Apple-shaped microsphere molecular sieve catalyst, preparation method and application thereof, and cyclohexanone-oxime gas phase Beckmann rearrangement reaction method
By preparing apple-shaped microsphere molecular sieve catalysts, the problems of high wear, low conversion rate and short life of existing catalysts have been solved, realizing a highly efficient gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, which meets the needs of industrialization.
Patent Information
- Application Number
- CN202310595456.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-29
AI Technical Summary
Existing catalysts for the gas-phase Beckmann rearrangement of cyclohexanone oxime have high attrition index, low cyclohexanone oxime conversion and caprolactam selectivity, and short catalyst lifetime, which cannot meet the needs of industrialization.
By using apple-shaped microsphere molecular sieve catalysts and controlling the pulping conditions and spray drying process, all-silica molecular sieves with MFI topology and silica binders are prepared to form microsphere catalysts with appropriate pore volume and packing density, avoiding the use of additional additives and improving the strength and flowability of the catalyst.
This catalyst achieves a low attrition index, excellent catalytic performance and stability, improves the conversion rate of cyclohexanone oxime and the selectivity of caprolactam, extends catalyst life, and meets the needs of industrial applications.
Smart Images

Figure CN119034791A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of catalyst preparation, and in particular to an apple-shaped microsphere molecular sieve catalyst, a preparation method and application thereof, and a method for gas-phase Beckmann rearrangement reaction of cyclohexanone oxime. Background Art
[0002] Silica molecular sieve is an aluminum-free molecular sieve with MFI topological structure. It can be used as a membrane separation material and a catalyst for the production of caprolactam by the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime. However, the silica molecular sieve synthesized by the prior art has a high content of amorphous silicon oxide, poor relative crystallinity and large crystal particles.
[0003] Caprolactam is generally obtained through the Beckmann rearrangement reaction of cyclohexanone oxime. The vapor-phase Beckmann rearrangement reaction of cyclohexanone oxime using a solid acid catalyst is a new process for achieving caprolactam production without ammonium sulfide. It has the advantages of no equipment corrosion, no environmental pollution, and no by-product of ammonium sulfide. The separation and purification of the product is also greatly simplified. Therefore, the vapor-phase Beckmann rearrangement reaction process without ammonium sulfide has attracted great attention from industry insiders.
[0004] In order to develop solid acid catalysts suitable for gas-phase Beckmann rearrangement reaction, researchers at home and abroad have conducted a lot of research. The earliest research was on single-component oxides, such as SiO 2 、Al 2 O 3 、ZrO 2 and B 2 O 3 etc., developed into revived oxides, such as B 2 O 3 / SiO 2 , B 2 O 3 / Al 2 O 3 , B 2 O 3 / ZrO 2 、 2 O 5 / SiO 2 , WO 3 / SiO 2 These oxide catalysts all have common problems such as low cyclohexanone oxime conversion rate, low caprolactam selectivity and short catalyst life, which cannot meet the requirements of industrialization.
[0005] In April 2003, Sumitomo of Japan first used Silicalite-1 molecular sieve with high silicon / aluminum ratio with MFI topology as catalyst for the new fluidized bed process of cyclohexanone oxime gas-phase Beckmann rearrangement reaction for industrial production and achieved success, with the production capacity of the device reaching 55,000 tons / year of caprolactam production scale. However, Sumitomo of Japan has not disclosed the technology of preparing gas-phase rearrangement catalyst by spray molding.
[0006] Prior art also reports the technology of preparing gas phase rearrangement catalyst by spray forming, but there are some problems. For example, the catalyst wear index is high, the cyclohexanone oxime conversion rate and caprolactam selectivity are still not high enough, the catalyst life is short, the overall economic benefit is not obvious, and lacks the coordination with the overall process of cyclohexanone oxime gas phase Beckmann rearrangement, and the economy of industrial production needs to be further improved. For example, EP576295 discloses that molecular sieve is made into microspheres by spray drying without adding any binding agent, and then heat-treated in water, so that the microsphere catalyst can be used for cyclohexanone oxime conversion into caprolactam reaction. Although the catalyst has certain activity, its intensity cannot meet the needs of industrial application, the catalyst is easily deactivated, and the life is short, which can not meet the requirements of industrialization. Therefore, the spray forming process suitable for the catalyst of cyclohexanone oxime conversion into caprolactam industrial reaction still has a technical gap, and it is necessary to develop a new catalyst. Summary of the invention
[0007] The purpose of the present invention is to overcome the problems of high wear index, low cyclohexanone oxime conversion rate and caprolactam selectivity, and short catalyst life of the catalyst for the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime in the prior art, and to provide an apple-shaped microsphere molecular sieve catalyst and a preparation method and application thereof, and a method for the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime. The catalyst has the characteristics of lower wear index, higher cyclohexanone oxime conversion rate and caprolactam selectivity, and longer catalyst life.
[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides an apple-shaped microsphere molecular sieve catalyst, the catalyst comprising an all-silicon molecular sieve with an MFI topological structure and a binder, wherein the binder is silicon dioxide; according to scanning electron microscopy, the catalyst has an apple-shaped microsphere morphology, the microsphere surface has one and only one large hole, and the bulk density of the catalyst is not less than 0.64 g / cm 3 , the pore volume is not less than 0.3mL / g.
[0009] The second aspect of the present invention provides a method for preparing an apple-shaped microsphere molecular sieve catalyst, comprising the following steps:
[0010] (1) mixing and slurrying an all-silicon molecular sieve having an MFI topological structure, a binder and water to obtain a molecular sieve-binder slurry;
[0011] The viscosity of the molecular sieve-binder slurry is 30-100 mPa·s, and the particle size of the particles in the molecular sieve-binder slurry satisfies: D100≤30 μm, D90≤20 μm, D70≤10 μm;
[0012] (2) spray drying the molecular sieve-binder slurry and forming and calcining the slurry;
[0013] (3) The product obtained in step (2) is contacted with an alkaline buffer solution of a nitrogen-containing compound and then dried.
[0014] The third aspect of the present invention provides an apple-shaped microsphere molecular sieve catalyst prepared by the above preparation method.
[0015] The fourth aspect of the present invention provides the use of the apple-shaped microsphere molecular sieve catalyst described in the first aspect or the third aspect in the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime.
[0016] The fifth aspect of the present invention provides a method for the vapor-phase Beckmann rearrangement reaction of cyclohexanone oxime, the method comprising: under the vapor-phase Beckmann rearrangement reaction conditions of cyclohexanone oxime and in the presence of a solvent, contacting cyclohexanone oxime with a catalyst for reaction, wherein the catalyst is the apple-shaped microsphere molecular sieve catalyst described in the first aspect or the third aspect.
