Carbon-based catalyst, preparation method and application thereof, and formaldehyde removal material
By mixing activated carbon supported by transition metal oxide with activated carbon supported by precious metals and combining with optimized impregnation treatment methods, the problems of high cost and low efficiency of precious metal catalysts are solved, and the efficient formaldehyde removal effect is achieved.
Patent Information
- Application Number
- CN202411534915.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-10-31
AI Technical Summary
The existing supported precious metal catalysts are costly to prepare and the precious metal particles are prone to agglomeration, resulting in low catalytic efficiency.
By using the preparation method of carbon-based catalyst, the load of precious metals is reduced by mixing activated carbon supported by transition metal oxides with activated carbon supported by noble metals, and selecting reducing agents by preparing and optimizing the chemical properties of transition metals and precious metals, ensuring that The impregnation treatment effect can avoid heavy metal poisoning and improve the dispersion and utilization of precious metals.
It effectively reduces the preparation cost of the catalyst, improves the economic benefits of the catalytic industry, and achieves a formaldehyde removal efficiency of more than 85% at room temperature, improving the long-term stability and catalytic efficiency of the catalyst.
Smart Images

Figure CN119034723A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmental functional materials and atmosphere treatment, and specifically relates to a carbon-based catalyst and a preparation method and application thereof, and a formaldehyde removal material. Background Art
[0002] Formaldehyde (HCHO) is a typical volatile organic compound (VOC). It is colorless and has a pungent odor. Indoor formaldehyde mainly comes from furniture decoration materials and building materials, mainly artificial board furniture, wall stickers, multi-layer solid wood floors, and wall paint. Exposure to formaldehyde can greatly damage human health. Studies have shown that when the formaldehyde concentration exceeds 0.5mg / m 3 The human body will feel strong stimulation and shed tears, even at a low concentration of 0.1 mg / m 3 Formaldehyde can also make the human body feel uncomfortable. More seriously, long-term exposure to formaldehyde can cause a series of serious diseases such as leukemia and chromosomal abnormalities, and in severe cases, can lead to a variety of cancers. Epidemiological studies have confirmed that exposure to formaldehyde can cause physical harm, such as asthma and dermatitis. 3 Exposure to low formaldehyde concentrations for 1-5 minutes may cause eye irritation. 3 Exposure to high concentrations of formaldehyde for 1 minute will affect the functional state of the cerebral cortex. Therefore, the problem of indoor formaldehyde needs to be solved urgently, which requires innovation in technology and materials. This is not only related to everyone's quality of life, but also to people's survival and health.
[0003] At present, the methods of removing indoor formaldehyde can be generally classified into two categories, namely, controlling the generation of formaldehyde from the source and eliminating the generated formaldehyde through a series of methods, including pollution source control, mechanical purification (such as opening windows for ventilation, air conditioning and exhaust fans, etc.), plant and biological purification, physical adsorption, catalytic oxidation, etc. The catalytic oxidation method relies on the catalytic action of a specific catalyst to react formaldehyde with oxygen to generate non-toxic small molecules of water (H2O) and carbon dioxide (CO2). Due to the special indoor environment, the catalytic oxidation of free formaldehyde in the room is mainly photocatalytic oxidation, thermal catalytic oxidation and room temperature catalytic oxidation. Electrocatalytic oxidation and other methods are difficult to apply due to the special indoor environment. Thermal catalytic oxidation requires a certain temperature to achieve good catalytic performance, which will be limited in daily application. Room temperature catalytic oxidation is more practical.
[0004] Carbon materials are excellent supported catalyst carriers. For example, activated carbon and graphene have been widely used in the preparation of polymer nanocomposites. As a porous material with a large number of industrial applications, activated carbon has a strong basic adsorption capacity, a large specific surface area and thermal stability. The presence of the carbonized structure gives it adjustable electron transfer and charge storage characteristics. Its electronic structure can be further adjusted by modifying metal substances, thereby improving the catalytic performance. Among them, supported precious metal catalysts can achieve a relatively ideal conversion rate at a relatively low temperature or even at room temperature, and realize the rapid conversion of high-concentration formaldehyde at low temperature. At present, among many precious metals, platinum (Pt), palladium (Pd), rhodium (Rh), gold (Au), and silver (Ag) have better catalytic effects and are widely studied. However, the disadvantage is that the cost of precious metals is high, and the atomic utilization rate is not high due to the easy agglomeration of precious metal particles. Therefore, how to reduce the content of precious metals and improve the utilization rate is the top priority of research.
[0005] However, supported precious metal catalysts have the following problems: (1) Due to the high cost of precious metals, if the amount used is large, the catalyst preparation cost is high; (2) Due to the easy agglomeration of precious metal particles, their atomic utilization rate is not high, resulting in low catalytic efficiency. Summary of the invention
[0006] Therefore, the present invention provides a carbon-based catalyst and a preparation method and application thereof, and a formaldehyde removal material, which can solve the technical problem of high preparation cost of supported precious metal catalysts in the prior art.
[0007] In order to solve the above problems, the present invention provides a method for preparing a carbon-based catalyst, comprising the following steps: Step 1) preparing activated carbon loaded with transition metal oxides; preparing activated carbon loaded with noble metals; Step 2) Mixing the activated carbon loaded with transition metal oxides with the activated carbon loaded with noble metals to obtain a carbon-based catalyst.
[0008] Furthermore, in step 1), the preparation step of the activated carbon loaded with transition metal oxides comprises: The transition metal salt solution and the buffer solution are mixed and reacted to obtain a mixed solution; then the mixed solution is used to impregnate the activated carbon, and then filtered and dried to obtain the activated carbon loaded with the transition metal oxide.
[0009] Furthermore, stirring is performed during the mixing reaction; the stirring time is 5 to 10 minutes.
[0010] Furthermore, the step of impregnating the activated carbon with the mixed solution comprises: Add activated carbon to the mixed solution at room temperature and stir; the stirring time is 60 to 120 minutes.
[0011] Furthermore, the drying temperature is 60 to 80° C. and the drying time is 24 to 48 hours.
[0012] Furthermore, the transition metal salt is potassium permanganate KMnO4; and / or The buffer is ammonium carbonate (NH4)2CO3; and / or In the activated carbon loaded with transition metal oxides: Mn 2+ The content is 4.28%~5.08%, Mn 3+ The content is 51.8%~54.8%, Mn 4+ The content is 40.12%~43.92%, Mn 3+ / Mn 4+ The ratio is 1.08~1.37; the crystal structure of manganese includes δ-MnO x , the δ-MnO x Uniformly present on the surface of activated carbon; and / or When the transition metal salt solution and the buffer solution are mixed and reacted, the weight ratio of the transition metal salt in the transition metal salt solution to the buffer in the buffer solution is 3.5:1 to 4.5:1; and / or When the mixed solution is used to impregnate the activated carbon, the weight ratio of the transition metal salt to the activated carbon in the transition metal salt solution is 2:1 to 3:1.
[0013] Further, the concentration of the transition metal salt solution is 65.7-67.7 mg / mL; and / or The concentration of the buffer solution is 20-30 mg / mL.
[0014] Furthermore, in step 1), the step of preparing activated carbon loaded with precious metals comprises: Step S1) impregnating activated carbon with a polyelectrolyte solution, filtering and drying the activated carbon to obtain activated carbon loaded with polyelectrolyte; Step S2) The activated carbon loaded with the polyelectrolyte is mixed with a noble metal salt solution and a reducing agent solution to obtain activated carbon loaded with the noble metal.
[0015] Furthermore, in the step S1), the impregnation treatment includes: Adding activated carbon to a polyelectrolyte solution at room temperature and stirring the mixture; wherein the weight ratio of the activated carbon to the polyelectrolyte in the polyelectrolyte solution is 31.7:1 to 95.5:1; and the stirring time is 60 to 120 minutes.
[0016] Furthermore, in the step S1), the drying temperature is 60 to 80° C. and the drying time is 24 to 48 hours.
[0017] Furthermore, the step S2) includes: Step S21) mixing the activated carbon loaded with polyelectrolyte with a noble metal salt solution to form a system to be reduced; Step S22) mixing the system to be reduced with the reducing agent solution to perform a reduction reaction; after the reduction reaction is completed, filtering and drying are performed to obtain primary loaded activated carbon; Step S23) The primary loaded activated carbon is mixed with a noble metal salt solution and a reducing agent solution for reaction, and then filtered and dried to obtain activated carbon loaded with noble metals.
[0018] Furthermore, in the step S21), the mass ratio of the activated carbon loaded with polyelectrolyte to the noble metal salt in the noble metal salt solution is 312.5:1 to 937.5:1.
[0019] Furthermore, in the step S22), the drying temperature is 60 to 80° C. and the drying time is 24 to 48 hours.
[0020] Furthermore, in the step S23), the drying temperature is 60 to 80° C. and the drying time is 24 to 48 hours.
