Preparation method and application of sludge smoldering submicron rod denitration and desulfurization catalyst

By combining modified submicron rod TiO2@Al2O3 carrier and V2O5/CeO2 and Fe2O3/MnO2 composite oxides, an efficient sludge smelting submicron rod denitrogenation desulfurization catalyst was prepared, solving the insufficient catalytic activity in medium and low temperatures and anti-sulfur poisoning. The problem of poor ability achieves efficient removal of NOx and SO2 in flue gas and economic benefits.

CN119034760APending Publication Date: 2024-11-29NANJING TECH UNIV +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411386858.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

There are problems of insufficient catalytic activity of flue gas disposal and medium- and low-temperature denitrification catalysts during the existing sludge smoldering process, and commercial vanadium-based catalysts have poor low-temperature activity and poor anti-sulfur poisoning ability.

Method used

The modified submicron rod TiO2@Al2O3 is used as the support, the composite oxides of V2O5 and CeO2 are used as the active components, and the composite oxides of Fe2O3 and MnO2 are used as the cocatalysts, and the sludge smelting is prepared through hydrothermal reaction and calcination process. The submicron rod denitrogenation and desulfurization catalyst is first supported and then supported for active components. It uses a mixed atmosphere of CO and N2 and a calcination atmosphere of SO2 and water vapor to improve the anti-sulfur poisoning performance and catalytic activity of the catalyst.

Benefits of technology

Highly efficient catalyzing of NO reduction and SO2 oxidation at medium and low temperatures achieves the coordinated removal of NOx and SO2, improving the catalyst's anti-water sulfur poisoning performance and service life, reducing costs, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034760A_ABST
    Figure CN119034760A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a sludge smoldering submicron rod denitration and desulfurization catalyst. According to the catalyst, a modified submicron rod TiO2-coated Al2O3 is used as a carrier, a composite oxide of V2O5 and CeO2 is used as an active component, and a composite oxide of Fe2O3 and MnO2 is used as a cocatalyst. The catalyst not only is environment-friendly, but also can synergistically catalyze and remove SO2 and NOx in sludge smoldering flue gas at low temperature, and has important economic benefits and social effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a sludge smoldering submicron rod denitration and desulfurization catalyst, belonging to the field of industrial flue gas purification. Background Art

[0002] At present, biomass combustion in my country will cause VOCs, SO2, NO x , solid particles, solid slag and other emissions are high. SCR method is currently the most commonly used NO x Removal method: The core technology of SCR method is mainly focused on the research and development of new denitration catalysts. Currently, commercial catalysts are mainly divided into two categories: vanadium-based catalysts and rare earth-based catalysts. However, commercial vanadium-based catalysts still have some inevitable defects, such as poor low-temperature activity and poor resistance to sulfur poisoning, which seriously hinder their further development in practical applications. Therefore, it is very important to prepare an environmentally friendly catalyst that overcomes the above shortcomings.

[0003] Among the existing low-temperature denitration patents, patent CN201510488728.8 uses Cr2O3 and V2O5 as active components, NiSO4 as an auxiliary agent, and TiO2 as a carrier to prepare a low-temperature denitration catalyst, which improves the chemical adsorption capacity of NH3 at low temperatures, thereby improving the catalyst activity, while reducing the conversion rate of SO2 / SO3 and extending the service life of the low-temperature denitration catalyst. Patent CN201811654451.1 prepares a ruthenium-based ultra-low temperature denitration catalyst by segmented impregnation and roasting, achieving good denitration effect under ultra-low temperature conditions, significantly improving anti-poisoning performance, and having the advantages of long service life. Patent CN201710773182.X obtains a low-temperature denitration catalyst by loading metal oxides with nitrogen-doped graphene, which has a good denitration effect under low temperature conditions and can effectively combat sulfur dioxide. Although the above catalysts achieve high catalytic activity at low temperatures, the catalysts are expensive and not suitable for large-scale industrial applications. On the other hand, patent CN201610435984.5 discloses a method for treating flue gas from biomass pellet combustion, which only removes particulate matter in the flue gas and does not mention the treatment of incompletely burned gases. Patent CN201910522702.9 discloses a method for treating smoldering organic solid waste and purifying flue gas, which uses the addition of fuel gas to treat the flue gas. However, in small batch equipment, it is difficult to implement the regulation of the mixture of fuel gas and non-steady-state flue gas. Summary of the invention

[0004] The purpose of the present invention is to address the current problems of flue gas disposal in the sludge smoldering process and the insufficient catalytic activity of medium and low temperature denitrification catalysts, and propose a preparation method and application of a sludge smoldering submicron rod denitrification and desulfurization catalyst.