[0017] The microsphere molecular sieve catalyst provided by the present invention has an apple-shaped microsphere morphology according to scanning electron microscopy characterization, and the microsphere surface has one and only one large hole. The catalyst has a high packed density, has good fluidity when applied in a fluidized bed, is not easy to wear, has a long service life, and can meet the needs of industrial applications.
[0018] The preparation method provided by the present invention does not need to introduce additional pore-forming agents or other additives during the pulping process. By controlling the pulping conditions, the size distribution of particles in the molecular sieve-binder slurry obtained by pulping is controlled, the viscosity of the raw material slurry is improved, and a uniform, viscous molecular sieve-binder slurry is obtained. The slurry is directly used for spray drying and molding, and a microsphere molecular sieve catalyst with suitable particle size distribution, moderate bulk density, good sphericity, and an apple-shaped surface can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is a SEM image of the catalyst prepared in Example 1 at a magnification of 1000 times;
[0020] Figure 2 is a SEM image of the catalyst prepared in Example 1 at a magnification of 500 times;
[0021] Figure 3 is a SEM image of the catalyst prepared in Comparative Example 1 at a magnification of 200 times;
[0022] Figure 4 is a SEM image of the catalyst prepared in Comparative Example 2 at a magnification of 100 times;
[0023] Figure 5 This is a SEM image of the catalyst prepared in Comparative Example 3 at a magnification of 100 times. DETAILED DESCRIPTION
[0024] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0025] The first aspect of the present invention provides an apple-shaped microsphere molecular sieve catalyst, the catalyst comprising an all-silicon molecular sieve with an MFI topological structure and a binder, wherein the binder is silicon dioxide; according to scanning electron microscopy, the catalyst has an apple-shaped microsphere morphology, the microsphere surface has one and only one large hole, and the bulk density of the catalyst is not less than 0.64 g / cm 3 , the pore volume is not less than 0.3mL / g.
[0026] In the present invention, the “apple-shaped microsphere morphology, with one and only one large hole on the surface of the microsphere” means that the surface of the catalyst particle is smooth and spherical as a whole, with a high degree of sphericity, and the surface of the microsphere has a large hole formed by a surface depression, forming an apple-like morphology, such as Figure 1 There may also be small particles shaped like apple stems on the surface of the catalyst and / or in the macropores, and the composition of the small particles may be the same as or different from that of the catalyst.
[0027] The wear index of the catalyst is also closely related to the composition of the catalyst. In the present invention, the MFI topology molecular sieve is an all-silicon molecular sieve with extremely low metal content or substantially no metal elements. Compared with silicon-aluminum molecular sieves, all-silicon molecular sieves are hydrophobic molecular sieves. The crushing strength and abrasion resistance of molecular sieve catalysts produced by conventional extrusion molding or spray molding are not ideal, and it is more difficult to improve.
[0028] In the preparation technology of catalysts, the catalytic activity of catalysts is improved by forming limited partially hollow structures or introducing macropores to exert spatial confinement effects. However, for microsphere catalysts used in fluidized beds, the introduction of a large number of surface depressions may cause a decrease in catalyst strength, resulting in easy wear of the catalyst, which in turn increases the difficulty of industrial fluidized bed reaction production. In order to improve the strength of the catalyst, it is often necessary to introduce additional additives such as adhesives and thickeners into the catalyst to improve the physical properties of the catalyst.
[0029] In particular, in the fluidized bed process of the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, the catalyst has a high wear index and is easily worn into small particles, resulting in a short catalyst life and increased catalyst consumption, which causes fluctuations in the cyclohexanone oxime conversion rate and caprolactam selectivity.
[0030] The inventors of the present invention have found through a large number of experiments that by introducing large pores with surface depressions on the surface of the microspheres of the microsphere molecular sieve catalyst, while ensuring that the microspheres have appropriate pore depressions and packing density, the catalyst can have a low wear index, excellent catalytic performance and stability.
[0031] In the present invention, the morphology of the microsphere molecular sieve catalyst is observed using a field emission scanning electron microscope S-4800 produced by Hitachi Corporation of Japan.
[0032] In the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, the bulk density of the catalyst has a very important influence on the effect of the catalytic reaction due to the influence of the bulk density and particle size of the catalyst on the fluidized reaction state in the fluidized bed. According to the present invention, preferably, the bulk density of the catalyst is 0.65-0.8 g / cm 3 For example, it can be 0.65g / cm 3 , 0.68g / cm 3 , 0.7g / cm 3 , 0.72g / cm 3 , 0.75g / cm 3 、0.78g / cm 3 , 0.8g / cm 3 In the above preferred case, the catalyst has a good fluidized reaction state in the fluidized bed, and the catalyst is not easily worn into small particles, which is conducive to increasing the service life of the catalyst.
[0033] In the present invention, the bulk density of the catalyst is determined by passing the catalyst powder through a small funnel, allowing the powder to fall freely from the funnel into a 100mL measuring cylinder and weighing its mass. During this period, the measuring cylinder is continuously vibrated or tapped until the volume of the catalyst powder reaches the 100mL scale line and no longer changes. The bulk density of the catalyst is obtained by the ratio of the mass and volume of the catalyst at this time.
[0034] In fluidized bed technology, attrition index and particle size distribution are two important physical indicators of catalysts.
[0035] The particle characteristics of the catalyst affect the bulk density of the catalyst and are related to the particle size distribution of the catalyst. For coarse and heavy particles, that is, large particle size and high bulk density, a higher flow rate is usually required to achieve a more ideal fluidized state; conversely, light and fine particles, that is, small particle size and low bulk density, usually require a lower flow rate to achieve a more ideal fluidized state.
[0036] Fine particles have good flow properties like liquids, but coarse particles do not. Particles of a single size are not good enough either. Appropriate particle size distribution is required to improve flow properties and achieve ideal fluidization. When there are some fine particles, the fine particles are particularly easy to fluidize, and can flow to various parts of the bed and the gaps between large particles, and transfer their kinetic energy to the large particles, thereby promoting more uniform fluidization of the entire bed. Therefore, a certain amount of fine particles is essential in a fluidized bed reactor.
[0037] According to the present invention, preferably, the pore volume of the catalyst is 0.3-0.55 mL / g, preferably 0.4-0.5 mL / g.
[0038] According to the present invention, preferably, the specific surface area of the catalyst is 200-400m 2 / g, preferably 250-350m 2 In the present invention, the specific surface area of the catalyst is within the above preferred range, which is beneficial to the conversion rate of the catalyst and the selectivity of caprolactam.