[0021] Furthermore, the polyelectrolyte is polydiallyl dimethylpropyl ammonium chloride (PDDA); and / or The noble metal salt is selected from chloroplatinic acid hexahydrate H2PtCl6·6H2O; and / or The reducing agent solution is obtained by mixing a sodium borohydride NaBH4 solution with a sodium hydroxide NaOH solution; and / or The mass fraction of the noble metal in the noble metal-loaded activated carbon is 0.18-0.22 wt %.
[0022] Further, the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is 5:1 to 5.4:1; and / or The concentration of the polydiallyl dimethyl propyl ammonium chloride (PDDA) solution is 2.10 to 6.30 mg / mL; and / or The concentration of the hexahydrate chloroplatinic acid H2PtCl6·6H2O solution is 0.96 to 2.88 mg / mL; and / or The concentration of sodium borohydride NaBH4 solution is 3.0-9.1 mg / mL; and / or The concentration of the sodium hydroxide NaOH solution is 16-48 mg / mL.
[0023] Furthermore, in the step 2), the mass ratio of the activated carbon loaded with transition metal oxides to the activated carbon loaded with noble metals is 6.5-7.5:2.5-3.5.
[0024] Furthermore, before step 1), a purification step of activated carbon is also included: The original activated carbon is added into deionized water for soaking, and then filtered and dried to obtain purified activated carbon.
[0025] Furthermore, in the activated carbon loaded with precious metals: the precious metals are loaded in the activated carbon in the form of nanoparticles; preferably, the particle size of the nanoparticles is 1 to 5 nm.
[0026] On the other hand, the present invention also provides a carbon-based catalyst, wherein the carbon-based catalyst is obtained by mixing activated carbon loaded with transition metal oxides and activated carbon loaded with noble metals.
[0027] Preferably, the transition metal oxide is manganese oxide; in the activated carbon loaded with transition metal oxide: Mn 2+ The content is 4.28%~5.08%, Mn 3+ The content is 51.8%~54.8%, Mn 4+ The content is 40.12%~43.92%, Mn 3+ / Mn 4+ The ratio is 1.08~1.37; the crystalline structure of transition metals includes δ-MnO x , the δ-MnO x Uniformly present on the surface of activated carbon; Preferably, in the activated carbon loaded with precious metals: the precious metals are loaded in the activated carbon in the form of nanoparticles; preferably, the particle size of the nanoparticles is 1 to 5 nm; Preferably, the carbon-based catalyst is obtained by any of the preparation methods described above.
[0028] In another aspect, the present invention provides an application of the above-mentioned carbon-based catalyst, wherein the carbon-based catalyst is used for removing indoor formaldehyde at room temperature.
[0029] On the other hand, the present invention also provides a formaldehyde removal material, which is the carbon-based catalyst described above.
[0030] Compared with the prior art, the present invention has at least the following beneficial effects: 1. The present invention provides a method for preparing a carbon-based catalyst, which comprises mixing activated carbon loaded with transition metal oxides with activated carbon loaded with noble metals to obtain a carbon-based catalyst; based on the above method, the loading amount of the noble metal is reduced; the preparation cost of the catalyst is effectively reduced, and the economic benefits of the catalytic industry are improved; at the same time, by separately preparing activated carbon loaded with transition metal oxides and activated carbon loaded with noble metals, the problem of heavy metal poisoning of the noble metals during the loading process can be avoided by avoiding the presence of heavy metals in other raw and auxiliary materials (for example, when preparing a carbon-based catalyst, if transition metal oxides and noble metals are loaded at the same time, the transition metals present in the surrounding environment of the noble metals can easily deactivate the noble metals), thereby causing the activated carbon loaded with the noble metals to be deactivated, affecting the catalytic effect of the final carbon-based catalyst.
[0031] 2. Furthermore, the present invention separately prepares activated carbon loaded with transition metal oxides and activated carbon loaded with noble metals, and then mixes them. Reducing agents can be selected based on the chemical properties of transition metals and noble metals, so that transition metal salts and noble metal salts are fully reduced to ensure the loading effect after impregnation treatment, thereby ensuring the catalytic effect of the final carbon-based catalyst.
[0032] 3. Furthermore, the present invention performs at least two loadings on the activated carbon loaded with precious metals, and the loading amount each time is relatively small, so that the concentration of reactants and the ionic strength of the impregnation solution can be regulated, the particle size of the precious metal nanoparticles can be reduced, and the dispersibility of the precious metals can be enhanced; at the same time, it can avoid a large loading amount at one time, agglomeration of the precious metal particles, low utilization rate of the precious metal after reduction, high preparation cost, and low catalytic efficiency.
[0033] 4. On the other hand, the present invention provides a carbon-based catalyst prepared by the above method, which is a carbon-based catalyst co-loaded with transition metal oxides and precious metals, which can reduce the preparation cost of the loaded catalyst and improve the catalytic efficiency; the above-mentioned carbon-based catalyst of the present invention is used for removing indoor formaldehyde at room temperature, and can remove more than 85% of indoor formaldehyde. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0035] Figure 1 This is a diagram showing the removal efficiency of formaldehyde by different ratios of platinum and activated carbon in the present invention; Figure 2 This is a graph showing the removal efficiency of formaldehyde with different added amounts of the carbon-based catalyst in the present invention. DETAILED DESCRIPTION
[0036] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0037] According to an embodiment of the present invention, a method for preparing a carbon-based catalyst is provided, comprising the following steps: Step 1) Purification of activated carbon: soaking the original activated carbon in deionized water, filtering and drying to obtain purified activated carbon; the activated carbon used in the following method is purified activated carbon (AC); the ash content of the purified AC is ≤10%, and the particle size is 30-60 mesh; The steps of preparing activated carbon loaded with transition metal oxides are as follows: mixing a transition metal salt solution with a buffer solution to obtain a mixed solution; then adding activated carbon to the mixed solution at room temperature, and performing secondary stirring, filtering, and drying (i.e., impregnating the activated carbon with the mixed solution) to obtain activated carbon loaded with transition metal oxides after drying; The transition metal salt is potassium permanganate KMnO4, and the concentration of the potassium permanganate KMnO4 solution is 65.7-67.7 mg / mL; the buffer is ammonium carbonate (NH4)2CO3, and the concentration of the ammonium carbonate (NH4)2CO3 solution is 20-30 mg / mL; when the transition metal salt solution and the buffer solution are mixed and reacted, KMnO4 (i.e., solute) in the potassium permanganate KMnO4 solution reacts with (NH4)2CO3 in the ammonium carbonate (NH4)2CO3 solution. 3 (i.e., solute) is 3.5:1 to 4.5:1; when the mixed solution is used to impregnate the activated carbon, the weight ratio of KMnO4 to the activated carbon in the potassium permanganate KMnO4 solution is 2:1 to 3:1; stirring is performed once during the mixing reaction; preferably, the time for the first stirring is 5 to 10 minutes; preferably, the time for the second stirring is 60 to 120 minutes; the temperature for the drying treatment is 60 to 80°C; and the time for the drying treatment is 24 to 48 hours; Steps for preparing activated carbon loaded with precious metals: Step S1) adding activated carbon to a polyelectrolyte solution at room temperature, stirring, filtering and drying to obtain activated carbon loaded with polyelectrolyte; wherein the weight ratio of activated carbon to polyelectrolyte (i.e., solute) in the polyelectrolyte solution is 31.7:1 to 95.5:1; preferably, the stirring time is 60 to 120 minutes; the drying temperature is 60 to 80° C.; and the drying time is 24 to 48 hours; Step S21) Mixing the activated carbon loaded with polyelectrolyte with the noble metal salt solution to form a system to be reduced; wherein the mass ratio of the activated carbon loaded with polyelectrolyte to the noble metal salt (ie, solute) in the noble metal salt solution is 312.5:1 to 937.5:1.
[0038] Step S22) mixing the system to be reduced with the reducing agent solution (reducing liquid) to carry out a reduction reaction; after the reduction reaction is completed, filtering and drying are carried out to obtain a primary loaded activated carbon; preferably, the drying temperature is 60 to 80° C.; and the drying time is 24 to 48 hours; Step S23) the primary loaded activated carbon is mixed with the noble metal salt solution and the reducing agent solution for reaction, and then filtered and dried; The polyelectrolyte is polydiallyl dimethylpropyl ammonium chloride (PDDA); the noble metal salt is chloroplatinic acid hexahydrate (H2PtCl6·6H2O); the reducing agent solution is obtained by mixing sodium borohydride (NaBH4) solution with sodium hydroxide (NaOH) solution; the obtained activated carbon loaded with noble metals is platinum (Pt) modified activated carbon, wherein platinum is loaded in the activated carbon in the form of platinum nanoparticles, and the particle size of the platinum nanoparticles is 1 to 5 nm; Step 2) Mixing activated carbon loaded with transition metal oxides with activated carbon loaded with noble metals to obtain a carbon-based catalyst synergistically loaded with transition metal oxides and noble metals; wherein the mass ratio of activated carbon loaded with transition metal oxides to activated carbon loaded with noble metals is 6.5-7.5:2.5-3.5.