[0005] A sludge smoldering submicron rod denitrification and desulfurization catalyst, the catalyst uses modified submicron rod TiO2@Al2O3 as a carrier, a composite oxide of V2O5 and CeO2 as an active component, and a composite oxide of Fe2O3 and MnO2 as a co-catalyst;

[0006] Based on the mass of the carrier, the mass percentage of the active component is 1-10%, the mass ratio of V2O5 and CeO2 in the active component is 1:0.5-5, the mass percentage of the co-catalyst is 10-40%, the mass ratio of Fe2O3 and MnO2 in the co-catalyst is 1:1-25, and the mass ratio of TiO2 and Al2O3 in the carrier is 1:0.5-5.

[0007] In some preferred technical schemes: based on the mass of the carrier, the mass percentage of the active component is 1-3%, the mass ratio of V2O5 and CeO2 in the active component is 1:0.5-1, the mass percentage of the co-catalyst is 10-20%, the mass ratio of Fe2O3 and MnO2 in the co-catalyst is 1:1-2, and the mass ratio of TiO2 and Al2O3 in the carrier is 1:0.5-1.

[0008] A method for preparing the above-mentioned sludge smoldering submicron rod denitrification and desulfurization catalyst, the preparation method of the catalyst is as follows:

[0009] (1) Preparation of submicron rod carriers

[0010] The Al2O3 nanorod fibers, deionized water and oxalic acid are mixed and then subjected to a hydrothermal reaction. After the hydrothermal reaction is completed, the modified Al2O3 nanorod fibers are filtered and dried to obtain the modified Al2O3 nanorod fibers. The modified Al2O3 nanorod fibers, titanium source, anhydrous ethanol and dilute hydrochloric acid solution are mixed and then subjected to a second hydrothermal reaction to obtain a submicron rod TiO2@Al2O3 carrier.

[0011] The submicron rod TiO2@Al2O3 carrier is placed in a muffle furnace for high temperature calcination, the calcined carrier is added into a dilute sulfuric acid solution and placed in a hydrothermal reactor for a third hydrothermal reaction, and the modified submicron rod TiO2@Al2O3 carrier is obtained after drying;

[0012] (2) Catalyst loading

[0013] Weigh iron salt and manganese salt, dissolve them in deionized water and stir them evenly to obtain a catalyst precursor solution, then place the modified submicron rod TiO2@Al2O3 carrier obtained in step (1) in the catalyst precursor solution, immerse and dry;

[0014] After drying, the catalyst is placed in a tubular atmosphere furnace and calcined with a mixture of CO and N2 as the calcination atmosphere, and then calcined again with a mixture of SO2, water vapor and N2 as the calcination atmosphere, thereby obtaining a catalyst-supported carrier;

[0015] (3) Active component loading

[0016] Weigh cerium salt, vanadium salt and monohydrated citric acid, dissolve in deionized water and stir evenly to obtain an active component precursor mixed solution, then place the co-catalyst loaded carrier prepared in step (2) in the active component precursor mixed solution, immerse and dry, and calcine at low temperature to obtain a sludge smoldering submicron rod denitrification and desulfurization catalyst.

[0017] In the technical solution of the present invention: the temperature of the first hydrothermal reaction in step (1) is 120-140° C., and the time of the hydrothermal reaction is 60-120 min;

[0018] The drying temperature is 80-100°C and the drying time is 4-8h.

[0019] The temperature of the second hydrothermal reaction is 140-160°C, and the time of the second hydrothermal reaction is 4-6 hours;

[0020] The temperature of high temperature roasting is 600-800°C, and the time of high temperature roasting is 2-4h;

[0021] The temperature of the third hydrothermal reaction is 100-120°C, and the time of the third hydrothermal reaction is 30-60 minutes.