[0039] In the present invention, the BET specific surface area and pore volume of the catalyst are expressed as N 2 The adsorption-desorption method was used to measure the NH4+ / -2H4O2. Specifically, the NH4+ / -2H4O2 was measured by an American Micromeritics ASAP-2460 automatic adsorption instrument. The test conditions were: N 2 As adsorbent, the adsorption temperature was -196.15℃ (liquid nitrogen temperature), and degassing was carried out at a constant temperature of 1.3Pa and 300℃ for 6h.
[0040] The present invention has a wide range of particle size selection for the catalyst. In a preferred embodiment, the D50 of the catalyst is 50-100 μm, preferably 60-90 μm, and more preferably 75-90 μm. Under the above preferred particle size distribution, it is beneficial to obtain a more ideal fluidized state, which is beneficial to the conversion rate of the catalyst and the selectivity of caprolactam.
[0041] In the present invention, the particle size and particle size distribution of the catalyst are measured using a 2000E laser particle size analyzer from Dandong Better Instrument Co., Ltd. The test method is a wet test, water is used as the medium, the sample mass concentration is 0.5%-2%, and the scanning speed is 2000 times / second.
[0042] In the present invention, the lower the wear index K, the higher the wear resistance of the catalyst, and the wear resistance of the catalyst is closely related to the composition and morphology of the catalyst. Preferably, the wear index K of the catalyst is less than 3% / h, preferably 1.5-2.5% / h, and more preferably 1.5-2% / h. In this preferred embodiment, the strength of the catalyst is higher, which is more conducive to improving the stability of the catalyst.
[0043] In the present invention, the wear index K is measured on a wear index analyzer according to the RIPP29-90 method in "Petrochemical Analysis Methods" (Yang Cuiding et al., Science Press, 1990).
[0044] The present invention has no particular limitation on the source of the all-silicon molecular sieve with the MFI topological structure, and the molecular sieve may be purchased from a commercial source or prepared by a method known in the prior art, for example, the molecular sieves disclosed in CN111847472A, CN109775714A, CN102233277A, CN102050464A, CN111847472A, and CN107337213A or prepared by the preparation methods disclosed therein may be used.
[0045] Preferably, the BET specific surface area of the molecular sieve is 400-500m 2 / g, preferably 420-450m 2 / g.
[0046] Preferably, the molecular sieve has a crystal particle size of 0.1-0.3 μm, preferably 0.1-0.25 μm.
[0047] Preferably, the external specific surface area of the molecular sieve is 30-60m 2 / g, preferably 35-60m 2 / g.
[0048] The present invention has a wide selection range for the content of molecular sieve and binder in the catalyst. Preferably, based on the dry weight of the catalyst, the content of the molecular sieve in the catalyst is 50-95% by weight, preferably 50-70% by weight, and the content of the binder in terms of oxide is 5-50% by weight, preferably 30-50% by weight.
[0049] The second aspect of the present invention provides a method for preparing an apple-shaped microsphere molecular sieve catalyst, comprising the following steps:
[0050] (1) mixing and slurrying an all-silicon molecular sieve having an MFI topological structure, a binder and water to obtain a molecular sieve-binder slurry;
[0051] The viscosity of the molecular sieve-binder slurry is 30-100 mPa·s, and the particle size of the particles in the molecular sieve-binder slurry satisfies: D100≤30 μm, D90≤20 μm, D70≤10 μm;
[0052] (2) spray drying the molecular sieve-binder slurry and forming and calcining the slurry;
[0053] (3) The product obtained in step (2) is contacted with an alkaline buffer solution of a nitrogen-containing compound and then dried.
[0054] In the prior art, in order to form a hollow or surface-depressed spherical catalyst, it is usually necessary to introduce pore-forming agents, surfactants and other additives into the slurry used for spray molding, and form hole depressions by decomposition of the additives. The preparation method provided by the present invention only controls the size distribution of particles in the molecular sieve-binder slurry obtained by beating by controlling the beating conditions, and obtains a uniform, viscous molecular sieve-binder slurry, which is directly used for spray drying molding, and can obtain apple-shaped microsphere molecular sieve catalysts with suitable particle size distribution, moderate bulk density, good sphericity and surface depressions. No additional thickener, defoamer or other additives are required during the beating process, and the physical and chemical properties of the catalyst such as roundness and smoothness can be improved.
[0055] The inventors of the present invention have found in their research that the viscosity of the molecular sieve-binder slurry has an important influence on the morphology and structure of the catalyst obtained by spray molding. In conventional spray molding, a pulping machine is generally used to pulp the raw materials, so the viscosity of the molecular sieve-binder slurry obtained by pulping is often low, and the particle size distribution of the particles in the slurry is not considered; however, the viscosity of the molecular sieve-binder slurry controlled in the present invention is much higher than the conventional level of the prior art. Preferably, a ball mill is used to pulp the raw materials to form a viscous molecular sieve-binder slurry, and at the same time, the particles in the slurry form a suitable particle size distribution, thereby forming a microsphere catalyst with a specific concave morphology through spray molding.
[0056] It should be noted that the viscosity and particle size distribution of the molecular sieve-binder slurry are controlled by operating conditions such as beating time and stirring rate in the present invention. The present invention has no particular limitation on the specific operating conditions, as long as the molecular sieve-binder slurry obtained after beating meets the above requirements. Those skilled in the art can make a selection based on actual experimental and equipment conditions, for example, a ball mill can be used for the beating. Preferably, when a ball mill is used for the beating, the beating time is not less than 1 hour, preferably 1-5 hours.
[0057] According to a preferred embodiment of the present invention, the viscosity of the molecular sieve-binder slurry is 50-80 mPa·s, for example, it can be 50 mPa·s, 55 mPa·s, 60 mPa·s, 65 mPa·s, 70 mPa·s, 75 mPa·s, 80 mPa·s, etc. Typical but non-limiting viscosity values or ranges therebetween. In the above preferred case, it is conducive to obtaining ideal catalyst physical and chemical performance indicators. Too low viscosity of the slurry may lead to a high catalyst wear index, and too high viscosity is not conducive to spray molding, and the nozzle is easily blocked.
[0058] In the present invention, the viscosity of the molecular sieve-binder slurry is measured by a capillary method using a viscometer, specifically comprising: using a liquid (water) with a known kinematic viscosity as a standard (viscosity is p 0 , mPa·s), and measure the time t for it to flow out of the capillary viscometer 1 , and then measure the time t for the mixed slurry to flow out of the same viscometer 2 , the viscosity of the mixed slurry p (mPa·s) = t 2 / t 1 ×p 0 .
[0059] In a further preferred embodiment, the particle size of the particles in the molecular sieve-binder slurry satisfies: D100 is ≤20 μm, D90 is ≤10 μm, and D70 is ≤5 μm. In this preferred case, it is beneficial to obtain a microsphere particle catalyst with an ideal particle size distribution, high roundness, good smoothness, and low wear index.
