preparation process were the same as those in Example 1, except that unmodified silica nanoparticles were used.

[0057] The distribution morphology of the microcapsules on the surface of the self-repairing coating chip prepared in Example 1 and Comparative Example 1 was observed by scanning electron microscopy. The results are as follows Figure 1 , Figure 2 As shown. Figure 1 , Figure 2By comparison, it can be seen that the use of modified silica nanoparticle microcapsules has better uniformity and dispersion, which can effectively prevent agglomeration.

[0058] Comparative Example 2 The difference from Example 1 is that different proportions of modified silica nanoparticles are used in the preparation of microcapsules. The modified silica nanoparticles are ultrasonically dispersed in deionized water to form a suspension with a mass fraction of 0.2%. The morphology of the prepared microcapsules is as follows: Figure 3 As shown, Figure 1 , Figure 2 By comparison, it can be seen that the proportion of modified silica nanoparticles affects the distribution state of microcapsules. The microcapsules prepared in Example 1 are more uniform.

[0059] Comparative Example 3 The modification process of silica nanoparticles and the preparation process of microcapsules are the same as those in Example 1. The coating is prepared by mixing polyethylene glycol octylphenyl ether and hexamethylene diisocyanate in a ratio of 1:1, ultrasonically mixing the prepared microcapsules and the mixed solution in a mass ratio of 4:100, and adding a 25% ammonium chloride solution with a mixing mass ratio of 0.02 to mix the two evenly. The mixed solution is coated on the chip surface and cured at 80°C for 5 hours to obtain a chip with a self-healing coating.

[0060] Test Example 1 The three-phase contact angles of silica nanoparticles before and after modification were tested respectively: the nano-silica particles were pressed into 1 mm thick slices using a tablet press and placed in a watch glass. A mixture of hexamethylene diisocyanate and chlorobenzene was added to the watch glass until the slice was covered. 5 μL of deionized water was added to the surface of the slice. The contact angle of the water droplet on the surface of the slice was observed to be the three-phase contact angle of the nanoparticles.

[0061] The results are as follows Figure 4 As shown, the modification improves the oil-phase affinity of the surface of silica nanoparticles, and the contact angle increases from 30 to about 75, which can better combine with oil droplets, thereby improving the dispersibility of microcapsules in the coating matrix.

[0062] Test Example 2 The chip surface prepared in Example 1 was scratched with a carving knife to detect the self-repairing effect of the chip.

[0063] The results are as follows Figure 5 As shown, the scratched chip was left at room temperature for 30 minutes, and the scratch was repaired, and the self-repairing conditions were mild.

[0064] The repair effects of the chips of Comparative Example 1 and Comparative Example 3 were tested under the same repair conditions. Comparative Example 3 can achieve the same repair effect as Example 1 after standing for 12 hours. The microcapsules in the coating of the chip of Comparative Example 1 are unevenly distributed, and the repair effect is poor. Almost no difference can be observed before and after standing for 12 hours.

[0065] Test Example 3 The chips prepared in Example 1 and Comparative Example 1 were subjected to acid and alkali corrosion resistance tests: the chips were immersed in a sulfuric acid solution with a pH of 1 and a sodium hydroxide solution with a pH of 14, respectively, and the static contact angles of the chips were tested by sampling at different days. The change curves are shown in FIG. Figure 6 As shown. Figure 6 It can be seen that the chip of Example 1 has good stability in acidic and alkaline environments, and the wettability of the coating surface has almost no change after immersion for 15 days. However, the chip of Comparative Example 1 has poor acid and alkali corrosion resistance under the same conditions.

[0066] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a self-repairing microcapsule, the method comprising the following steps: (1) Preparing modified silica nanoparticles: mixing silica nanoparticles with hydroxy polyether, silane modifier and catalyst, adjusting the pH to 8-9, heating for reaction; separating the reaction liquid to obtain modified silica nanoparticles; (2) Preparing a prepolymer: reacting an isocyanate solution with 1,4-butanediol to obtain the prepolymer; (3) Preparing microcapsules: dispersing the modified silica nanoparticles prepared in step (1) in water to prepare a modified silica nanoparticle suspension; mixing the prepolymer prepared in step (2) with ethyl acetate and hexamethylene diisocyanate to form an oil phase; adding the oil phase to the modified silica nanoparticle suspension, and then adding 1,4-butanediol to react to obtain microcapsules.

2. The preparation method according to claim 1, characterized in that: In step (1), the hydroxy polyether is selected from one, two or more of polyethylene glycol, polyethylene glycol octylphenyl ether, and polytetramethylene glycol ether; And / or, in step (1), the silane modifier is selected from one, two or more of isocyanate propyl triethoxy silane, isocyanate propyl trimethoxy silane, vinyl triethoxy silane, and γ-glycidyloxypropyl trimethoxy silane; And / or, in step (1), the catalyst is selected from one, two or more of dibutyltin dilaurate, triphenylbismuth, and N,N-dimethylbenzylamine; and / or, in step (1), the molar ratio of the silane modifier to the hydroxy polyether is 1:1-1:4; And / or, in step (1), the molar amount of the catalyst is 0.05%-0.3% of the molar amount of the silane modifier.

3. The preparation method according to claim 1, characterized in that: In step (2), the isocyanate is selected from one, two or more of toluene diisocyanate, methylene diphenyl diisocyanate, p-phenylene diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate; and / or, in step (2), the molar ratio of isocyanate to 1,4-butanediol is 1:0.1-0.5; and / or, in step (3), the mass concentration of the modified silica nanoparticle suspension is 0.5-5%; and / or, in step (3), the mixing ratio of the prepolymer prepared in step (2) to ethyl acetate and hexamethylene diisocyanate is 1-5:1-5:1-5; And / or, in step (3), the volume ratio of the oil phase to the modified silica nanoparticle suspension is 1:5-5:

1.

4. The self-repairing microcapsule prepared by the preparation method according to any one of claims 1 to 3.

5. A self-repairing coating, comprising the self-repairing microcapsules according to claim 4.

6. The self-repairing coating according to claim 5, characterized in that: The self-repairing coating also includes self-repairing polyurethane; The preparation method of the self-repairing polyurethane is as follows: hydroxy polyether and isocyanate are mixed, disulfide, a catalyst and a cross-linking agent are added, and the mixture is mixed and stirred to obtain the self-repairing polyurethane.

7. A method for preparing the self-repairing coating according to claim 5 or 6, the method comprising: The self-repairing microcapsules described in claim 4 and optional self-repairing polyurethane are mixed to obtain the self-repairing coating.

8. A chip comprising the self-repairing coating according to claim 5 or 6.

9. The method for preparing the chip according to claim 8, comprising: The self-repairing coating according to claim 5 or 6 is coated on the surface of the chip and cured to obtain the chip.

10. Use of the self-repairing microcapsule according to claim 4 or the self-repairing coating according to any one of claims 5 to 6 in preparing a chip.

Citation Information

Patent Citations

  • Preparation method for epoxy microcapsule by taking polyurethane as wall material

    CN103638881A

  • Composite shell microcapsule with self-repairing and anti-corrosion function and preparation method thereof

    CN109535315A

  • Self-repairing polyurethane elastomer based on multiple dynamic reversible effects, and preparation method thereof

    CN110511344A

  • Self-repairing waterborne polyurethane coating composition and coating

    CN113045981A

  • Self-repairing color-changing film and preparation method thereof

    CN114835870A

Cited By

  • Self-repairing lubricating composition, preparation method and engine oil containing composition

    CN120865981A

  • A self-healing lubricating composition, a method for preparing it, and an engine oil containing the composition.

    CN120865981B