[0022] In the technical scheme of the present invention: the iron salt described in step (2) is one of ferric nitrate nonahydrate or ferric chloride hexahydrate, and the manganese salt is one of manganese chloride or manganese nitrate hexahydrate; the drying temperature is 80-100° C., and the drying time is 4-8 hours;

[0023] The volume ratio of CO and N2 described in step (2) is 1-2:100, the rate at which the mixed gas of CO and N2 is introduced into the tubular reactor is 20-40 mL / min, the calcination temperature is 500-600°C, and the calcination time is 2-4 h.

[0024] The volume ratio of SO2, water vapor and N2 described in step (2) is 1-2:3-5:100, the rate at which the mixed gas of SO2, water vapor and N2 is introduced into the tubular reactor is 20-40 mL / min, the temperature of the secondary calcination is 500-600°C, and the time of the secondary calcination is 2-4 h.

[0025] In the technical solution of the present invention: the cerium salt described in step (3) is one of cerium nitrate hexahydrate or cerium chloride hexahydrate, and the vanadium salt is ammonium metavanadate;

[0026] The drying temperature is 80-100°C, and the drying time is 4-8 hours; the low-temperature roasting temperature is 350-450°C, and the low-temperature roasting time is 3-6 hours.

[0027] In the technical solution of the present invention, the catalyst is used in the desulfurization and denitrification of flue gas; preferably, the flue gas is the smoke generated during the smoldering process of sludge.

[0028] In the technical solution of the present invention, the catalyst carrier is first loaded with a co-catalyst and then loaded with an active component. The reason for this design is that the active component mainly provides catalytic activity, and the co-catalyst improves the catalytic activity and plays a major role in improving the anti-sulfur poisoning performance. If the active component is loaded first and then the co-catalyst is loaded, then when SO2 and water vapor are used as an atmosphere for roasting, SO2 will also react with the active component to generate sulfate, which will reduce the catalytic activity.

[0029] In the technical solution of the present invention, ammonium metavanadate and cerium nitrate or cerium chloride will form an acid-base reaction in an aqueous solution to generate a precipitate, and citric acid monohydrate is used to allow ammonium metavanadate and cerium nitrate or cerium chloride to form a complex, and the vanadium salt and the cerium salt will not react during the preparation, so the role of citric acid monohydrate is to improve its ability to be evenly dispersed on the carrier.

[0030] The experimental conditions for evaluating the activity of the catalyst of the present invention are as follows: 1 mL of a 40-60 mesh catalyst is taken and poured into a quartz tube with an inner diameter of 8 mm, the quartz tube is placed in a tubular furnace, and the actual temperature of the catalytic reaction is adjusted by controlling the heating temperature of the tubular furnace. Intake gas components: NO (500 ppm), SO2 (200 ppm), NH3 (500 ppm), O2 (11 vol.%), and the rest are N2, the total gas flow rate is 500 mL / min, the temperature is controlled at 120-300°C, and it stays stable for 30 minutes every 30°C. The concentrations of NO and SO2 are tested using a Laoying 3021 portable carbon emission monitor. At 150-240°C, the NO conversion rate is 100% after 3 minutes, and the SO2 conversion rate is higher than 90%.

[0031] Beneficial effects:

[0032] The catalyst prepared by the present invention can efficiently catalyze the reduction of NO to generate N2 at medium and low temperatures, and simultaneously catalyze the oxidation of SO2 to generate SO3. Compared with the prior art, the Al2O3 nanorod fiber in the catalyst first undergoes hydrothermal reaction with oxalic acid, and its surface is modified to increase the number of hydroxyl groups on its surface, so that TiO2 can stably grow around Al2O3 during the secondary hydrothermal reaction to obtain a submicron rod TiO2@Al2O3 carrier; and tetrabutyl titanate cannot be completely converted into TiO2 during the hydrothermal reaction, so high-temperature roasting is required, which can not only completely convert tetrabutyl titanate into TiO2, but also further promote the improvement of the bonding strength between TiO2 and Al2O3. In addition, after the submicron rod TiO2@Al2O3 carrier undergoes hydrothermal reaction with a dilute sulfuric acid solution, it can not only slightly corrode TiO2 to make its microscopic surface rough, enhance its hydrophobicity, thereby improving the catalyst's resistance to water sulfur poisoning in smoldering flue gas, but also replace the oxygen atoms on the surface of TiO2 with sulfate, thereby inhibiting the adsorption of SO3 on the catalyst surface, further enhancing its resistance to sulfur poisoning. Finally, according to Tanabe's rule, the composite carrier of TiO2@Al2O3 can enhance the acidity of the catalyst surface, which is beneficial to promote the adsorption of the reaction gas NH3 and inhibit the adsorption of the acidic gas SO3, thereby improving the catalytic activity. After the Fe2O3 and MnO2 precursors are impregnated, they are first calcined using CO as a reducing atmosphere, thereby increasing the oxygen vacancy concentration in the catalyst and enhancing the performance of low-temperature catalytic reduction of NO and catalytic oxidation of SO2; when switching to SO2 and water vapor as the calcination atmosphere, some of the oxygen atoms of the co-catalyst can also be replaced by sulfate. It is well known that both Fe2O3 and MnO2 have excellent catalytic oxidation capabilities, but they are easy to react with SO2 to form sulfates, thereby causing sulfur poisoning of the catalyst. Although replacing some of the oxygen atoms with sulfates in advance will reduce the catalytic activity to a certain extent, O-SO4 2- The strong acidic surface structure can inhibit the adsorption of SO3 from both chemical and physical aspects, so that it will not form sulfate after catalytic oxidation of SO2, resulting in a decrease in the catalytic reduction of NO. After the V2O5 and CeO2 precursors are impregnated, they are converted into composite oxides by low-temperature calcination without affecting the sulfate and oxygen vacancies on the surface of the carrier and the co-catalyst, thereby making full use of the component effects of the carrier, active components and co-catalysts to achieve excellent performance of simultaneous denitration and desulfurization and excellent resistance to water-sulfur poisoning.

[0033] Therefore, the catalyst prepared by the present invention is not only environmentally friendly, but also can convert SO2 and NO in the smoldering flue gas of sludge at medium and low temperatures. x Synergistic catalytic removal has important economic and social effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is the SEM image of the catalyst prepared in Example 1;

[0035] Figure 2 This is the SEM image of the catalyst prepared in Comparative Example 1;

[0036] Figure 3 The NO efficiency diagram of the catalysts prepared in Examples 1, 2 and Comparative Examples 1, 2, and 3;

[0037] Figure 4 The SO2 efficiency diagram of the catalysts prepared in Examples 1, 2 and Comparative Examples 1, 2, and 3;

[0038] Figure 5 The NO efficiency of the catalysts prepared in Example 1 and Comparative Examples 1 and 3 varies with time. DETAILED DESCRIPTION

[0039] The present invention is further described below in conjunction with examples. The examples are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operating processes are given, but the protection scope of the present invention is not limited to the following examples.

[0040] Example 1

[0041] (1) Preparation of submicron rod carriers

[0042] Weigh 2g of Al2O3 nanorod fiber, 60g of deionized water and 6g of oxalic acid, mix them evenly, then place them in a hydrothermal reactor for hydrothermal reaction at 120°C for 120min, filter them after the hydrothermal reaction and place them in an oven for drying at 80°C for 8h to obtain the modified Al2O3 nanorod fiber; weigh 1.5g of the modified Al2O3 nanorod fiber, 12.78g of tetrabutyl titanate, 60g of anhydrous ethanol and 7.5g of a 5% by mass dilute hydrochloric acid solution, mix them evenly, place them in a hydrothermal reactor for secondary hydrothermal reaction at 140°C for 6h to obtain a submicron rod TiO2@Al2O3 carrier; then weigh 4g of the submicron rod TiO2@Al2O3 carrier, place them in a muffle furnace for high temperature calcination at 600°C for 4h, add 80g of a 5% by mass dilute sulfuric acid solution after calcination and place them in a hydrothermal reactor for tertiary hydrothermal reaction at 100°C for 60min to obtain a modified submicron rod TiO2@Al2O3 carrier;