[0060] The present invention has a wide selection range for the solid content of the molecular sieve-binder slurry. Preferably, the solid content of the molecular sieve-binder slurry is 10-60% by weight, preferably 30-60% by weight. In this preferred case, it is more conducive to spray molding, so that the catalyst wear index is lower.
[0061] According to the method provided by the present invention, preferably, the binder is a precursor of silicon dioxide. In the present invention, the precursor of silicon dioxide refers to a substance that can be converted into silicon dioxide by subsequent calcination, and those skilled in the art can select it according to actual needs. Preferably, the precursor of silicon dioxide is silica sol and / or white carbon black, and more preferably silica sol. The above preferred binder is conducive to further optimizing the pulping effect.
[0062] According to the present invention, preferably, the molecular sieve calculated on a dry basis and the SiO 2 The weight ratio of the binder to the catalyst is 1:(0.05-1), preferably 1:(0.4-0.9), and more preferably 1:(0.5-0.8). In this preferred case, the catalyst has better performance and is more conducive to improving the conversion rate of cyclohexanone oxime and the selectivity of caprolactam.
[0063] In the present invention, the selection of the all-silicon molecular sieve with the MFI topological structure in step (1) is the same as the composition in the above text, which will not be repeated here. The prepared all-silicon molecular sieve with the MFI topological structure can be used in step (1), and the slurry containing the molecular sieve obtained in the molecular sieve preparation process (i.e., the uncalcined molecular sieve) can also be used in step (1) to provide the all-silicon molecular sieve with the MFI topological structure, and the present invention has no special limitation on this.
[0064] According to a preferred embodiment of the present invention, the spray drying method is centrifugal spray drying, and the rotation speed of the atomizing wheel in the centrifugal spray drying is 15-45 Hz, for example, it can be 15 Hz, 20 Hz, 25 Hz, 30 Hz, 35 Hz, 40 Hz, 45 Hz and other typical but non-limiting rotation speeds, preferably 20-30 Hz. By adjusting the rotation speed of the atomizing wheel in the centrifugal spray drying, a catalyst with an ideal catalyst compact density and wear index can be obtained.
[0065] According to the present invention, preferably, the inlet temperature of the spray drying is 180-350° C., preferably 200-260° C., and the outlet temperature is 80-150° C., preferably 100-130° C. In this preferred embodiment, the performance of the catalyst is better, which is more conducive to improving the conversion rate of cyclohexanone oxime and the selectivity of caprolactam.
[0066] According to the present invention, preferably, the temperature of the molding and calcining in step (2) is 450-650°C, preferably 500-600°C, and the time is 1-20h, preferably 6-18h.
[0067] In a further preferred embodiment, the molding calcination method is a step-by-step temperature increase calcination, that is, the temperature is increased stepwise from room temperature to the above molding calcination temperature, the step temperature gradient is preferably 50-300°C, and the step insulation time is preferably 1-3h. The above preferred molding calcination method is beneficial to improving the roundness and smoothness of the catalyst.
[0068] According to a specific embodiment of the present invention, in step (3), the alkaline buffer solution of the nitrogen-containing compound contains an ammonium salt and a base.
[0069] The present invention has a wide range of solvents for the alkaline buffer solution of the nitrogen-containing compound, and water is preferred.
[0070] In the present invention, the ammonium salt is preferably ammonium nitrate and / or ammonium acetate. The base is selected from at least one of aqueous ammonia, tetramethylammonium hydroxide, tetraethylammonium hydroxide and tetrapropylammonium hydroxide, preferably aqueous ammonia.
[0071] According to a preferred embodiment of the present invention, the content of the ammonium salt is 0.1-20% by weight, preferably 0.5-15% by weight; the content of the alkali is 5-30% by weight, preferably 10-28% by weight.
[0072] Preferably, the pH value of the alkaline buffer solution of the nitrogen-containing compound is 8.5-13.5, preferably 10-12, and more preferably 11-11.5.
[0073] The present invention has a wide range of selection for the amount of the nitrogen-containing compound alkaline buffer solution. Preferably, the amount of the nitrogen-containing compound alkaline buffer solution is 500-1500 parts by weight, preferably 700-1200 parts by weight, relative to 100 parts by weight of the product obtained in step (2) on a dry basis.
[0074] Preferably, the contact conditions include: a temperature of 50-120°C, preferably 70-100°C; a pressure of 0.5-10 kg / cm 2 , preferably 1.5-4kg / cm 2; The time is 0.1-5h, preferably 1-3h. In the present invention, the contact is preferably carried out under stirring conditions. The present invention has no particular limitation on the stirring speed, and those skilled in the art can make an appropriate selection according to actual conditions.
[0075] According to the method provided by the present invention, the contact process can be repeated. The present invention does not specifically limit the number of repetitions, which can be determined according to the effect of the contact, in order to improve the performance of the catalyst, for example, it can be repeated 1-3 times, preferably 2-3 times.
[0076] In the present invention, the conditions for drying the product obtained by contacting the calcined product with the alkaline buffer solution of the nitrogen-containing compound are not particularly limited, and can be carried out according to any existing technical means in the art, as long as the solvent is removed. The drying method includes but is not limited to natural drying, heating drying, and forced air drying. Specifically, for example, the drying temperature can be 100-120° C., and the drying time can be 2-36 hours.
[0077] According to the present invention, preferably, before the drying in step (3), the process further comprises: filtering and washing the product obtained in step (2) after contacting the product with an alkaline buffer solution of a nitrogen-containing compound. The present invention has no particular limitation on the washing agent used in the washing process, and the washing agent may be water, for example. Specifically, the washing process may include washing until the pH of the filtrate is 9-10.5.
[0078] The third aspect of the present invention provides an apple-shaped microsphere molecular sieve catalyst prepared by the above-mentioned preparation method.
[0079] The catalyst comprises an all-silicon molecular sieve with an MFI topological structure and a binder. According to scanning electron microscopy, the catalyst has an apple-shaped microsphere morphology, and the microsphere surface has one and only one large hole. The bulk density of the catalyst is not less than 0.65 g / cm 3 , pore volume is not less than 0.3mL / g, and wear index K is less than 3% / h.
[0080] The fourth aspect of the present invention provides use of the apple-shaped microsphere molecular sieve catalyst described in the first aspect or the third aspect in a gas-phase Beckmann rearrangement reaction of cyclohexanone oxime.