[0039] Among them, the weight ratio of NaOH (i.e., solute) in the sodium hydroxide NaOH solution to NaBH4 (i.e., solute) in the sodium borohydride NaBH4 solution is 5:1-5.4:1; the concentration of the polydiallyl dimethylpropyl ammonium chloride PDDA solution is 2.10-6.30 mg / mL; the concentration of the hexahydrate chloroplatinic acid H2PtCl6·6H2O solution is 0.96-2.88 mg / mL; the concentration of the sodium borohydride NaBH4 solution is 3.0-9.1 mg / mL; and the concentration of the sodium hydroxide NaOH solution is 16-48 mg / mL.
[0040] Based on the above method, the amount of precious metals used can be reduced, the preparation cost of the catalyst can be effectively reduced, and the economic benefits of the catalytic industry can be improved; at the same time, by separately preparing activated carbon loaded with transition metal oxides and activated carbon loaded with precious metals, the presence of heavy metals in other raw and auxiliary materials can be avoided, which can easily cause heavy metal poisoning of precious metals during the loading process, thereby causing the activated carbon loaded with precious metals to be deactivated, affecting the catalytic effect of the final carbon-based catalyst; in addition, reducing agents can be selected based on the chemical properties of transition metals and precious metals, so that the transition metal salts and precious metal salts are fully reduced, ensuring the loading effect after impregnation treatment, thereby ensuring the catalytic effect of the final carbon-based catalyst.
[0041] When the mass ratio of activated carbon loaded with transition metal oxides to activated carbon loaded with precious metals is higher than the above range, the long-term stability of the final carbon-based catalyst will be weakened. Experiments have shown that, when other experimental conditions are kept the same, the stable formaldehyde removal ability of a single manganese oxide can only be maintained for 24 hours; as the mass ratio of the two gradually decreases, the formaldehyde removal stability period gradually extends. When the mass ratio of the two is in the range of 6.5-7.5:2.5-3.5, the optimal formaldehyde removal effect peak value is reached; when the mass ratio of the two is lower than the above range, it will lead to excessive use and waste of precious metal catalysts, resulting in cost growth.
[0042] The reduction products of KMnO4 are diverse, which affect the adsorption and conversion of HCHO and O2 by the catalyst. The one with formaldehyde catalysis function is Mn 3+ , Mn 4+ ,δ-MnO x In this application, ammonium carbonate (NH4)2CO3 solution is used as a buffer to ensure that KMnO4 converts Mn 3+ , Mn 4+ The conversion rate of δ-MnO x The generation rate and the loading and distribution uniformity on the AC surface are determined by the solution impregnation method at room temperature to prepare the manganese oxide catalyst, and the carbon-based manganese oxide modified catalyst is synthesized in one step using ammonium carbonate (NH4)2CO3 as a mild reducing agent. The catalytic activity of the manganese-based catalyst for formaldehyde depends on the Mn 3+ , Mn 4+ The content of Mn 3+ / Mn 4+ The ratio of MnO x In the manganese oxide catalyst (i.e., activated carbon loaded with transition metal oxide) obtained in the present application, Mn 2+ The content is 4.28%~5.08%, Mn 3+ The content is 51.8%~54.8%, Mn 4+ The content is 40.12%~43.92%, Mn3+ / Mn 4+ The ratio is 1.08 to 1.37; preferably, Mn 2+ The content is 4.68%, Mn 3+ The content is 53.8%, Mn 3+ The content is 41.5%, Mn 3+ / Mn 4+ The ratio is 1.30, compared with the existing manganese catalysts, Mn 3+ / Mn 4+ The ratio of MnO is further improved, and the crystal structure of Mn is mainly δ-MnO x And evenly exists on the surface of activated carbon.
[0043] Among them, Mn 2+ , Mn 3+ , Mn 4+ The sum of the contents is 100%; according to the known natural laws of redox reactions, potassium permanganate reduction is easily affected by the environmental pH value, and will show different decreased valences under different conditions. Potassium permanganate can easily obtain 5 electrons under acidic conditions and can be reduced to positive divalent manganese ions, and can be easily reduced to positive hexavalent manganese ions under strong alkaline conditions, both of which are not conducive to the catalytic removal of formaldehyde; while under weak alkaline conditions, it is easy to obtain three electrons to generate positive tetravalent manganese ions, namely MnO2, which is beneficial to the removal of formaldehyde. Therefore, this application selects ammonium carbonate (NH4)2CO3 as a warm buffer and as a reducing agent, which provides a suitable acid-base environment for the reduction of potassium permanganate and avoids the generation of positive divalent manganese ions and positive hexavalent manganese ions that are not conducive to formaldehyde catalysis; Manganese oxide crystal resources are abundant, and different crystal forms of manganese oxide can be obtained by controlling the preparation method, raw materials and preparation conditions. Compared with the thermal decomposition method, hydrothermal method, sol-gel method, precipitation method and other methods that require high temperature experiments, isothermal low pressure and other special difficult to control conditions, this application adopts a solution immersion redox method at room temperature, but the anions in the manganese salt solution in the redox method will affect the growth of manganese oxide crystals, so it is necessary to select a suitable reducing agent, sulfate ions and nitrate ions that are easy to promote β-MnO x The formation of ammonium carbonate (NH4)2CO3 is not conducive to the catalytic reaction of formaldehyde, while ammonium carbonate (NH4)2CO3 is conducive to the formation of δ-MnO x At the same time, the concentration of reactants in the redox reaction is also an important factor. The present invention can achieve δ-MnO by strictly controlling the concentration of potassium permanganate KMnO4 solution and the concentration of ammonium carbonate (NH4)2CO3 solution. x The concentration of potassium permanganate KMnO4 solution is 65.7-67.7 mg / mL, and the concentration of ammonium carbonate (NH4)2CO3 solution is 20-30 mg / mL.
[0044] In addition, compared with loading transition metals and noble metals at the same time, the platinum nanoparticles in the present application are loaded on the activated carbon surface in a more appropriate particle size range and more evenly, ensuring the stability of the catalytic active centers and the optimal utilization of platinum; preferably, the particle size of the nanoparticles is 1 to 5 nm.
[0045] In the process of constructing a uniformly dispersed noble metal active site catalyst, an alkaline environment is often required to achieve successful loading of the noble metal. In the process of preparing the catalyst using the impregnation method, the chloride salt or acid solution of the noble metal is first impregnated, and then neutralized with an alkaline solution, which will be converted into a hydroxide and precipitated on the pore surface of the carrier, which is conducive to the removal of chloride ions, thereby improving the activity of the catalyst, so a suitable pH value is crucial for the preparation of the catalyst. In the present application, sodium borohydride NaBH4 and sodium hydroxide NaOH create a suitable alkaline environment for it, and reduce hexahydrate chloroplatinic acid H2PtCl6·6H2O to Pt elemental. Due to the interaction between the noble metal particles, the Pt elemental agglomerates, and the particle size increases to form nanoparticles of a certain particle size. In order to ensure a suitable particle size range and avoid a one-time accumulation exceeding the range value of 1 to 5nm, resulting in a reduction in the utilization rate of the noble metal, the present application achieves a successful preparation of a particle size range of 1 to 5nm through two low-concentration loadings.
[0046] On the other hand, the present invention also provides a carbon-based catalyst, wherein the carbon-based catalyst is obtained by mixing activated carbon loaded with transition metal oxides and activated carbon loaded with noble metals; Preferably, the transition metal oxide is manganese oxide; in the activated carbon loaded with transition metal oxide: Mn 2+ The content is 4.28%~5.08%, Mn 3+ The content is 51.8%~54.8%, Mn 4+ The content is 40.12%~43.92%, Mn 3+ / Mn 4+ The ratio is 1.08~1.37; the crystalline structure of transition metals includes δ-MnO x , the δ-MnO x Uniformly present on the surface of activated carbon; further preferably, Mn 2+ The content is 4.68%, Mn 3+ The content is 53.8%, Mn 4+ The content is 41.5%, Mn 3+ / Mn 4+ The ratio is 1.30; Preferably, in the activated carbon loaded with precious metals: the precious metals are loaded in the activated carbon in the form of nanoparticles; preferably, the particle size of the nanoparticles is 1 to 5 nm; Preferably, the carbon-based catalyst is obtained by any of the preparation methods described above.
[0047] In another aspect, the present invention provides an application of the carbon-based catalyst, wherein the carbon-based catalyst is used to remove indoor formaldehyde at room temperature. The carbon-based catalyst can also be used to remove other volatile organic pollutants (such as aromatic hydrocarbon pollutants) in the room except HCHO.
[0048] In another aspect, the present invention provides an application of the above-mentioned carbon-based catalyst, wherein the carbon-based catalyst is used for removing indoor formaldehyde at room temperature.
[0049] The present invention is further described below with reference to specific embodiments and comparative examples.