[0043] (2) Catalyst loading

[0044] Weigh 0.76g of ferric nitrate nonahydrate and 0.22g of manganese chloride salt, dissolve them in 7.6g of deionized water and stir them evenly to obtain a catalyst precursor solution, then weigh 3g of the modified submicron rod TiO2@Al2O3 carrier obtained in step (1) and place it in the catalyst precursor solution, dry it at 80°C for 8h after impregnation, then place it in a tubular atmosphere furnace, introduce a mixed gas of CO and N2 (the introduction rate of the mixed gas is 20mL / min, wherein the volume ratio of CO and N2 is 1:100), heat it to 500°C and bake it for 4h, then stop introducing the mixed gas of CO and N2, introduce a mixed gas of SO2, water vapor and N2 (the introduction rate of the mixed gas is 20mL / min, wherein the volume ratio of SO2, water vapor and N2 is 1:3:100) into the tubular atmosphere furnace, and bake it again at 500°C for 4h, thereby obtaining a catalyst-loaded carrier;

[0045] (3) Active component loading

[0046] Weigh 25 mg of cerium nitrate hexahydrate, 26 mg of ammonium metavanadate and 50 mg of citric acid monohydrate, dissolve in 1.5 g of deionized water and stir evenly to obtain an active component precursor mixed solution, then place the promoter-loaded carrier obtained in step (2) in the active component precursor mixed solution, dry at 80°C for 8 h after impregnation, and then place it in a muffle furnace for low-temperature roasting at 350°C for 6 h to obtain a sludge smoldering submicron rod denitrification and desulfurization catalyst (based on the carrier mass, the mass percentage of the active component is 1%, the mass ratio of V2O5 and CeO2 in the active component is 1:0.5, the mass percentage of the promoter is 10%, the mass ratio of Fe2O3 and MnO2 in the promoter is 1:1, and the mass ratio of TiO2 and Al2O3 in the carrier is 1:0.5) (morphology see Figure 1 );

[0047] (4) Catalytic activity test

[0048] Take 1mL of 40-60 mesh catalyst, pour it into a quartz tube with an inner diameter of 8mm, place the quartz tube in a tubular furnace, and adjust the actual temperature of the catalytic reaction by controlling the heating temperature of the tubular furnace. Intake components: NO (500ppm), SO2 (200ppm), NH3 (500ppm), O2 (11vol.%), and the rest are N2. The total gas flow rate is 500mL / min, and the temperature is controlled at 120-300℃. Stay stable for 30min every 30℃. Use Laoying 3021 portable carbon emission monitor to test NO and SO2 concentrations. At 150-240℃, the NO conversion rate is 100% after 3min, and the SO2 conversion rate is higher than 90%. (For specific data, see Figure 3 and Figure 4 ).

[0049] Example 2

[0050] (1) Preparation of submicron rod carriers

[0051] Weigh 2g of Al2O3 nanorod fiber, 80g of deionized water and 10g of oxalic acid, mix them evenly, then place them in a hydrothermal reactor for hydrothermal reaction at 140°C for 60min, filter them after the hydrothermal reaction, place them in an oven for drying at 100°C for 4h to obtain the modified Al2O3 nanorod fiber; weigh 1.5g of the modified Al2O3 nanorod fiber, 4.28g of tetraethyl titanate, 90g of anhydrous ethanol, and 15g of a 2% by mass dilute hydrochloric acid solution, mix them evenly, place them in a hydrothermal reactor for secondary hydrothermal reaction at 160°C for 4h to obtain a submicron rod TiO2@Al2O3 carrier; then weigh 2.5g of the submicron rod TiO2@Al2O3 carrier, place them in a muffle furnace for high temperature calcination at 800°C for 2h, add 75g of a 1% by mass dilute sulfuric acid solution to the calcined carrier, place them in a hydrothermal reactor for tertiary hydrothermal reaction at 120°C for 30min to obtain a modified submicron rod TiO2@Al2O3 carrier;