[0081] The fifth aspect of the present invention provides a method for the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, the method comprising: under the conditions of the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, in the presence of a solvent, contacting cyclohexanone oxime with a catalyst for reaction, wherein the catalyst is the apple-shaped microsphere molecular sieve catalyst described in the first aspect or the third aspect. The solvent is preferably methanol and / or ethanol,
[0082] Preferably, the cyclohexanone oxime gas-phase Beckmann rearrangement reaction is carried out in a fluidized bed reactor.
[0083] According to the present invention, preferably, the cyclohexanone oxime gas phase Beckmann rearrangement reaction is carried out under an inert atmosphere. In the present invention, the inert atmosphere is provided by an inert gas, preferably the inert gas is selected from at least one of nitrogen, helium, argon and neon, more preferably nitrogen.
[0084] According to the present invention, preferably, the molar ratio of the inert gas to cyclohexanone oxime is 0-10: 1, preferably 0.1-5: 1, and more preferably 0.2-3: 1. In this preferred case, it is more conducive to reducing energy consumption, thereby improving the economy of the overall process of the cyclohexanone oxime gas-phase Beckmann rearrangement reaction.
[0085] According to a preferred embodiment of the present invention, the cyclohexanone oxime gas-phase Beckmann rearrangement reaction conditions include: a reaction temperature of 300-500°C, preferably 350-400°C; a reaction pressure of 0.05-0.8MPa, preferably 0.1-0.5MPa, in terms of gauge pressure; a cyclohexanone oxime weight space velocity of 0.1-20h -1 , preferably 3-8h -1 , more preferably 3-6h -1 .
[0086] According to the present invention, preferably, cyclohexanone oxime accounts for 20-50 wt % of the total amount of cyclohexanone oxime and solvent.
[0087] According to the present invention, preferably, the method further comprises mixing cyclohexanone oxime with water (preferably in a molar ratio of 1:0.01-2.5), and then contacting the catalyst in the presence of the solvent to perform a gas-phase Beckmann rearrangement reaction. This preferred embodiment is more conducive to improving the stability of the catalyst and the selectivity of caprolactam.
[0088] According to the present invention, preferably, the method further comprises, in the solution of cyclohexanone oxime and methanol or ethanol, adding water (preferably the amount of water added is 0.1-1% by weight of the weight of the solution of cyclohexanone oxime and methanol or ethanol) and mixing, and then contacting with the catalyst to carry out gas-phase Beckmann rearrangement reaction. This preferred embodiment is more conducive to improving the stability of the catalyst and the selectivity of caprolactam.
[0089] Preferably, the method further comprises: regenerating the catalyst after the reaction under air conditions. The regeneration can be carried out under conventional catalyst regeneration conditions in the art.
[0090] The present invention will be described in detail below through examples.
[0091] In the following examples, unless otherwise specified, pressure is gauge pressure; normal pressure means one atmosphere; normal temperature means 25°C;
[0092] The external specific surface area and BET specific surface area were measured by the American Micromeritics ASAP-2460 automatic adsorption instrument. The test conditions were: N 2 As adsorbate, the adsorption temperature was -196.15℃ (liquid nitrogen temperature), and the degassing was carried out at a constant temperature of 1.3Pa and 300℃ for 6h;
[0093] The morphology of the catalyst was analyzed using a field emission scanning electron microscope S-4800 produced by Hitachi, Japan;
[0094] The wear index K of the catalyst was measured on a wear index analyzer according to the RIPP29-90 method in "Petrochemical Analysis Methods" (Yang Cuiding et al., Science Press, 1990);
[0095] The particle size and particle size distribution of the catalyst were measured using a 3000plus laser particle size analyzer from Dandong Better Instrument Co., Ltd. The test method was a wet test, with water as the medium, a sample mass concentration of 0.5%-2%, and a scanning speed of 2000 times / second;
[0096] In the following examples, the spray forming is carried out in a spray forming device, which is produced by Wuxi Tianyang Spray Drying Equipment Co., Ltd. and has a model number of LT-300.
[0097] Example 1
[0098] According to the method disclosed in Example 1 of CN102050464A, an all-silicon molecular sieve with an MFI topological structure was prepared. The BET specific surface area of the molecular sieve was 439 m 2 / g, the grain size is 0.1-0.2μm, and the external specific surface area is 60m 2 / g.
[0099] The molecular sieve slurry that was partially crystallized but not dried and calcined was mixed with alkaline silica sol (pH 9.5, sodium ion content 324 ppm, SiO 2 The content is 40% by weight, and the SiO 2 The surface area is 225m 2 / g) mixed, wherein the molecular sieve calculated on a dry basis is mixed with SiO 2The weight ratio of the alkaline silica sol is 60:40, and an appropriate amount of water is added to adjust the solid content to 50%; the mixture is stirred evenly, and slurry is made for 4 hours using a German NETZSCH LME1 ball mill (with a diameter of 1 mm zirconium oxide balls as the medium, and a mass ratio of the balls to the slurry of 1:3); the viscosity of the molecular sieve-binder slurry is 63 mPa·s, and the particle size distribution of the particles in the molecular sieve-binder slurry is measured to be: D100 is 18.5 μm, D90 is 9.3 μm, and D70 is 4.6 μm.
[0100] The molecular sieve-binder slurry was sent to a centrifugal spray forming device for spray forming. The inlet and outlet temperatures were 240°C and 125°C respectively. The speed of the atomizing wheel in the centrifugal spray drying was 26 Hz. Then, the 3M 3 The mixture was heated in a shuttle furnace (manufactured by Hubei Huanggang Huaxia Mechanical and Electrical Thermal Equipment Co., Ltd., the same below), and calcined at 280°C, 400°C, and 480°C for 2 h, and finally calcined at 580°C for 12 h to obtain a microsphere molecular sieve, wherein the content of the MFI topological structure silicon molecular sieve was 60.2% by weight, and the content of SiO 2 The calculated binder content is 39.8% by weight.
[0101] 100 g of the microsphere molecular sieve and 1000 g of an alkaline buffer solution of a nitrogen-containing compound (the alkaline buffer solution of the nitrogen-containing compound is a mixture of ammonia water and an ammonium nitrate aqueous solution, with a pH value of 11.35, wherein the content of ammonia water is 26% by weight, the content of ammonium nitrate in the ammonium nitrate aqueous solution is 7.5% by weight, and the weight ratio of ammonia water to ammonium nitrate aqueous solution is 3:2) are added into a 2000 mL stainless steel reactor (KCF-2 magnetic stirring autoclave, Yantai High-tech Zone Keli Automatic Control Equipment Research Institute, the same below) and heated at 86°C, 2.7 kg / cm 2 Stirring at a constant temperature for 2 hours under pressure, then filtering and drying at 90°C for 12 hours, repeating the same treatment once, then filtering and washing until the pH of the filtered clear liquid is about 9, and then drying at 120°C for 24 hours to obtain catalyst S1. A photo of catalyst S1 is shown in FIG. Figure 1 and Figure 2 As shown in the figure, it can be seen that the catalyst has good particle size sphericity, the catalyst has an apple-shaped microsphere morphology, and there is only one large hole on the surface of the microsphere. The characterization results of catalyst S1 are shown in Table 1.