[0050] Example 1 This embodiment provides a method for preparing a carbon-based catalyst, comprising the following steps: Step 1) activated carbon purification step: 40 g of original activated carbon was added to 400 mL of deionized water, soaked for 5 min, filtered, and then placed in an oven at a constant temperature of 80°C for 24 h to obtain purified activated carbon AC; Preparation steps of activated carbon loaded with transition metal oxides: 100mL of ammonium carbonate (NH4)2CO3 solution (concentration of 25mg / mL) was quickly injected into 150mL of potassium permanganate KMnO4 solution (concentration of 66.7mg / mL) (the weight ratio of KMnO4 in potassium permanganate KMnO4 solution to (NH4)2CO3 in ammonium carbonate (NH4)2CO3 solution was about 4:1) and stirred for 5min, then 25g AC (the weight ratio of KMnO4 to activated carbon in potassium permanganate KMnO4 solution was 2.5:1) was added, and the reaction was stirred for a second time at room temperature. The second stirring time was 60min, then filtered, and then placed in a constant temperature oven at 80℃ for 24h to obtain activated carbon loaded with manganese oxide (MnO x / AC); Preparation steps of activated carbon loaded with precious metals: Step S1) 15 g AC was added to 75 mL polydiallyl dimethylpropyl ammonium chloride PDDA (polyelectrolyte) solution (concentration of 2.1 mg / mL) (the weight ratio of activated carbon to polyelectrolyte in the polyelectrolyte solution was 95.5:1), and the mixture was stirred at room temperature for 60 min and then filtered, and then placed in an oven at a constant temperature of 80° C. and dried for 24 h to obtain activated carbon loaded with PPDA (PDDA / AC); Step S21) 15 g of PDDA / AC was mixed with 16.65 mL of hexahydrate chloroplatinic acid H2PtCl6·6H2O (i.e., noble metal salt) solution (concentration of 0.96 mg / mL) to obtain a system (suspension) to be reduced (the mass ratio of the activated carbon loaded with polyelectrolyte to the noble metal salt in the noble metal salt solution was 937.5:1); Step S22) Take 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 3.0 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 16 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.3:1), mix them evenly to obtain 15 mL of reducing solution; quickly inject the reducing solution into the system to be reduced, continue stirring the reaction for 30 minutes, filter it, and then place it in a constant temperature oven at 80°C for 24 hours to obtain a primary loaded activated carbon; Step S23) Take 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 3.0 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 16 mg / mL), respectively (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.3:1), mix them evenly to obtain 15 mL of reducing solution; 15 g of primary loaded activated carbon and 16.65 mL of H2PtCl6·6H2O solution are added. The reduced solution was mixed with a solution (concentration of 0.96 mg / mL) to obtain a suspension (the mass ratio of the primary loaded activated carbon to the precious metal salt in the precious metal salt solution was 937.5:1); the reduced solution was quickly injected into the above suspension, and the suspension was continuously stirred for reaction for 30 minutes and then filtered, and then placed in an oven at a constant temperature of 80°C for drying for 24 hours to obtain platinum-modified activated carbon (Pt / AC); the mass fraction of platinum in the Pt / AC obtained in this embodiment was 0.08wt% (recorded as 0.08wt%Pt / AC); Step 2) Take 21g of the above MnO x / AC and 9g of the above Pt / AC (i.e., MnO x The mass ratio of Pt / AC to Pt / AC was 7:3), and the materials were evenly stirred by physical rotation mixing to obtain a carbon-based catalyst.
[0051] In this example, manganese oxide activated carbon (MnO x / AC):Mn 2+ The content is 4.68%, Mn 3+ The content is 53.8%, Mn 4+ The content is 41.5%, Mn 3+ / Mn 4+ The ratio is 1.30; the crystalline structure of transition metals includes δ-MnO x ,δ-MnOx Uniformly present on the surface of activated carbon; In Pt / AC: platinum is loaded on activated carbon in the form of nanoparticles; the particle size of the nanoparticles is 1 to 5 nm.
[0052] Example 2 This embodiment provides a method for preparing a carbon-based catalyst, comprising the following steps: Step 1) activated carbon purification step: 40 g of original activated carbon was added to 400 mL of deionized water, soaked for 5 min, filtered, and then placed in an oven at a constant temperature of 80°C for 24 h to obtain purified activated carbon AC; Preparation steps of activated carbon loaded with transition metal oxides: 100mL of ammonium carbonate (NH4)2CO3 solution (concentration of 25mg / mL) was quickly injected into 150mL of potassium permanganate KMnO4 solution (concentration of 66.7mg / mL) (the weight ratio of KMnO4 in potassium permanganate KMnO4 solution to (NH4)2CO3 in ammonium carbonate (NH4)2CO3 solution was about 4:1) and stirred for 5min, then 25g AC was added (the weight ratio of KMnO4 to activated carbon in potassium permanganate KMnO4 solution was 2.5:1) and stirred for a second time at room temperature. After the second stirring time was 60min, it was filtered and then placed in a constant temperature oven at 80℃ for 24h to obtain activated carbon loaded with manganese oxide (MnO x / AC); Preparation steps of activated carbon loaded with precious metals: Step S1) 15 g AC was added to 75 mL polydiallyl dimethylpropyl ammonium chloride PDDA (polyelectrolyte) solution (concentration of 3.15 mg / mL), (the weight ratio of activated carbon to polyelectrolyte in the polyelectrolyte solution was 63.5:1), the mixture was stirred and reacted for 60 min at room temperature, filtered, and then placed in an oven at a constant temperature of 80° C. and dried for 24 h to obtain activated carbon loaded with PPDA (PDDA / AC); Step S21) 15 g of PDDA / AC was mixed with 16.65 mL of hexahydrate chloroplatinic acid H2PtCl6·6H2O (precious metal salt) solution (concentration of 1.44 mg / mL) to obtain a system (suspension) to be reduced (the mass ratio of the activated carbon loaded with polyelectrolyte to the precious metal salt in the precious metal salt solution was 625:1); Step S22) Take 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 4.6 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 24 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.2:1), mix them evenly to obtain 15 mL of reducing solution; quickly inject the reducing solution into the system to be reduced, continue stirring the reaction for 30 minutes, filter it, and then place it in a constant temperature oven at 80°C for 24 hours to obtain a primary loaded activated carbon; Step S23) 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 4.6 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 24 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.2:1) are taken respectively, and mixed evenly to obtain 15 mL of reducing solution; 15 g of primary loaded activated carbon and 16.65 mL of H2PtCl6·6H2O solution (concentration of 1.44 mg / mL) are mixed (the mass ratio of primary loaded activated carbon to the precious metal salt in the precious metal salt solution is 625:1) to obtain a suspension; the reducing solution is quickly injected into the above suspension, the reaction is continuously stirred for 30 minutes, and then filtered, and then placed in a constant temperature oven of 80°C for drying for 24 hours to obtain platinum modified activated carbon (Pt / AC); the mass fraction of platinum in the Pt / AC obtained in this embodiment is 0.12wt% (recorded as 0.12wt%Pt / AC); Step 2) Take 21g of the above MnO x / AC and 9g of the above Pt / AC (i.e., MnO x The mass ratio of Pt / AC to Pt / AC was 7:3), and the materials were evenly stirred by physical rotation mixing to obtain a carbon-based catalyst.
[0053] In this example, manganese oxide activated carbon (MnO x / AC):Mn 2+ The content is 4.68%, Mn 3+ The content is 53.8%, Mn 4+ The content is 41.5%, Mn 3+ / Mn 4+ The ratio is 1.30; the crystalline structure of transition metals includes δ-MnO x ,δ-MnO x Uniformly present on the surface of activated carbon; In Pt / AC: platinum is loaded on activated carbon in the form of nanoparticles; the particle size of the nanoparticles is 1 to 5 nm.
[0054] Example 3 This embodiment provides a method for preparing a carbon-based catalyst, comprising the following steps: Step 1) activated carbon purification step: 40 g of original activated carbon was added to 400 mL of deionized water, soaked for 5 min, filtered, and then placed in an oven at a constant temperature of 80°C for 24 h to obtain purified activated carbon AC; Preparation steps of activated carbon loaded with transition metal oxides: 100mL of ammonium carbonate (NH4)2CO3 solution (concentration of 25mg / mL) was quickly injected into 150mL of potassium permanganate KMnO4 solution (concentration of 66.7mg / mL) (the weight ratio of KMnO4 in potassium permanganate KMnO4 solution to (NH4)2CO3 in ammonium carbonate (NH4)2CO3 solution was about 4:1) and stirred for 5min, then 25g AC was added (the weight ratio of KMnO4 to activated carbon in potassium permanganate KMnO4 solution was 2.5:1) and stirred for a second time at room temperature. After the second stirring time was 60min, it was filtered and then placed in a constant temperature oven at 80℃ for 24h to obtain activated carbon loaded with manganese oxide (MnO x / AC); Preparation steps of activated carbon loaded with precious metals: Step S1) 15 g AC was added to 75 mL polydiallyl dimethylpropyl ammonium chloride PDDA (polyelectrolyte) solution (concentration of 4.2 mg / mL), (the weight ratio of activated carbon to polyelectrolyte in the polyelectrolyte solution was 47.6:1), the mixture was stirred and reacted for 60 min at room temperature, filtered, and then placed in an oven at a constant temperature of 80° C. and dried for 24 h to obtain activated carbon loaded with PPDA (PDDA / AC); Step S21) 15 g of PDDA / AC was mixed with 16.65 mL of hexahydrate chloroplatinic acid H2PtCl6·6H2O (precious metal salt) solution (concentration of 1.92 mg / mL) to obtain a system (suspension) to be reduced (the mass ratio of the activated carbon loaded with polyelectrolyte to the precious metal salt in the precious metal salt solution was 468.6:1); Step S22) Take 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 6.1 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 32 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.2:1), mix them evenly to obtain 15 mL of reducing solution; quickly inject the reducing solution into the system to be reduced, continue stirring the reaction for 30 minutes, filter it, and then place it in a constant temperature oven at 80°C for 24 hours to obtain a primary loaded activated carbon; Step S23) Take 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 6.1 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 32 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.2:1), mix them evenly to obtain 15 mL of reducing solution; add 15 g of primary loaded activated carbon and 16.65 mL of H2PtCl6·6H2O solution (concentration of 1.92 mg / mL) and mixed (the mass ratio of the primary loaded activated carbon to the precious metal salt in the precious metal salt solution is 468.6:1) to obtain a suspension; the reducing solution is quickly injected into the above suspension, and the reaction is continued with stirring for 30 minutes, and then filtered, and then placed in an oven at a constant temperature of 80°C for drying for 24 hours to obtain platinum-modified activated carbon (Pt / AC); the mass fraction of platinum in the Pt / AC obtained in this embodiment is 0.16wt% (recorded as 0.16wt%Pt / AC); Step 2) Take 21g of the above MnO x / AC and 9g of the above Pt / AC (i.e., MnO x The mass ratio of Pt / AC to Pt / AC was 7:3), and the materials were evenly stirred by physical rotation mixing to obtain a carbon-based catalyst.