[0052] (2) Catalyst loading

[0053] Weigh 0.45g of ferric chloride hexahydrate and 0.88g of manganese nitrate hexahydrate, dissolve them in 9g of deionized water and stir them evenly to obtain a catalyst precursor solution, then weigh 2g of the modified submicron rod TiO2@Al2O3 carrier obtained in step (1) and place it in the catalyst precursor solution, dry it at 100°C for 4h after impregnation, then place it in a tubular atmosphere furnace, introduce a mixed gas of CO and N2 (the introduction rate of the mixed gas is 40mL / min, wherein the volume ratio of CO and N2 is 1:50), heat it to 600°C and bake it for 2h, then stop introducing the mixed gas of CO and N2, introduce a mixed gas of SO2, water vapor and N2 (the introduction rate of the mixed gas is 40mL / min, wherein the volume ratio of SO2, water vapor and N2 is 2:5:100) into the tubular atmosphere furnace, and bake it again at 600°C for 2h, thereby obtaining a catalyst-loaded carrier;

[0054] (3) Active component loading

[0055] Weigh 46 mg of cerium chloride hexahydrate, 39 mg of ammonium metavanadate and 138 mg of citric acid monohydrate, dissolve in 1.84 g of deionized water and stir evenly to obtain an active component precursor mixed solution, then place the promoter-loaded carrier obtained in step (2) in the active component precursor mixed solution, dry at 100° C. for 4 h after impregnation, and then place in a muffle furnace for low-temperature roasting at 450° C. for 3 h to obtain a sludge smoldering submicron rod denitrification and desulfurization catalyst (based on the carrier mass, the mass percentage of the active component is 3%, the mass ratio of V2O5 and CeO2 in the active component is 1:1, the mass percentage of the promoter is 20%, the mass ratio of Fe2O3 and MnO2 in the promoter is 1:2, and the mass ratio of TiO2 and Al2O3 in the carrier is 1:1);

[0056] (4) Catalytic activity test

[0057] Take 1mL of 40-60 mesh catalyst, pour it into a quartz tube with an inner diameter of 8mm, place the quartz tube in a tubular furnace, and adjust the actual temperature of the catalytic reaction by controlling the heating temperature of the tubular furnace. Intake components: NO (500ppm), SO2 (200ppm), NH3 (500ppm), O2 (11vol.%), and the rest are N2. The total gas flow rate is 500mL / min, and the temperature is controlled at 120-300℃. Stay stable for 30min every 30℃. Use Laoying 3021 portable carbon emission monitor to test NO and SO2 concentrations. At 150-240℃, the NO conversion rate is 100% after 3min, and the SO2 conversion rate is higher than 90%. (For specific data, see Figure 3 and Figure 4 ).

[0058] Comparative Example 1

[0059] (1) Preparation of carrier

[0060] Except that Al2O3 nanorod fibers were not used in the catalyst preparation, other conditions were the same as those in Example 1;

[0061] (2) Catalytic activity test

[0062] Take 1mL of 40-60 mesh catalyst and pour it into a quartz tube with an inner diameter of 8mm. Place the quartz tube in a tubular furnace and adjust the actual temperature of the catalytic reaction by controlling the heating temperature of the tubular furnace. Intake gas components: NO (500ppm), SO2 (200ppm), NH3 (500ppm), O2 (11vol.%), and the rest are N2. The total gas flow rate is 500mL / min. The temperature is controlled at 120-300℃, and stays stable for 30min every 30℃. The Laoying 3021 portable carbon emission monitor is used to test the NO and SO2 concentrations. At 210-240℃, the NO conversion rate is higher than 80% after 3min, and the SO2 conversion rate reaches 58% at 210℃ (see for specific data). Figure 3 and Figure 4 ).

[0063] (3) Contrast effect

[0064] Compared with Example 1, when the catalyst is prepared without using Al2O3 nanorod fibers, that is, without a template, the carrier does not form a nanorod shape, but forms a submicron block of nanosphere accumulation ( Figure 2 ), the surface acidity of the catalyst will be significantly reduced, and the long-range ordered and short-range disordered state of the microscopic interface will not be formed, so the hydrophobicity will also be significantly reduced, resulting in a decrease in the catalyst's anti-sulfur poisoning performance ( Figure 5 ).