[0102] Example 2
[0103] The molecular sieve slurry in Example 1 was mixed with an alkaline silica sol (pH 9.5, sodium ion content 324 ppm, SiO 2 The content is 40% by weight, and the SiO 2 The surface area is 225m2 / g) mixed, wherein the molecular sieve calculated on a dry basis is mixed with SiO 2 The weight ratio of the alkaline silica sol is 50:50, and an appropriate amount of water is added to obtain a molecular sieve-binder slurry with a solid content of 54.4% by weight. The mixture is stirred evenly and slurried for 5 hours using a German NETZSCH LME1 ball mill (with a diameter of 1 mm zirconium oxide balls as the medium, and a mass ratio of the balls to the slurry of 1:2). The viscosity of the obtained molecular sieve-binder slurry is 68 mPa·s, and the particle size distribution of the particles in the molecular sieve-binder slurry is measured to be: D100 is 17.3 μm, D90 is 8.8 μm, and D70 is 4.3 μm.
[0104] The molecular sieve-binder slurry after beating is sent to a centrifugal spray forming device for spray forming. The inlet and outlet temperatures are 230°C and 105°C respectively. The speed of the atomizing wheel in the centrifugal spray drying is 27Hz. Then, the 3M 3 The catalyst was heated in a shuttle furnace and calcined at 280°C, 400°C, and 480°C for 2 h, and finally calcined at 550°C for 12 h to obtain a microsphere molecular sieve catalyst, wherein the content of the MFI topological structure silicon molecular sieve was 50.6% by weight, and the content of SiO 2 The calculated binder content is 49.4% by weight.
[0105] 100 g of the microsphere molecular sieve and 1000 g of an alkaline buffer solution of a nitrogen-containing compound (the alkaline buffer solution of a nitrogen-containing compound is a mixture of ammonia water and an ammonium nitrate aqueous solution, with a pH value of 11.35, wherein the content of ammonia water is 26% by weight, the content of ammonium nitrate in the ammonium nitrate aqueous solution is 7.5% by weight, and the weight ratio of ammonia water to ammonium nitrate aqueous solution is 3:2) are added into a 2000 mL stainless steel reactor and heated at 86°C and 2.7 kg / cm 2 The catalyst was stirred at a constant temperature for 2 hours under pressure, then filtered and dried at 90°C for 12 hours. The same treatment was repeated once, and then filtered and washed until the pH of the filtered clear liquid was about 9, and then dried at 120°C for 24 hours to obtain catalyst S2. The morphology of S2 was similar to that of Figure 1 The catalyst S2 has an apple-like microsphere morphology and has only one large hole on its surface.
[0106] Example 3
[0107] The molecular sieve slurry in Example 1 was mixed with an alkaline silica sol (pH 9.5, sodium ion content 324 ppm, SiO 2 The content is 40% by weight, and the SiO 2 The surface area is 225m 2 / g) mixed, wherein the molecular sieve calculated on a dry basis is mixed with SiO2 The weight ratio of the alkaline silica sol is 70:30, and an appropriate amount of water is added to adjust the solid content to 52%. The mixture is stirred evenly, and slurry is made for 4 hours using a German NETZSCH LME1 ball mill (with a diameter of 1 mm zirconium oxide balls as the medium, and a mass ratio of the balls to the slurry of 1:5). The viscosity of the obtained molecular sieve-binder slurry is 55 mPa·s, and the particle size distribution of the particles in the molecular sieve-binder slurry is measured to be: D100 is 19.4 μm, D90 is 9.2 μm, and D70 is 4.8 μm.
[0108] Then it is sent to a centrifugal spray forming device for spray forming, with the inlet and outlet temperatures being 230°C and 105°C respectively, and the speed of the atomizing wheel in the centrifugal spray drying is 25Hz. Then it is sent to a 3M 3 The catalyst was heated in a shuttle furnace (manufactured by Hubei Huanggang Huaxia Mechanical and Electrical Thermal Equipment Co., Ltd., the same below), and calcined at 280°C, 400°C, and 480°C for 2 h, and finally calcined at 560°C for 12 h to obtain a microsphere molecular sieve catalyst, wherein the content of MFI topological structure silicon molecular sieve was 69.6% by weight, and SiO 2 The calculated binder content is 30.4% by weight.
[0109] 100 g of the microsphere molecular sieve and 1000 g of an alkaline buffer solution of a nitrogen-containing compound (the alkaline buffer solution of a nitrogen-containing compound is a mixture of ammonia water and an ammonium nitrate aqueous solution, with a pH value of 11.35, wherein the content of ammonia water is 26% by weight, the content of ammonium nitrate in the ammonium nitrate aqueous solution is 7.5% by weight, and the weight ratio of ammonia water to ammonium nitrate aqueous solution is 3:2) are added into a 2000 mL stainless steel reactor and heated at 86°C and 2.7 kg / cm 2 Stirring at a constant temperature for 2 hours under pressure, then filtering and drying at 90°C for 12 hours, repeating the same treatment once, then filtering and washing until the pH of the filtered clear liquid is about 9, and then drying at 120°C for 24 hours to obtain catalyst S3, which has an apple-shaped microsphere morphology, and there is only one large hole on the surface of the microsphere. The characterization results of catalyst S3 are shown in Table 1.
[0110] Example 4
[0111] The method of Example 1 is followed, except that the molecular sieve on a dry basis is different from the SiO 2The weight ratio of alkaline silica sol is 80:20, and an appropriate amount of water is added to adjust the solid content to 53%. Stir evenly, and use a German NETZSCH LME1 ball mill (1mm diameter zirconium oxide balls as medium, the mass ratio of balls to slurry is 1:5) for 4 hours. The viscosity of the molecular sieve-binder slurry is 51mPa·s, and the particle size of the particles in the molecular sieve-binder slurry meets: D100 is 23μm, D90 is 11.2μm, and D70 is 5.6μm. Spray molding is carried out in the same way as in Example 1 to obtain a microsphere molecular sieve catalyst, wherein the content of MFI topological structure silicon molecular sieve is 79.8% by weight, and SiO 2 The calculated binder content is 20.2% by weight.
[0112] The obtained catalyst is recorded as S4. The characterization results of catalyst S4 are shown in Table 1.