[0055] In this example, manganese oxide activated carbon (MnO x / AC):Mn 2+ The content is 4.68%, Mn 3+ The content is 53.8%, Mn 4+ The content is 41.5%, Mn 3+ / Mn 4+ The ratio is 1.30; the crystalline structure of transition metals includes δ-MnO x ,δ-MnO x Uniformly present on the surface of activated carbon; In Pt / AC: platinum is loaded in activated carbon in the form of nanoparticles; the particle size of the nanoparticles is 1 to 5 nm.
[0056] Example 4 This embodiment provides a method for preparing a carbon-based catalyst, comprising the following steps: Step 1) activated carbon purification step: 40 g of original activated carbon was added to 400 mL of deionized water, soaked for 5 min, filtered, and then placed in an oven at a constant temperature of 80°C for 24 h to obtain purified activated carbon AC; Preparation steps of activated carbon loaded with transition metal oxides: 100mL of ammonium carbonate (NH4)2CO3 solution (concentration of 25mg / mL) was quickly injected into 150mL of potassium permanganate KMnO4 solution (concentration of 66.7mg / mL) (the weight ratio of KMnO4 in potassium permanganate KMnO4 solution to (NH4)2CO3 in ammonium carbonate (NH4)2CO3 solution was about 4:1) and stirred for 5min, then 25g AC was added (the weight ratio of KMnO4 to activated carbon in potassium permanganate KMnO4 solution was 2.5:1) and stirred for a second time at room temperature. After the second stirring time was 60min, it was filtered and then placed in a constant temperature oven at 80℃ for 24h to obtain activated carbon loaded with manganese oxide (MnO x / AC); Preparation steps of activated carbon loaded with precious metals: Step S1) 15 g AC was added to 75 mL polydiallyl dimethylpropyl ammonium chloride PDDA (polyelectrolyte) solution (concentration of 5.25 mg / mL) (the weight ratio of activated carbon to polyelectrolyte in the polyelectrolyte solution was 38.1:1), and the mixture was stirred at room temperature for 60 min and then filtered, and then placed in an oven at a constant temperature of 80° C. and dried for 24 h to obtain activated carbon loaded with PPDA (PDDA / AC); Step S21) 15 g of PDDA / AC was mixed with 16.65 mL of hexahydrate chloroplatinic acid H2PtCl6·6H2O (precious metal salt) solution (concentration of 2.4 mg / mL) to obtain a system (suspension) to be reduced (the mass ratio of the activated carbon loaded with polyelectrolyte to the precious metal salt in the precious metal salt solution was 375:1); Step S22) Take 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 7.6 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 40 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.3:1), mix them evenly to obtain 15 mL of reducing solution; quickly inject the reducing solution into the system to be reduced, continue stirring the reaction for 30 minutes, filter it, and then place it in a constant temperature oven at 80°C for 24 hours to obtain a primary loaded activated carbon; Step S23) 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 7.6 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 40 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.3:1) are taken respectively, and mixed evenly to obtain 15 mL of reducing solution; 15 g of primary loaded activated carbon and 16.65 mL of H2PtCl6·6H2O solution (concentration of 2.4 mg / mL) are mixed (the mass ratio of primary loaded activated carbon to the precious metal salt in the precious metal salt solution is 375:1) to obtain a suspension; the reducing solution is quickly injected into the above suspension, the reaction is continuously stirred for 30 minutes, and then filtered, and then placed in an oven at a constant temperature of 80°C for drying for 24 hours to obtain platinum modified activated carbon (Pt / AC); the mass fraction of platinum in the Pt / AC obtained in this embodiment is 0.2wt% (recorded as 0.2wt%Pt / AC); Step 2) Take 21g of the above MnO x / AC and 9g of the above Pt / AC (i.e., MnO x The mass ratio of Pt / AC to Pt / AC was 7:3), and the materials were evenly stirred by physical rotation mixing to obtain a carbon-based catalyst.
[0057] In this example, manganese oxide activated carbon (MnO x / AC):Mn 2+ The content is 4.68%, Mn 3+ The content is 53.8%, Mn 4+ The content is 41.5%, Mn 3+ / Mn 4+ The ratio is 1.30; the crystalline structure of transition metals includes δ-MnO x ,δ-MnO x Uniformly present on the surface of activated carbon; In Pt / AC: platinum is loaded in activated carbon in the form of nanoparticles; the particle size of the nanoparticles is 1 to 5 nm.
[0058] Example 5 This embodiment provides a method for preparing a carbon-based catalyst, comprising the following steps: Step 1) activated carbon purification step: 40 g of original activated carbon was added to 400 mL of deionized water, soaked for 5 min, filtered, and then placed in an oven at a constant temperature of 80°C for 24 h to obtain purified activated carbon AC; Preparation steps of activated carbon loaded with transition metal oxides: 100mL of ammonium carbonate (NH4)2CO3 solution (concentration of 25mg / mL) was quickly injected into 150mL of potassium permanganate KMnO4 solution (concentration of 66.7mg / mL) (the weight ratio of KMnO4 in potassium permanganate KMnO4 solution to (NH4)2CO3 in ammonium carbonate (NH4)2CO3 solution was about 4:1) and stirred for 5min, then 25g AC was added (the weight ratio of KMnO4 to activated carbon in potassium permanganate KMnO4 solution was 2.5:1) and stirred for a second time at room temperature. After the second stirring time was 60min, it was filtered and then placed in a constant temperature oven at 80℃ for 24h to obtain activated carbon loaded with manganese oxide (MnO x / AC); Preparation steps of activated carbon loaded with precious metals: Step S1) 15 g AC was added to 75 mL polydiallyl dimethylpropyl ammonium chloride PDDA (polyelectrolyte) solution (concentration of 6.3 mg / mL), (the weight ratio of activated carbon to polyelectrolyte in the polyelectrolyte solution was 31.7.1:1), the mixture was stirred and reacted for 60 min at room temperature, filtered, and then placed in an oven at a constant temperature of 80° C. and dried for 24 h to obtain activated carbon loaded with PPDA (PDDA / AC); Step S21) 15 g of PDDA / AC was mixed with 16.65 mL of hexahydrate chloroplatinic acid H2PtCl6·6H2O (precious metal salt) solution (concentration of 2.88 mg / mL) to obtain a system (suspension) to be reduced (the mass ratio of the activated carbon loaded with polyelectrolyte to the precious metal salt in the precious metal salt solution was 312.5:1); Step S22) Take 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 9.1 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 48 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.3:1), mix them evenly to obtain 15 mL of reducing solution; quickly inject the reducing solution into the system to be reduced, continue stirring and reacting for 30 minutes, filter, and then place in a constant temperature oven at 80°C for 24 hours to obtain a primary loaded activated carbon; Step S23) 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 9.1 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 48 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.3:1) are taken respectively, and mixed evenly to obtain 15 mL of reducing solution; 15 g of primary loaded activated carbon and 16.65 mL of H2PtCl6·6H2O solution (concentration of 2.88 mg / mL) are mixed (the mass ratio of primary loaded activated carbon to the precious metal salt in the precious metal salt solution is 312.5:1) to obtain a suspension; the reducing solution is quickly injected into the above suspension, the reaction is continuously stirred for 30 minutes, and then filtered, and then placed in a constant temperature oven of 80°C for drying for 24 hours to obtain platinum modified activated carbon (Pt / AC); the mass fraction of platinum in the Pt / AC obtained in this embodiment is 0.24wt%; (recorded as 0.24wt%Pt / AC) Step 2) Take 21g of the above MnO x / AC and 9g of the above Pt / AC (i.e., MnO x The mass ratio of Pt / AC to Pt / AC was 7:3), and the materials were evenly stirred by physical rotation mixing to obtain a carbon-based catalyst.
