Low-hydroxyl low-inclusion quartz sand as well as preparation method and application thereof
Through the hydrolysis, gelation and sonication of quartz sand, low hydroxyl group and low inclusion quartz sand are prepared, which solves the problem of high hydroxyl and inclusion content in the prior art, and improves the strength of the quartz crucible and Service life and reduce production energy consumption.
Patent Information
- Application Number
- CN202411534398.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-31
- Publication Date
- 2024-11-29
AI Technical Summary
In the existing quartz sand preparation methods, there are more hydroxyl content and inclusions, which leads to a reduction in the strength of the quartz crucible, making it difficult to achieve large-scale production and high energy consumption.
By hydrolyzing the mixed system of silicates, deionized water and alcohols, adjusting the pH to 8-12, performing gelation treatment, and sonication at the maximum gelation speed, followed by aging and calculating Treatment to prepare low hydroxyl low inclusion quartz sand.
The low hydroxyl and low inclusion content of quartz sand are achieved, which improves the crystal pulling quality and service life of the quartz crucible, while simplifying the synthesis process and reducing energy consumption.
Smart Images

Figure CN119038562A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of photovoltaic technology, and in particular relates to low-hydroxyl and low-inclusion quartz sand and a preparation method and application thereof. Background Art
[0002] High-purity quartz sand is an important special material, which is widely used in high-end fields such as semiconductors, optoelectronics, optical fiber, photovoltaics, light sources, military aerospace, optics, etc. Quartz sand is used to make quartz crucibles in the photovoltaic field. The quality of quartz sand will affect the crystal pulling quality and service life of the quartz crucible. The hydroxyl content affects the strength of the crucible. Too high a content will cause the crucible to soften and deform; impurities mainly come from fluid inclusions and lattice impurities in quartz sand, especially alkali metal ions, which will accelerate crystallization and reduce the strength of the crucible; the bubble content will affect the crystallization of silicon and the quality of single crystal silicon. Therefore, using high-purity and low-bubble-density quartz sand to make quartz crucibles can improve the crystal pulling quality and service life of quartz crucibles.
[0003] There are two methods for chemically synthesizing high-purity quartz sand: direct method and indirect method. The direct method includes electrofusion method, gas refining method, vapor deposition method and plasma vapor deposition method (PCVD), etc. These methods can prepare high-purity and high-quality quartz sand, but the equipment requirements and energy consumption are high, and it is difficult to achieve large-scale production. The indirect method is also called the two-step method. In the first step, the silicon source is hydrolyzed to obtain a low-density SiO2 loose body. The loose body contains a large amount of impurities, such as hydroxyl groups, moisture, bubbles, etc., which need to be removed in the second step. The synthesis process of the indirect method is relatively simple compared to the direct method, with lower equipment requirements and energy consumption, and it is feasible for large-scale production, but there are still problems with high hydroxyl content and inclusions. Summary of the invention
[0004] The main purpose of the present invention is to provide a method for preparing low-hydroxyl and low-inclusion quartz sand. The quartz sand prepared by the method has low hydroxyl content and inclusion content, and has the characteristics of simple synthesis process and low energy consumption.
[0005] The present invention also provides low-hydroxyl and low-inclusion quartz sand, which is prepared by the above preparation method and has the characteristics of low hydroxyl content and low inclusion content.
[0006] The present invention also provides a quartz crucible, comprising the above-mentioned quartz sand. Therefore, the hydroxyl content and inclusion content in the quartz crucible are relatively low, thereby improving the crystal pulling quality and service life thereof.
[0007] In a first aspect, the present invention provides a method for preparing low-hydroxyl and low-inclusion quartz sand, comprising the following steps: 1) hydrolyzing a mixed system including silicate, deionized water and alcohol to obtain a hydrolysis product; 2) adjusting the pH value of the hydrolyzate to 8-12 to obtain a sol; 3) allowing the sol to stand for gelation, and after a period of time t from the time when the system reaches the maximum gelation speed, subjecting the system to ultrasonic treatment to obtain an ultrasonic system; 4) performing an aging treatment and a calcination treatment on the ultrasonic system in sequence to obtain the low-hydroxyl and low-inclusion quartz sand; Among them, (t max -t0)≤t≤1.2(t max -t0), t max t0 is the moment when the maximum speed of the gelation process appears during the gelation process; t1 is the critical moment when gel is produced during the gelation process.