[0113] Example 5
[0114] The method of Example 1 was followed, except that the rotation speed of the atomizing wheel in the centrifugal spray drying was 18 Hz. The obtained catalyst was recorded as S5. The characterization results of catalyst S5 are shown in Table 1.
[0115] Comparative Example 1
[0116] The method of Example 1 is followed, except that the beating time is 1 hour, and the viscosity of the molecular sieve-binder slurry obtained after beating is 33 mPa·s. After testing, the particle size of the particles in the molecular sieve-binder slurry meets the following requirements: D100 is 35 μm, D90 is 23 μm, and D70 is 12 μm.
[0117] The obtained catalyst was recorded as DS1. The morphology of the obtained catalyst was characterized by scanning electron microscopy. Figure 3 As shown, it can be seen that the sphericity of DS1 is poor. The physical and chemical properties test results of catalyst DS1 are shown in Table 1.
[0118] Comparative Example 2
[0119] The molecular sieve slurry prepared in Example 1 was mixed with alkaline silica sol (pH value was 9.5, sodium ion content was 324 ppm, SiO 2 The content is 40% by weight, and the SiO 2 The surface area is 225m 2 / g), activated carbon and water, wherein the molecular sieve calculated on a dry basis and the SiO 2The weight ratio of alkaline silica sol and activated carbon is 54:36:10; the beating time is 1 hour, and the viscosity of the molecular sieve-binder slurry obtained after beating is 38 mPa·s. The particle size distribution of the particles in the molecular sieve-binder slurry is tested as follows: D100 is 38 μm, D90 is 26 μm, and D70 is 14 μm.
[0120] The molecular sieve-binder slurry was spray-formed according to the method of Example 1. The obtained catalyst was recorded as DS2. The morphology of the obtained catalyst was characterized by scanning electron microscopy. Figure 4 The physicochemical performance test results of catalyst DS2 are shown in Table 1.
[0121] Comparative Example 3
[0122] The method of Example 1 is followed, except that the beating time is 0.5 hours, the viscosity of the molecular sieve-binder slurry obtained by beating is 28 mPa·s, and the particle size of the particles in the molecular sieve-binder slurry is measured to meet the following requirements: D100 is 34 μm, D90 is 22 μm, and D70 is 11 μm.
[0123] The obtained catalyst is recorded as DS3. The morphology of the obtained catalyst is characterized by scanning electron microscopy. Figure 5 As shown, it can be seen that there are a large number of unqualified broken microspheres in the catalyst.
[0124] The characterization results of catalyst DS3 are shown in Table 1.
[0125] Table 1
[0126]
[0127]
[0128] Test Case
[0129] This test example is used to evaluate the catalytic reaction effect of the catalysts prepared in the examples and comparative examples in the gas-phase Beckmann rearrangement reaction:
[0130] Quick evaluation: The vapor-phase Beckmann rearrangement reaction of cyclohexanone oxime was carried out in a fixed bed reactor with an inner diameter of 5 mm, containing 0.375 g of 40-60 mesh catalyst in terms of molecular sieve, about 30 mm high 30 mesh coarse quartz sand on the catalyst bed, and 50 mesh fine quartz sand below the catalyst bed. The rearrangement reaction conditions include: normal pressure; reaction temperature of 380°C; cyclohexanone oxime weight space velocity (WHSV, cyclohexanone oxime flow in feed / catalyst weight in terms of molecular sieve in bed) of 16 h -1 ; The reaction solvent is ethanol, the weight of which is 65% of the weight of the reaction raw materials; the carrier gas (N 2) flow rate was 45 mL / min, and the reaction product was cooled by ice-water mixture and then entered into a collection bottle for gas-liquid separation. After 6 hours of reaction, the product composition was analyzed. The rapid evaluation results are shown in Table 2.
[0131] The catalyst prepared in Example 1 was subjected to reaction evaluation in a fixed fluidized bed: The reaction performance of the microsphere molecular sieve catalyst was evaluated using a fixed fluidized bed, and the catalyst was regenerated after 10 hours of reaction, and the above reaction and regeneration process were repeated. The reaction results of the 10th repetition are shown in Table 3. The reaction conditions include: a temperature range of 380-390°C; a catalyst loading of 260 grams; cyclohexanone oxime accounting for 35% by weight of the total amount of cyclohexanone oxime and ethanol, wherein the water content is 0.8% by weight; a molar ratio of nitrogen to cyclohexanone oxime of 2:1; a reaction pressure of 0.05-0.1 MPa; and a cyclohexanone oxime weight space velocity of 4.2 h -1 The regeneration conditions include: regeneration temperature 500°C, regeneration air volume: 3L / min, and regeneration time 20h.
[0132] The reaction products were quantitatively analyzed using an Agilent 6890 gas chromatograph (hydrogen flame ionization detector, PEG20M capillary column, column length 50 m). The vaporization chamber temperature was 250°C, the detection chamber temperature was 240°C, and the column temperature was programmed from 110°C for 8 minutes, then increased to 230°C at 15°C / min and maintained at that temperature for 14 minutes.
[0133] The contents of rearrangement products of caprolactam and cyclohexanone oxime after the reaction were calculated using the area normalization method, and the solvent was not involved in the integration.
[0134] The molar percentage of cyclohexanone oxime in the reaction product and the molar percentage of caprolactam in the reaction product are obtained through the above analysis, and the cyclohexanone oxime conversion rate and caprolactam selectivity are calculated by the following formula:
[0135] Cyclohexanone oxime conversion rate (mol%) = (cyclohexanone oxime molar content in feed - cyclohexanone oxime molar content in product) / cyclohexanone oxime molar content in feed × 100%;
[0136] Total caprolactam selectivity (mol%) = mole percentage of caprolactam in the product / (100-mole percentage of cyclohexanone oxime in the product) × 100%;
[0137] Among the by-products of the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, ethyl-ε-caprolactam (AEH) accounts for about 40% of the total amount of all by-products. This by-product is generated by the alcoholysis reaction between ethanol and the tautomer of the enol structure of caprolactam. Under the action of water, ethyl-ε-caprolactam continues to generate caprolactam through hydrolysis reaction. Therefore, the amount of caprolactam generated by the hydrolysis of ethyl-ε-caprolactam is included in the calculation of the total selectivity of caprolactam.
[0138] Table 2 Rapid evaluation results
[0139]
[0140] In the above table, CPL stands for caprolactam; AEH stands for ethyl-ε-caprolactimide.