[0059] In this example, manganese oxide activated carbon (MnO x / AC):Mn 2+ The content is 4.68%, Mn 3+ The content is 53.8%, Mn 4+ The content is 41.5%, Mn 3+ / Mn 4+ The ratio is 1.30; the crystalline structure of transition metals includes δ-MnO x ,δ-MnO x Uniformly present on the surface of activated carbon; In Pt / AC: platinum is loaded in activated carbon in the form of nanoparticles; the particle size of the nanoparticles is 1 to 5 nm.
[0060] The following experiments were conducted on the carbon-based catalysts prepared with different Pt loadings in Examples 1 to 5 of the present invention to obtain the effects of different Pt loadings on the HCHO removal efficiency.
[0061] The experimental conditions are as follows: 0.3 g of the carbon-based catalyst in the embodiment is placed in the middle of quartz wool in a stainless steel thermocouple tube with a diameter of 5 mm; a stable HCHO gas flow with a concentration of 100 ppm is generated by a formalin solution (37 vol% HCHO) and a carrier gas (21 vol% O2 and 79 vol% N2 balanced, relative humidity (RH) of 25%); the total flow rate is 100 mL / min, the corresponding weight hourly space velocity (WHSV) is 60 L / (gcath), and the reaction time is 12 h. The initial and outlet concentrations of HCHO and CO2 at the outlet are measured by a real-time photoacoustic infrared multi-gas detector (LumaSense INNOVA, model 1512, the detection limits of HCHO and CO2 are 0.02 and 5.1 ppm, respectively), and the degradation efficiency is calculated.
[0062] Test results such as Figure 1 As shown, it can be seen that as the platinum loading in the platinum-modified activated carbon increases, the catalytic effect gradually improves. However, when a certain ratio is reached, the Pt nanoparticles begin to agglomerate, the exposed surface becomes smaller, and thus the catalytic efficiency also decreases. Therefore, the preferred Pt loading in the carbon-based catalyst of the present invention is 0.18-0.22 wt% (i.e., the mass fraction of platinum in Pt / AC is preferably 0.18-0.22 wt%).
[0063] Comparative Example 1 This comparative example provides a method for preparing a carbon-based catalyst, comprising the following steps: Step 1) activated carbon purification step: 40 g of original activated carbon was added to 400 mL of deionized water, soaked for 5 min, filtered, and then placed in an oven at a constant temperature of 80°C for 24 h to obtain purified activated carbon AC; Preparation steps of activated carbon loaded with transition metal oxides: 100mL of ammonium carbonate (NH4)2CO3 solution (concentration of 25mg / mL) was quickly injected into 150mL of potassium permanganate KMnO4 solution (concentration of 66.7mg / mL) (the weight ratio of KMnO4 in potassium permanganate KMnO4 solution to (NH4)2CO3 in ammonium carbonate (NH4)2CO3 solution was about 4:1) and stirred for 5min, then 25g AC was added (the weight ratio of KMnO4 to activated carbon in potassium permanganate KMnO4 solution was 2.5:1) and stirred for a second time at room temperature. After the second stirring time was 60min, it was filtered and then placed in a constant temperature oven at 80℃ for 24h to obtain activated carbon loaded with manganese oxide (MnO x / AC); Preparation steps of activated carbon loaded with precious metals: Step S1) 15 g AC was added to 75 mL polydiallyl dimethylpropyl ammonium chloride PDDA (polyelectrolyte) solution (concentration of 5.25 mg / mL) (the weight ratio of activated carbon to polyelectrolyte in the polyelectrolyte solution was 38.1:1), and the mixture was stirred at room temperature for 60 min and then filtered, and then placed in an oven at a constant temperature of 80° C. and dried for 24 h to obtain activated carbon loaded with PPDA (PDDA / AC); Step S21) 15 g of PDDA / AC was mixed with 16.65 mL of hexahydrate chloroplatinic acid H2PtCl6·6H2O (precious metal salt) solution (concentration of 2.4 mg / mL) to obtain a system (suspension) to be reduced (the mass ratio of the activated carbon loaded with polyelectrolyte to the precious metal salt in the precious metal salt solution was 375:1); Step S22) Take 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 7.6 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 40 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.3:1), mix them evenly to obtain 15 mL of reducing solution; quickly inject the reducing solution into the system to be reduced, continue stirring the reaction for 30 minutes, filter it, and then place it in a constant temperature oven at 80°C for 24 hours to obtain a primary loaded activated carbon; Step S23) 7.5 mL of sodium borohydride (NaBH4) solution (concentration of 7.6 mg / mL) and 7.5 mL of sodium hydroxide (NaOH) solution (concentration of 40 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.3:1) are taken respectively, and mixed evenly to obtain 15 mL of reducing solution; 15 g of primary loaded activated carbon and 16.65 mL of H2PtCl6·6H2O solution (concentration of 2.4 mg / mL) are mixed (the mass ratio of primary loaded activated carbon to the precious metal salt in the precious metal salt solution is 375:1) to obtain a suspension; the reducing solution is quickly injected into the above suspension, the reaction is continuously stirred for 30 minutes, and then filtered, and then placed in a constant temperature oven of 80°C for drying for 24 hours to obtain platinum modified activated carbon (Pt / AC); the mass fraction of platinum in the Pt / AC obtained in this embodiment is 0.2wt% (recorded as 0.2wt%Pt / AC); Step 2) Take 15g of the above MnO x / AC and 15g of the above Pt / AC (i.e., MnO x The mass ratio of Pt / AC to Pt / AC was 1:1), and the materials were evenly stirred by physical rotation mixing to obtain a carbon-based catalyst.
[0064] In this comparative example, activated carbon of manganese oxide (MnO x / AC):Mn2+ The content is 4.68%, Mn 3+ The content is 53.8%, Mn 4+ The content is 41.5%, Mn 3+ / Mn 4+ The ratio is 1.30; the crystalline structure of transition metals includes δ-MnO x ,δ-MnO x Uniformly present on the surface of activated carbon; In Pt / AC: platinum is loaded in activated carbon in the form of nanoparticles; the particle size of the nanoparticles is 1 to 5 nm.
[0065] Under the above experimental conditions, the formaldehyde removal rate of the carbon-based catalyst in this comparative example was calculated to be 63.4%, which was much lower than the 87.6% formaldehyde removal rate of the carbon-based catalyst in Example 4. This is because the MnO x / AC content is high, MnO x / AC's stable formaldehyde removal ability can only be maintained for 24 hours, so the formaldehyde removal rate is low.
[0066] Comparative Example 2 This comparative example provides a method for preparing a carbon-based catalyst, comprising the following steps: Step 1) 40 g of the original activated carbon was added to 400 mL of deionized water, soaked for 5 min, filtered, and then placed in an oven at a constant temperature of 80° C. for 24 h to obtain purified activated carbon AC; Step S1) adding 15 g AC to 75 mL polydiallyl dimethylpropyl ammonium chloride PDDA (polyelectrolyte) solution (concentration of 5.25 mg / mL) (the weight ratio of activated carbon to polyelectrolyte in the polyelectrolyte solution is 38.1:1), stirring and reacting at room temperature for 60 min, filtering, and then drying in an oven at a constant temperature of 80° C. for 24 h to obtain activated carbon loaded with PPDA (PDDA / AC); Step S21) 15 g of PDDA / AC was mixed with 33.3 mL of chloroplatinic acid hexahydrate (H2PtCl6·6H2O) solution (concentration of 2.4 mg / mL) to obtain a system (suspension) to be reduced (the mass ratio of the activated carbon loaded with polyelectrolyte to the noble metal salt in the noble metal salt solution was 187.7:1); Step S22) Take 15 mL of sodium borohydride (NaBH4) solution (concentration of 7.6 mg / mL) and 15 mL of sodium hydroxide (NaOH) solution (concentration of 40 mg / mL) (the weight ratio of NaOH in the sodium hydroxide NaOH solution to NaBH4 in the sodium borohydride NaBH4 solution is about 5.3:1), mix them evenly to obtain 15 mL of reducing solution; quickly inject the reducing solution into the system to be reduced, continue stirring to react for 30 minutes, then filter, and then place it in a constant temperature oven at 80°C for 24 hours to obtain platinum-modified activated carbon (Pt / AC), that is, the carbon-based catalyst of this comparative example.
[0067] In the Pt / AC of this comparative example: platinum is loaded in the activated carbon in the form of nanoparticles; the particle size of the nanoparticles is 4 to 17 nm.
[0068] The one-time loading of precious metals leads to more serious agglomeration of precious metal nanoparticles on the catalyst surface. The larger particle size of the nanoparticles reduces the relative area of precious metal exposure, reduces atomic utilization, and reduces the contact area with formaldehyde molecules, which is not conducive to catalysis.