[0008] According to the preparation method described above, the ultrasonic treatment time is 0.3-0.6 (t max -t0).
[0009] In the preparation method as described above, the ultrasonic treatment is carried out under vacuum conditions.
[0010] According to the preparation method described above, the aging treatment is carried out under vacuum conditions, and the aging treatment time is 1-3 (t max -t0).
[0011] The preparation method as described above, before the calcination treatment, further comprises: washing, filtering and drying the product after the aging treatment in sequence; The drying process is carried out at a temperature of 100-180°C and for a time of more than 6 hours.
[0012] The preparation method as described above, wherein the calcination treatment includes a first calcination treatment and a second calcination treatment; The temperature of the second calcination treatment is 300-950° C. higher than the temperature of the first calcination treatment.
[0013] In the preparation method as described above, the first calcination treatment is carried out under oxygen-containing conditions, the temperature of the first calcination treatment is 450-600° C., and the time is 6-24 hours.
[0014] In the preparation method as described above, the second calcination treatment is carried out under vacuum conditions, the temperature of the second calcination treatment is 900-1400° C., and the time is 6-24 hours.
[0015] In a second aspect, the present invention provides a low-hydroxyl and low-inclusion quartz sand prepared using the above-mentioned preparation method.
[0016] In a third aspect, the present invention provides a quartz crucible, comprising the low-hydroxyl and low-inclusion quartz sand described above or the low-hydroxyl and low-inclusion quartz sand prepared by the above preparation method.
[0017] The preparation method of low-hydroxyl and low-inclusion quartz sand provided by the present invention comprises the following steps: performing ultrasonic treatment on the system during the gelation process of the sol, and then performing aging and calcining treatment on the ultrasonic system, so as to obtain quartz sand with low hydroxyl content and inclusion content. Meanwhile, the ultrasonic treatment has the advantages of simple synthesis process and low energy consumption compared with the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the following briefly introduces the drawings required for use in the embodiments of the present invention or related technologies. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0019] Figure 1 This is a trend diagram of scattering intensity variation during the preparation of quartz sand in Example 1 of the present invention; Figure 2 This is a graph showing the trend of scattering intensity changes during the preparation of quartz sand in Example 9 of the present invention. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] In a first aspect, the present invention provides a method for preparing low-hydroxyl and low-inclusion quartz sand, comprising the following steps: 1) hydrolyzing a mixed system including silicate, deionized water and alcohol to obtain a hydrolysis product; 2) adjusting the pH value of the hydrolyzate to 8-12 to obtain a sol; 3) allowing the sol to stand for gelation, and after a period of time t from the time when the system reaches the maximum gelation speed, subjecting the system to ultrasonic treatment to obtain an ultrasonic system; 4) performing an aging treatment and a calcination treatment on the ultrasonic system in sequence to obtain the low-hydroxyl and low-inclusion quartz sand; Among them, (t max -t0)≤t≤1.2(t max -t0), t maxt0 is the moment when the maximum speed of the gelation process appears during the gelation process; t1 is the critical moment when gel is produced during the gelation process.
[0022] The method for preparing low-hydroxyl and low-inclusion quartz sand provided by the invention comprises the following steps: subjecting a mixed system to hydrolysis treatment, pH value adjustment, ultrasonic treatment, aging treatment and roasting treatment to obtain low-hydroxyl and low-inclusion quartz sand.
[0023] Specifically, in step 1), the hydrolysis treatment refers to the reaction of silicate with deionized water to generate a hydrolysis product consisting of silicic acid and alcohols. Since silicate is insoluble in water, additional alcohols need to be added to increase the solubility of silicate in water, thereby increasing the hydrolysis rate of silicate.
[0024] The present invention does not limit the type of silicate. For example, the silicate can be selected from at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate, pentyl orthosilicate, isopropyl orthosilicate, isobutyl orthosilicate, isopentyl orthosilicate, dimethyl orthosilicate, diethyl orthosilicate and diisopropyl orthosilicate, preferably at least one of ethyl orthosilicate, propyl orthosilicate and butyl orthosilicate.
[0025] The present invention does not limit the selection of alcohols. For example, the alcohol can be selected from at least one of methanol, ethanol, n-propanol, n-butanol, n-pentanol, isopropanol, isobutanol, isopentanol and isopropanol, preferably at least one of methanol, ethanol and n-propanol.