[0065] Comparative Example 2

[0066] (1) Preparation of carrier

[0067] Except that the mixed gas of CO and N2 was not introduced during the catalyst preparation, other conditions were the same as those in Example 2;

[0068] (2) Catalytic activity test

[0069] Take 1mL of 40-60 mesh catalyst and pour it into a quartz tube with an inner diameter of 8mm. Place the quartz tube in a tubular furnace and adjust the actual temperature of the catalytic reaction by controlling the heating temperature of the tubular furnace. Intake gas components: NO (500ppm), SO2 (200ppm), NH3 (500ppm), O2 (11vol.%), and the rest are N2. The total gas flow rate is 500mL / min. The temperature is controlled at 120-300℃, and stays stable for 30min every 30℃. The Laoying 3021 portable carbon emission monitor is used to test the NO and SO2 concentrations. At 210-240℃, the NO conversion rate is higher than 85% after 3min, and the SO2 conversion rate reaches 69% at 210℃ (see for specific data). Figure 3 and Figure 4 ).

[0070] (3) Contrast effect

[0071] Compared with Example 2, if the mixed gas of CO and N2 is not introduced during the preparation of the catalyst, the oxygen vacancy concentration on the catalyst surface will decrease significantly, and the oxygen vacancy concentration is an important factor affecting the catalytic activity, so the NO conversion rate and SO2 conversion rate will decrease significantly.

[0072] Comparative Example 3

[0073] (1) Preparation of carrier

[0074] Except that the mixed gas of SO2, water vapor and N2 was not introduced during the catalyst preparation, other conditions were the same as those in Example 2; (2) Catalytic Activity Test

[0075] Take 1mL of 40-60 mesh catalyst and pour it into a quartz tube with an inner diameter of 8mm. Place the quartz tube in a tubular furnace and adjust the actual temperature of the catalytic reaction by controlling the heating temperature of the tubular furnace. Intake gas components: NO (500ppm), SO2 (200ppm), NH3 (500ppm), O2 (11vol.%), and the rest are N2. The total gas flow rate is 500mL / min. The temperature is controlled at 120-300℃, and stays stable for 30min every 30℃. The Laoying 3021 portable carbon emission monitor is used to test the NO and SO2 concentrations. At 210-240℃, the NO conversion rate is higher than 90% after 3min, and the SO2 conversion rate reaches 93% at 210℃ (see for specific data). Figure 3 and Figure 4 ).

[0076] (3) Contrast effect

[0077] Compared with Example 2, if the mixed gas of SO2, water vapor and N2 is not introduced during the preparation of the catalyst, the oxygen atoms on the surface of the co-catalyst will not be replaced by sulfate. Although the effect on the catalytic activity is small, the lack of O-SO4 2- Due to the strong acidic surface structure, SO3 will gradually react with the catalytic active sites to generate sulfate species during the catalytic reaction of NO and SO2, resulting in a significant decrease in its anti-sulfur poisoning performance ( Figure 5 ).

Claims

1. A sludge smoldering submicron rod denitrification and desulfurization catalyst, characterized in that: The catalyst uses modified submicron rod TiO2@Al2O3 as a carrier, a composite oxide of V2O5 and CeO2 as an active component, and a composite oxide of Fe2O3 and MnO2 as a co-catalyst. Based on the mass of the carrier, the mass percentage of the active component is 1-10%, the mass ratio of V2O5 and CeO2 in the active component is 1:0.5-5, the mass percentage of the co-catalyst is 10-40%, the mass ratio of Fe2O3 and MnO2 in the co-catalyst is 1:1-25, and the mass ratio of TiO2 and Al2O3 in the carrier is 1:0.5-5.

2. The sludge smoldering submicron rod denitrification and desulfurization catalyst according to claim 1, characterized in that: Based on the carrier mass, the mass percentage of the active component is 1-3%, the mass ratio of V2O5 and CeO2 in the active component is 1:0.5-1, the mass percentage of the co-catalyst is 10-20%, the mass ratio of Fe2O3 and MnO2 in the co-catalyst is 1:1-2, and the mass ratio of TiO2 and Al2O3 in the carrier is 1:0.5-1.