[0069] Using the above experimental conditions, the formaldehyde removal rate of the carbon-based catalyst in this comparative example was calculated to be 85.3%, which is a significant decrease compared to the 99.8% formaldehyde removal rate of Pt / AC obtained by double loading. At the same time, since only platinum-loaded activated carbon is used, the preparation cost is relatively high.
[0070] Comparative Example 3 This comparative example provides a method for preparing a carbon-based catalyst, comprising the following steps: 40 g of the original activated carbon was added to 400 mL of deionized water, soaked for 5 min, filtered, and then placed in an oven at a constant temperature of 80 ° C for 24 h to obtain the purified activated carbon AC; 150 mL of potassium permanganate KMnO4 solution (concentration of 66.7 mg / mL) and 33.3 mL of hexahydrate chloroplatinic acid H2PtCl6·6H2O solution (concentration of 2.4 mg / mL) were mixed evenly (the weight ratio of KMnO4 in potassium permanganate KMnO4 solution to the solute in hexahydrate chloroplatinic acid H2PtCl6·6H2O solution was about 125.2:1) to obtain a mixed solution; then 100 mL of ammonium oxalate (NH4)2C2O4 solution (concentration of 2 5 mg / mL, as a reducing agent) was quickly injected into the above mixed solution (the weight ratio of KMnO4 in potassium permanganate KMnO4 solution to (NH4)2C2O4 in ammonium oxalate (NH4)2C2O4 solution was about 4:1) and stirred for 5 to 10 minutes, and then 25 g AC was added and stirred at room temperature for 60 to 120 minutes, then filtered, and then placed in a constant temperature oven at 60 to 80°C for drying for 24 to 48 hours to obtain modified activated carbon, i.e., the carbon-based catalyst of this comparative example.
[0071] In this comparative example, activated carbon of manganese oxide (MnO x / AC):Mn 2+ The content is 40.26%, Mn 3+ The content is 20.7%, Mn 4+ The content is 39.04%, Mn 3+ / Mn 4+ The ratio is 0.53; in Pt / AC: platinum is loaded in the activated carbon in the form of nanoparticles; the particle size of the nanoparticles is 2 to 7 nm.
[0072] Mn 3+ and Mn 4+ It can promote the chemical adsorption, activation and dissociation of O2 on the catalyst surface, thereby generating more active free radical oxygen vacancies OVs that enter the oxide lattice, and then mineralize the formaldehyde molecules into non-toxic H2O and CO2. However, in this method, Mn 2+ The largest proportion, Mn 3+ / Mn 4+ The ratio is smaller; The formaldehyde purification performance of the modified activated carbon (carbon-based catalyst) obtained in this comparative example was evaluated according to the following test conditions: 0.3 g of the obtained carbon-based catalyst was placed in the middle of quartz wool in a stainless steel thermocouple tube with a diameter of 5 mm. A stable HCHO gas flow with a concentration of 100 ppm was generated by formalin solution (37 vol% HCHO) and carrier gas (21 vol% O2 and 79 vol% N2 balanced, relative humidity (RH) of 25%). The total flow rate was 100 mL / min, and the corresponding weight hourly space velocity (WHSV) was 60 L / (gcath). The reaction time was 12 h.
[0073] The formaldehyde removal rate of the modified activated carbon in this comparative example is 80.4%. Compared with the formaldehyde removal rate of 87.6% of the carbon-based catalyst in Example 4, it is much lower. In order to simultaneously reduce the precious metal salt and permanganate under safe conditions to avoid explosion, this comparative example selects ammonium oxalate with weak reducibility and certain weak acidity as a reducing agent. However, since the precious metal salt and permanganate have different chemical properties, weak acid reducing agents such as ammonium oxalate are only more suitable for reducing permanganate. In the process of constructing a uniformly dispersed precious metal active site catalyst, in order to achieve the successful loading of the precious metal, the required environment is often an alkaline environment. In the preparation process of the catalyst, different pH values and different environments provided have a certain influence on the protonation, crystal structure and electron distribution of certain catalysts. As shown in formula (1), in the process of preparing the catalyst by impregnation, the chloride salt or acid solution of the precious metal is first impregnated and then neutralized with an alkaline solution, which will be converted into hydroxide and precipitated on the pore surface of the carrier, which is conducive to the removal of chloride ions, thereby improving the activity of the catalyst, so the appropriate pH value is crucial to the preparation of the catalyst.
[0074] (1) Therefore, the formaldehyde removal rate of the modified activated carbon obtained by using weakly acidic ammonium oxalate as a reducing agent in this comparative example is low. In addition, transition metal manganese and precious metal platinum exist in the raw and auxiliary materials during the preparation process. The presence of metal manganese will occupy the active center of the precious metal to a certain extent, causing the temporary deactivation of the precious metal that plays a major catalytic role, thereby affecting the catalytic performance of the catalyst.
[0075] The applicant also studied the effect of different addition amounts of carbon-based catalyst on the HCHO degradation efficiency. The carbon-based catalyst used was MnO prepared in Example 4. x Carbon-based catalysts supported in concert with platinum.
[0076] Specifically, 0.05g, 0.1g, 0.2g, 0.25g and 0.3g of the synergistically loaded carbon-based catalyst were placed in the middle of quartz wool in a stainless steel thermocouple tube with a diameter of 5mm. The effect of different catalyst addition amounts on the HCHO removal efficiency was studied. Other experimental conditions: A stable HCHO gas flow with a concentration of 100ppm was generated by formalin solution (37vol% HCHO) and carrier gas (21vol% O2 and 79vol% N2 balanced, relative humidity (RH) of 25%). The total flow rate was 100mL / min, and the corresponding weight hourly space velocity (WHSV) was 60L / (gcath) and the reaction time was 12h.
[0077] The test results are as follows Figure 2As shown, it can be seen that with the increase in the amount of carbon-based catalyst added, the catalytic effect gradually improves. Under the premise of keeping other experimental conditions the same, the catalyst addition amount is 0.25g, the reaction time is 12h, and the HCHO removal efficiency at room temperature can reach 87.6%. Further increasing the addition amount does not significantly improve the catalytic effect. Therefore, the addition amount of the carbon-based catalyst prepared in this application is preferably 0.25-0.30g.
[0078] The applicant selected MnO prepared in Example 4 x The following experiment was conducted with a carbon-based catalyst co-loaded with platinum to study the effect of different reaction times on the removal efficiency of formaldehyde (HCHO). Experimental conditions: 0.3g of carbon-based catalyst was placed in the middle of quartz wool in a stainless steel thermocouple tube with a diameter of 5mm. A stable HCHO gas flow with a concentration of 100ppm was generated by formalin solution (37vol% HCHO) and carrier gas 21vol% O2 and 79vol% N2 balanced, with a relative humidity (RH) of 25%). The total flow rate was 100mL / min, and the corresponding weight hourly space velocity (WHSV) was 60L / (gcath). The reaction time was controlled to 3h, 6h, 12h, 18h, and 24h, respectively.
[0079] The carbon-based catalyst obtained in Example 4 can achieve an HCHO removal efficiency of more than 98% in as short as 1 minute. The long-term test conducted so far has shown that the HCHO removal efficiency has been stably maintained at >80% for a long time up to 21 days. Therefore, compared with the prior art, the catalyst of the present application can make the reaction time longer.
[0080] In addition, the carbon-based catalyst of the present invention can also be used to remove other volatile organic pollutants (such as aromatic hydrocarbon pollutants) in indoor air except HCHO.
[0081] The applicant selected MnO prepared in Example 4 x The carbon-based catalyst co-loaded with platinum was studied for its removal effect on other volatile organic pollutants in the air (except HCHO). Specifically, the aromatic hydrocarbon pollutant toluene (C6H5CH3) was taken as an example. 0.3g of the carbon-based catalyst was placed in the middle of the quartz wool of a homemade 5mm diameter British tube (high temperature resistant) reactor. A stable C7H8 gas flow with a concentration of 1000mg / m3 was generated by an analytical pure C7H8 solution and a carrier gas (21vol%O2 and 79vol%N2 balanced, relative humidity (RH) of 50%). The total flow rate was 120mL / min. The reaction time was 12h. The initial and outlet concentrations of C6H5CH3 and CO2 were measured by a real-time photoacoustic infrared multi-gas detector (LumaSenseINNOVA, model 1512, the detection limits of C6H5CH3 and CO2 were 0.02 and 5.1ppm respectively), and the degradation efficiency was calculated.
[0082] Compared with unmodified purified activated carbon (AC), the carbon-based catalyst of Example 4 of the present invention has significantly improved C6H5CH3 catalytic reaction activity. At 152°C and 172°C, the removal rate of C6H5CH3 increased from 45% and 79% to 50% and 92%, respectively.
[0083] The applicant also tested the stability of the carbon-based catalyst of the present invention. x The carbon-based catalyst supported in coordination with platinum is washed with pure water and ethanol after each reaction (i.e., after the catalytic reaction), dried and used again as a room temperature catalyst for HCHO degradation to react, and the above process is regarded as a cycle, and the previous reaction cycle is repeated multiple times. After each reaction, the degradation efficiency is calculated, and the relative change in the HCHO removal efficiency in each reaction cycle is used as an evaluation standard for evaluating the stability of the coordinated supported carbon-based catalyst of the present invention.