[0026] It is understandable that in order to make the rate of silicate hydrolysis faster, and thus make the preparation method provided by the present invention have higher production efficiency, in one embodiment, after the silicate, deionized water and alcohol are mixed, an acidic catalyst is added to the mixture, and heated and stirred. The present invention does not limit the type, heating temperature and stirring time of the acidic catalyst, and the technical effect of accelerating the hydrolysis treatment speed of the silicate is sufficient. In a specific embodiment, the acidic catalyst can be selected from at least one of sulfuric acid, hydrochloric acid, nitric acid, acetic acid, citric acid, phosphoric acid, formic acid, hydrofluoric acid, etc., the heating temperature is 60-90°C, and the stirring time is 0.5-3h.
[0027] In step 2), an alkaline substance is added dropwise to the hydrolyzate, and the pH value of the system is detected in real time, and the pH value of the system is adjusted to a range of 8-12 to form a sol. The pH value is controlled at 8-12, preferably 8.5-10.5. Within this range, the generated sol particles are usually more uniform and stable, reducing the possibility of premature aggregation and precipitation of particles. By accurately controlling the pH value, a sol with good dispersibility can be obtained to form a uniform three-dimensional network structure.
[0028] The present invention does not limit the selection of the alkaline substance. For example, the alkaline substance can be selected from at least one of aqueous ammonia, aqueous sodium carbonate solution, aqueous sodium hydroxide solution, aqueous potassium hydroxide solution, aqueous sodium bicarbonate solution, aqueous calcium hydroxide solution, aqueous barium hydroxide solution, and aqueous aluminum hydroxide solution, preferably at least one of aqueous ammonia, aqueous sodium carbonate solution, and aqueous sodium hydroxide solution.
[0029] In step 3), the sol is kept at a pH value within the range of 8-12, and allowed to stand for gelation. After a period of t from the time when the system reaches the maximum gelation speed, the system is subjected to ultrasonic treatment. Under the action of ultrasonic waves, the bubbles inside the system are subjected to vibration and pressure changes, gradually grow larger and rise to the surface of the gel, thereby reducing the number of inclusions and obtaining an ultrasonic system; wherein (t max -t0)≤t≤1.2(t max -t0), t max It is the moment when the maximum speed of gelation occurs during the gelation process; t0 is the critical moment when gel is produced during the gelation process.
[0030] t max and t0 can be determined by analyzing the light scattering state of the sol. Specifically, the system can be sampled every 0.5h, and the scattering intensity of the sample can be determined by the dynamic light scattering (DLS) method. In the sol stage, the particles in the system are small and well dispersed, and the light scattering intensity is low, because the scattering of light by individual nanoparticles is weak. In the gel stage, the sol particles gradually aggregate to form a three-dimensional network structure, and the light scattering intensity will change significantly. Therefore, this principle can be used to detect the scattering curve of the sample over time, and then make a differential curve by calculating the scattering curve as a differential value, that is, the differential curve represents the change of the scattering intensity change rate over time. The rapid increase in scattering intensity corresponds to the process of sol turning into gel, in which the gel network gradually forms and becomes tighter. The peak time of the differential curve corresponds to the critical moment of producing gel in the gelation process, that is, the moment when the sol just begins to turn into gel, and the gel structure just begins to form. The peak time point of the differential curve represents the fastest moment of gelation, that is, the moment when the maximum speed of gelation occurs in the gelation process, and the gel structure is initially formed, but has not yet been fully solidified. After selecting the time t, the system is subjected to ultrasonic treatment to ensure that the ultrasonic treatment time is long enough to remove bubbles, but not too long to destroy the gel structure that has been formed. Among them, the main component of the gel is the silica loose body formed by the dehydration condensation of silicic acid. The silica loose body is a silica species with a loose three-dimensional network structure formed by interconnected silicon oxygen tetrahedron (SiO4) structures.
[0031] In step 4), the ultrasonic system is aged. During the aging process, the three-dimensional network structure of the gel will be further improved, and Si-O-Si bonds will continue to form, making the gel more stable and compact, thereby improving the mechanical strength, thermal stability and chemical stability of the gel. In addition, aging and calcination treatments can also promote the discharge of impurities such as hydroxyl groups in the system, which is beneficial to reducing the content of hydroxyl groups in the final quartz sand.