[0141] Table 3 Results of the 10th fixed fluidized bed evaluation
[0142] Time / h 1 2 3 5 6 7 8 9 10 Conversion rate 99.97 99.94 99.91 99.82 99.74 99.67 99.59 99.54 99.57 Selectivity 96.53 96.47 96.58 96.63 96.55 96.49 96.56 96.52 96.48 Condensation 0.924 0.982 0.958 0.908 0.957 0.975 0.981 0.991 1.00 Capronitrile 0.109 0.115 0.114 0.115 0.116 0.117 0.116 0.118 0.127 Cyclohexanone 0.249 0.292 0.280 0.255 0.275 0.282 0.263 0.269 0.307 5-Hexenenitrile 0.669 0.650 0.640 0.641 0.638 0.642 0.633 0.629 0.621 Cyclopentane 0.144 0.175 0.196 0.224 0.238 0.252 0.261 0.281 0.301 Cyclohexenone 0.344 0.287 0.247 0.206 0.197 0.188 0.176 0.161 0.147 RT 15.023 0.110 0.127 0.122 0.132 0.123 0.136 0.129 0.130 0.132 aniline 0.058 0.053 0.052 0.048 0.047 0.045 0.043 0.043 0.043 RT 30.705 0.015 0.026 0.035 0.045 0.051 0.056 0.062 0.064 0.073 Valerolactam 0.057 0.057 0.057 0.058 0.062 0.064 0.065 0.064 0.068 RT 34.788 0 0.037 0.042 0.053 0.049 0.050 0.047 0.048 0.048 Octahydrophenazine 0.042 0.02 0.023 0.029 0.029 0.031 0.031 0.032 0.029
[0143] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. An apple-shaped microsphere molecular sieve catalyst, characterized in that: The catalyst comprises an all-silicon molecular sieve having an MFI topological structure and a binder, wherein the binder is silicon dioxide; According to the scanning electron microscope, the catalyst has an apple-shaped microsphere morphology, and there is only one large hole on the surface of the microsphere. The bulk density of the catalyst is not less than 0.64 g / cm 3 , the pore volume is not less than 0.3mL / g.
2. The catalyst according to claim 1, wherein The bulk density of the catalyst is 0.65-0.8 g / cm 3 ; Preferably, the pore volume of the catalyst is 0.3-0.55 mL / g, preferably 0.4-0.5 mL / g; Preferably, the specific surface area of the catalyst is 200-400m 2 / g, preferably 250-350m 2 / g.
3. The catalyst according to claim 1 or 2, wherein The D50 of the catalyst is 50-100 μm, preferably 60-90 μm; Preferably, the attrition index K of the catalyst is less than 3% / h, preferably 1.5-2.5% / h, and more preferably 1.5-2% / h.
4. The catalyst according to any one of claims 1 to 3, wherein Based on the dry weight of the catalyst, the content of the molecular sieve in the catalyst is 50-95% by weight, preferably 50-70% by weight, and the content of the binder in terms of oxide is 5-50% by weight, preferably 30-50% by weight.
5. A method for preparing an apple-shaped microsphere molecular sieve catalyst, characterized in that: The following steps are involved: (1) mixing and slurrying an all-silicon molecular sieve having an MFI topological structure, a binder and water to obtain a molecular sieve-binder slurry; The viscosity of the molecular sieve-binder slurry is 30-100 mPa·s, and the particle size of the particles in the molecular sieve-binder slurry satisfies: D100≤30 μm, D90≤20 μm, D70≤10 μm; (2) spray drying the molecular sieve-binder slurry and forming and calcining the slurry; (3) The product obtained in step (2) is contacted with an alkaline buffer solution of a nitrogen-containing compound and then dried.
6. The preparation method according to claim 5, wherein: The viscosity of the molecular sieve-binder slurry is 50-80 mPa·s; And / or, the particle size of the particles in the molecular sieve-binder slurry satisfies: D100≤20μm, D90≤10μm, D70≤5μm; and / or, the molecular sieve-binder slurry has a solid content of 10-60 wt %, preferably 30-60 wt %; Preferably, the binder is silica sol and / or white carbon black, preferably silica sol; Preferably, the weight ratio of the molecular sieve calculated on a dry basis to the binder calculated on a SiO2 basis is 1:(0.05-1), preferably 1:(0.4-0.9), more preferably 1:(0.5-0.8).
7. The preparation method according to claim 5 or 6, wherein: The spray drying method is centrifugal spray drying, and the rotation speed of the atomizing wheel in the centrifugal spray drying is 15-45 Hz, preferably 20-30 Hz; Preferably, the inlet temperature of the spray drying is 180-350°C, preferably 200-260°C; the outlet temperature is 80-150°C, preferably 100-130°C.
8. The preparation method according to any one of claims 5 to 7, wherein: The molding and calcining in step (2) is carried out at a temperature of 450-650°C, preferably 500-600°C, and for a time of 1-20h, preferably 6-18h.
9. The preparation method according to any one of claims 5 to 8, wherein: In step (3), the alkaline buffer solution of the nitrogen-containing compound contains an ammonium salt and a base, the content of the ammonium salt is 0.1-20% by weight, the content of the base is 5-30% by weight, and the pH value of the alkaline buffer solution of the nitrogen-containing compound is 8.5-13.5; Preferably, the amount of the nitrogen-containing compound alkaline buffer solution is 500-1500 parts by weight, preferably 700-1200 parts by weight, relative to 100 parts by weight of the product obtained in step (2) on a dry basis; Preferably, the contact conditions include: a temperature of 50-120°C, preferably 70-100°C; a pressure of 0.5-10 kg / cm 2 , preferably 1.5-4kg / cm 2 ; The time is 0.1-5h, preferably 1-3h; Preferably, the number of contacts is 1-5 times, preferably 2-3 times.
10. The apple-shaped microsphere molecular sieve catalyst obtained by the preparation method according to any one of claims 5 to 9.
11. Use of the apple-shaped microsphere molecular sieve catalyst according to any one of claims 1 to 4 and 10 in the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime.
12. A method for the gas-phase Beckmann rearrangement reaction of cyclohexanone oxime, the method comprising: Under the conditions of cyclohexanone oxime gas-phase Beckmann rearrangement reaction, in the presence of a solvent, cyclohexanone oxime is contacted with a catalyst for reaction, wherein the catalyst is the apple-shaped microsphere molecular sieve catalyst according to any one of claims 1 to 4 and 10; the solvent is preferably methanol and / or ethanol; Preferably, the cyclohexanone oxime gas-phase Beckmann rearrangement reaction is carried out in a fluidized bed reactor.
Citation Information
Cited By
Production method of caprolactam
CN119552118A
Cyclohexanone-oxime gas phase Beckmann rearrangement reaction method and application thereof
CN119552119A
Method for preparing caprolactam
CN120025267A
Method for preparing caprolactam
CN120025268A
Cyclohexanone-oxime gas phase Beckmann rearrangement reaction method and reaction system
CN120365214A