[0084] After repeating the above reaction cycle for 5 times, the catalyst addition amount was 0.30 g, the reaction time was 12 h, and the HCHO removal efficiency at room temperature was still able to reach 75%, proving that the carbon-based catalyst of the present invention has good practical application stability and reliability.
[0085] It is easy for those skilled in the art to understand that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.
[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a carbon-based catalyst, It is characterized in that The following steps are involved: Step 1) preparing activated carbon loaded with transition metal oxides; preparing activated carbon loaded with noble metals; Step 2) mixing the activated carbon loaded with transition metal oxides with the activated carbon loaded with noble metals to obtain a carbon-based catalyst; The mass ratio of the activated carbon loaded with transition metal oxides to the activated carbon loaded with noble metals is 6.5-7.5:2.5-3.
5.
2. The method for preparing the carbon-based catalyst according to claim 1, It is characterized in that In the step 1), the step of preparing activated carbon loaded with transition metal oxides comprises: The transition metal salt solution and the buffer solution are mixed and reacted to obtain a mixed solution; then the mixed solution is used to impregnate the activated carbon, and then filtered and dried to obtain the activated carbon loaded with the transition metal oxide.
3. The method for preparing the carbon-based catalyst according to claim 2, It is characterized in that Stirring is performed during the mixing reaction; the stirring time is 5 to 10 minutes.
4. The method for preparing the carbon-based catalyst according to claim 2, It is characterized in that The step of impregnating the activated carbon with the mixed solution comprises: Add activated carbon to the mixed solution at room temperature and stir; the stirring time is 60 to 120 minutes.
5. The method for preparing the carbon-based catalyst according to claim 2, It is characterized in that The temperature of the drying treatment is 60 to 80° C.; the time of the drying treatment is 24 to 48 hours.
6. The method for preparing a carbon-based catalyst according to any one of claims 2 to 5, It is characterized in that The transition metal salt solution is potassium permanganate KMnO 4 solution; and / or The buffer solution is ammonium carbonate (NH 4 ) 2 CO 3 solution; and / or In the activated carbon loaded with transition metal oxides: Mn 2+ The content is 4.28%~5.08%, Mn 3+ The content is 51.8%~54.8%, Mn 4+ The content is 40.12%~43.92%, Mn 3+ / Mn 4+ The ratio is 1.08~1.37; the crystal structure of manganese includes δ-MnO x , the δ-MnO x Uniformly present on the surface of activated carbon; and / or When the transition metal salt solution and the buffer solution are mixed and reacted, the weight ratio of the transition metal salt in the transition metal salt solution to the buffer in the buffer solution is 3.5:1 to 4.5:1; and / or When the mixed solution is used to impregnate the activated carbon, the weight ratio of the transition metal salt to the activated carbon in the transition metal salt solution is 2:1 to 3:
1.
7. The method for preparing a carbon-based catalyst according to claim 6, It is characterized in that The concentration of the transition metal salt solution is 65.7 to 67.7 mg / mL; and / or The concentration of the buffer solution is 20-30 mg / mL.
8. The method for preparing a carbon-based catalyst according to claim 1, It is characterized in that In the step 1), the step of preparing activated carbon loaded with precious metals comprises: Step S1) impregnating activated carbon with a polyelectrolyte solution, filtering and drying the activated carbon to obtain activated carbon loaded with polyelectrolyte; Step S2) The activated carbon loaded with the polyelectrolyte is mixed with a noble metal salt solution and a reducing agent solution to obtain activated carbon loaded with the noble metal.
9. The method for preparing a carbon-based catalyst according to claim 8, It is characterized in that In the step S1), the immersion treatment includes: Add activated carbon to the polyelectrolyte solution at room temperature and stir; The weight ratio of the activated carbon to the polyelectrolyte in the polyelectrolyte solution is 31.7:1 to 95.5:1; and the stirring time is 60 to 120 minutes.
10. The method for preparing a carbon-based catalyst according to claim 8, It is characterized in that In the step S1), the drying temperature is 60 to 80° C. and the drying time is 24 to 48 hours.
11. The method for preparing a carbon-based catalyst according to claim 8, It is characterized in that The step S2) comprises: Step S21) mixing the activated carbon loaded with polyelectrolyte with a noble metal salt solution to form a system to be reduced; Step S22) mixing the system to be reduced with the reducing agent solution to perform a reduction reaction; after the reduction reaction is completed, filtering and drying are performed to obtain primary loaded activated carbon; Step S23) The primary loaded activated carbon is mixed with a noble metal salt solution and a reducing agent solution for reaction, and then filtered and dried to obtain activated carbon loaded with noble metals.
12. The method for preparing a carbon-based catalyst according to claim 11, It is characterized in that In the step S21), the mass ratio of the activated carbon loaded with polyelectrolyte to the noble metal salt in the noble metal salt solution is 312.5:1 to 937.5:
1.
13. The method for preparing a carbon-based catalyst according to claim 11, It is characterized in that In the step S22), the drying temperature is 60 to 80° C. and the drying time is 24 to 48 hours.
14. The method for preparing a carbon-based catalyst according to claim 11, It is characterized in that In the step S23), the drying temperature is 60 to 80° C. and the drying time is 24 to 48 hours.
15. A method for preparing a carbon-based catalyst according to any one of claims 8 to 14, It is characterized in that The polyelectrolyte is polydiallyl dimethyl propyl ammonium chloride (PDDA); and / or The noble metal salt is selected from chloroplatinic acid hexahydrate 2 PtCl 6 6H 2 O; and / or The reducing agent solution is sodium borohydride NaBH 4 The solution is mixed with a sodium hydroxide NaOH solution; and / or The mass fraction of the noble metal in the noble metal-loaded activated carbon is 0.18-0.22 wt %.
16. The method for preparing a carbon-based catalyst according to claim 15, It is characterized in that Sodium hydroxide NaOH solution NaOH and sodium borohydride NaBH 4 NaBH in solution 4 The weight ratio is 5:1 to 5.4:1; and / or The concentration of the polydiallyl dimethyl propyl ammonium chloride (PDDA) solution is 2.10 to 6.30 mg / mL; and / or Chloroplatinic acid hexahydrate 2 PtCl 6 6H 2 The concentration of O solution is 0.96-2.88 mg / mL; and / or Sodium borohydride NaBH 4 The concentration of the solution is 3.0 to 9.1 mg / mL; and / or The concentration of the sodium hydroxide NaOH solution is 16-48 mg / mL.
17. The method for preparing a carbon-based catalyst according to claim 1, It is characterized in that Before step 1), a purification step of activated carbon is also included: The original activated carbon is added into deionized water for soaking, and then filtered and dried to obtain purified activated carbon.
18. The method for preparing a carbon-based catalyst according to claim 1, It is characterized in that In the activated carbon loaded with precious metals: the precious metals are loaded in the activated carbon in the form of nanoparticles.
19. The method for preparing a carbon-based catalyst according to claim 18, It is characterized in that The particle size of the nanoparticles is 1 to 5 nm.
20. A carbon-based catalyst, It is characterized in that The carbon-based catalyst is obtained by mixing activated carbon loaded with transition metal oxides and activated carbon loaded with precious metals; The carbon-based catalyst is obtained by the preparation method according to any one of claims 1 to 19.
21. The carbon-based catalyst according to claim 20, It is characterized in that The transition metal oxide is manganese oxide; in the activated carbon loaded with transition metal oxide: Mn 2+ The content is 4.28%~5.08%, Mn 3+ The content is 51.8%~54.8%, Mn 4+ The content is 40.12%~43.92%, Mn 3+ / Mn 4+ The ratio is 1.08~1.37; the crystalline structure of transition metals includes δ-MnO x , the δ-MnO x Uniformly present on the surface of activated carbon.
22. The carbon-based catalyst according to claim 20 or 21, It is characterized in that In the activated carbon loaded with precious metals: the precious metals are loaded in the activated carbon in the form of nanoparticles; the particle size of the nanoparticles is 1 to 5 nm.
23. Use of the carbon-based catalyst according to any one of claims 20 to 22, It is characterized in that The carbon-based catalyst is used for removing indoor formaldehyde at room temperature.
24. A formaldehyde removal material, It is characterized in that The formaldehyde removal material is the carbon-based catalyst described in any one of claims 20 to 22.
Citation Information
Patent Citations
Preparation method of noble metal catalyst used for HPO process synthesized hydroxylamine phosphate
CN106732557A
Normal-temperature catalytic formaldehyde removal material and preparation method thereof, formaldehyde removal kit and air purification equipment
CN111957309A
Supported normal-temperature formaldehyde removal catalyst, preparation method thereof, formaldehyde removal kit and air purification equipment
CN111974451A
Normal-temperature formaldehyde removal catalyst as well as preparation method and application thereof
CN112604686A
Reducing noble metal loaded manganese oxide catalyst for catalytic combustion of multi-component organic waste gas and preparation method of reducing noble metal loaded manganese oxide catalyst