[0032] Furthermore, in order to obtain a more convenient quartz sand product, in one embodiment, after the calcination treatment, the obtained low-hydroxyl and low-inclusion quartz sand is crushed and sieved to obtain quartz sand with a particle size between 100-200 meshes.
[0033] The preparation method of low-hydroxyl and low-inclusion quartz sand provided by the present invention comprises the following steps: performing ultrasonic treatment on the system during the gelation process of the sol, and then performing aging and calcining treatment on the ultrasonic system, so as to obtain quartz sand with low hydroxyl content and inclusion content. Meanwhile, the ultrasonic treatment has the advantages of simple synthesis process and low energy consumption compared with the prior art.
[0034] In some embodiments of the present invention, the ultrasonic treatment time is 0.3-0.6 (t max -t0).
[0035] The main purpose of the ultrasonic treatment in the present invention is to promote the formation and rise of bubbles through acoustic vibration. If the ultrasonic treatment time is too long, it may have a negative impact on the gel structure that has been formed, such as destroying the network structure and causing the mechanical properties of the gel to decrease; if the ultrasonic treatment time is too short, the purpose of fully removing bubbles cannot be achieved. Therefore, making the ultrasonic treatment time within an appropriate range can achieve the removal of bubbles while protecting the structural integrity of the gel.
[0036] In some embodiments of the present invention, the ultrasonic treatment is performed under vacuum conditions.
[0037] In the present invention, the ultrasonic treatment is carried out under vacuum conditions, that is, a vacuum operation is carried out while the ultrasound is applied, which can reduce the ambient pressure and promote the expansion and escape of bubbles. When the gel is initially formed but not completely solidified, the gel structure has a certain plasticity and can release the internal bubbles under the simultaneous action of ultrasound and vacuum. If the gel is completely solidified, the bubbles will be trapped in the gel network and difficult to remove. By combining the ultrasonic treatment and vacuuming, the bubbles in the gel can be further removed to ensure the uniformity and stability of the gel structure.
[0038] In some embodiments of the present invention, the aging treatment is performed under vacuum conditions, and the aging treatment time is 1-3 (t max -t0).
[0039] In the present invention, the aging treatment is carried out under vacuum conditions, and the aging treatment time is within an appropriate range. Maintaining the vacuum environment can continue to reduce the pressure in the system, help the residual bubbles to further expand and escape from the gel, and if the normal pressure is quickly restored, the gas dissolved in the gel may re-form bubbles. In addition, the vacuum environment helps the volatilization of solvents and other volatile substances, promotes the drying and curing of the gel, and accelerates the curing and aging process of the gel, thereby improving the mechanical strength and stability of the gel.
[0040] Therefore, the aging treatment is carried out under vacuum conditions for an appropriate time to prevent the regeneration of bubbles, ensure that the bubbles are completely discharged, and improve the mechanical strength and stability of the gel.
[0041] In some embodiments of the present invention, before the calcination treatment, the process further comprises: washing, filtering and drying the product after the aging treatment in sequence; The drying process is carried out at a temperature of 100-180°C and for a time of more than 6 hours.
[0042] In the present invention, the aged product can be placed on a filter membrane or filter paper, preliminarily washed with deionized water to remove surface residues, then the washing-filtration cycle is repeated, and the conductivity of the washed liquid is tested using a conductivity meter until the conductivity drops below 5µS / cm, indicating that the residual chemical reagents and by-products have been completely removed. The drying temperature is 100-180°C and the drying time is greater than 6 hours, in order to ensure that the moisture and organic matter in the quartz sand are completely evaporated and removed, and to prevent the moisture and organic matter from decomposing and reacting under the subsequent roasting treatment conditions to produce hydroxyl groups and other compounds, thereby affecting the purity and quality of the quartz sand.
[0043] The present invention does not limit the treatment temperature of the aging treatment. In one embodiment, the aging temperature is 80°C.
[0044] In some embodiments of the present invention, the calcination process includes a first calcination process and a second calcination process; The temperature of the second calcination treatment is 300-950° C. higher than the temperature of the first calcination treatment.
[0045] The temperature of the second calcination treatment is defined as 300-950°C higher than that of the first calcination treatment. The first calcination treatment can remove the organic matter and water remaining in the gel, and can also promote the lattice rearrangement of the quartz crystal, so that the original oxygen defects in the quartz crystal are moved, eliminated or combined, thereby obtaining a quartz sand product with a stable structure. The second calcination treatment can accelerate the volatilization and decomposition of water and organic matter in the gel, and further improve the purity of the quartz sand product.