3. A method for preparing the sludge smoldering submicron rod denitrification and desulfurization catalyst according to claim 1, characterized in that: The preparation method of the catalyst is as follows: (1) Preparation of submicron rod carriers The Al2O3 nanorod fibers, deionized water and oxalic acid are mixed and then subjected to a hydrothermal reaction. After the hydrothermal reaction is completed, the modified Al2O3 nanorod fibers are filtered and dried to obtain the modified Al2O3 nanorod fibers. The modified Al2O3 nanorod fibers, titanium source, anhydrous ethanol and dilute hydrochloric acid solution are mixed and then subjected to a second hydrothermal reaction to obtain a submicron rod TiO2@Al2O3 carrier. The submicron rod TiO2@Al2O3 carrier is placed in a muffle furnace for high temperature calcination, the calcined carrier is added into a dilute sulfuric acid solution and placed in a hydrothermal reactor for a third hydrothermal reaction, and the modified submicron rod TiO2@Al2O3 carrier is obtained after drying; (2) Catalyst loading Weigh iron salt and manganese salt, dissolve them in deionized water and stir them evenly to obtain a catalyst precursor solution, then place the modified submicron rod TiO2@Al2O3 carrier obtained in step (1) in the catalyst precursor solution, immerse and dry; After drying, the catalyst is placed in a tubular atmosphere furnace and calcined with a mixture of CO and N2 as the calcination atmosphere, and then calcined again with a mixture of SO2, water vapor and N2 as the calcination atmosphere, thereby obtaining a catalyst-supported carrier; (3) Active component loading Weigh cerium salt, vanadium salt and monohydrated citric acid, dissolve in deionized water and stir evenly to obtain an active component precursor mixed solution, then place the co-catalyst loaded carrier prepared in step (2) in the active component precursor mixed solution, immerse and dry, and calcine at low temperature to obtain a sludge smoldering submicron rod denitrification and desulfurization catalyst.

4. The preparation method according to claim 3, characterized in that: The temperature of the first hydrothermal reaction in step (1) is 120-140° C., and the time of the hydrothermal reaction is 60-120 min; The drying temperature is 80-100°C and the drying time is 4-8h. The temperature of the second hydrothermal reaction is 140-160°C, and the time of the second hydrothermal reaction is 4-6 hours; The high temperature roasting temperature is 600-800°C, and the high temperature roasting time is 2-4h; The temperature of the third hydrothermal reaction is 100-120°C, and the time of the third hydrothermal reaction is 30-60 minutes.

5. The preparation method according to claim 3, characterized in that: The iron salt described in step (2) is one of ferric nitrate nonahydrate or ferric chloride hexahydrate, and the manganese salt is one of manganese chloride or manganese nitrate hexahydrate; the drying temperature is 80-100° C., and the drying time is 4-8 hours; The volume ratio of CO and N2 described in step (2) is 1-2:100, the rate at which the mixed gas of CO and N2 is introduced into the tubular reactor is 20-40 mL / min, the calcination temperature is 500-600°C, and the calcination time is 2-4 h. The volume ratio of SO2, water vapor and N2 described in step (2) is 1-2:3-5:100, the rate at which the mixed gas of SO2, water vapor and N2 is introduced into the tubular reactor is 20-40 mL / min, the temperature of the secondary calcination is 500-600°C, and the time of the secondary calcination is 2-4 h.

6. The preparation method according to claim 3, characterized in that: The cerium salt described in step (3) is one of cerium nitrate hexahydrate or cerium chloride hexahydrate, and the vanadium salt is ammonium metavanadate; The drying temperature is 80-100°C, and the drying time is 4-8 hours; the low-temperature roasting temperature is 350-450°C, and the low-temperature roasting time is 3-6 hours.

7. Use of the catalyst according to claim 1 in desulfurization and denitrification in flue gas; preferably, the flue gas is the smoke generated during the smoldering process of sludge.