[0046] In some embodiments of the present invention, the first calcination treatment is performed under oxygen-containing conditions, the temperature of the first calcination treatment is 450-600° C., and the time is 6-24 hours.
[0047] In the present invention, the first calcination treatment is carried out in an oxygen-containing atmosphere at a temperature of 450-600° C. and a time of 6-24 hours, which can further remove residual organic matter and moisture in the gel, promote lattice rearrangement of the quartz crystal, and move, eliminate or combine the original oxygen defects in the quartz crystal, thereby forming a quartz sand product with a more stable structure.
[0048] In some embodiments of the present invention, the second calcination treatment is performed under vacuum conditions, the temperature of the second calcination treatment is 900-1400° C., and the time is 6-24 hours.
[0049] The second calcination treatment in the present invention is carried out in a vacuum environment at 900-1400°C for 6-24h in order to further improve the purity and quality of the quartz sand. The second calcination treatment is carried out at high temperature for a suitable time, and the impurities and inclusions remaining in the quartz sand will gradually volatilize or decompose, and the discharge of the decomposed products can be accelerated under vacuum conditions.
[0050] In a second aspect, the present invention provides a low-hydroxyl and low-inclusion quartz sand prepared using the above-mentioned preparation method.
[0051] The low-hydroxyl and low-inclusion quartz sand of the present invention is prepared by the preparation method provided by the first aspect above, and therefore, the quartz sand has the characteristics of low hydroxyl content and low inclusion content.
[0052] In a third aspect, the present invention provides a quartz crucible, comprising the low-hydroxyl and low-inclusion quartz sand described above or the low-hydroxyl and low-inclusion quartz sand prepared by the above preparation method.
[0053] The quartz crucible of the present invention comprises the low-hydroxyl and low-inclusion quartz sand, so the hydroxyl content and inclusion content in the quartz crucible are low, thereby improving the crystal pulling quality and service life thereof.
[0054] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0055] Example 1 The preparation method of the low-hydroxyl and low-inclusion quartz sand of the present embodiment comprises the following steps: 1) Mix 30 kg of tetraethyl orthosilicate, 60 kg of deionized water, and 30 kg of ethanol, add 5 kg of 1 mol / L hydrochloric acid as an acid catalyst, heat to 60°C and stir for 1.5 hours to completely hydrolyze the tetraethyl orthosilicate to obtain a hydrolysis product.
[0056] 2) Adding aqueous ammonia to the hydrolyzate at a rate of 150 g / min until the pH value reaches 9.5 to obtain a sol.
[0057] 3) Keep the sol at a pH of 9.5 and place it in a constant temperature environment of 80°C. Take samples every 0.5 h for DLS light scattering intensity analysis. Differentiate the data curve to obtain a differential curve, such as Figure 1 As shown, from Figure 1 From the curve, we can see that the time when the differential curve begins to peak is the critical time for gelation, t0=3.5h, and the time when the peak appears is the time when the maximum gelation rate appears, t max =4.5h, then t max -t0=1h.
[0058] 4) From the moment when the maximum gelation speed appears t max = 4.5h, and after t time, ultrasonic treatment is performed and vacuum is simultaneously applied to promote the rapid detachment of bubbles in the gel fragments. Time t is 1.1 times t max -t0, that is, 1.1×1h=1.1h.
[0059] 5) Ultrasonic treatment 0.5 (t max After t0 = 0.5 h, turn off the ultrasound and continue to maintain the vacuum to allow the gel to continue aging for 2 (t max -t0) = 2h, and the aged product was obtained.
[0060] 6) The aged product was washed with deionized water, separated and dried at 120°C for 8 hours to obtain a dried product.
[0061] 7) Under air atmosphere, the dried product is subjected to a first calcination treatment at a heating rate of 2°C / min, a temperature of 550°C, and a time of 6 hours to obtain a first calcined product.
[0062] 8) Evacuate to an absolute pressure of 5 Pa, perform a second calcination treatment on the first calcined product, and heat up at a rate of 2°C / min. The temperature of the second calcination treatment is 1400°C for 24 hours to obtain a second calcined product.
[0063] 9) Cooling the second calcined product, taking out the cooled material, crushing it into coarse-grained quartz sand, and passing the crushed quartz sand through a screening device to separate quartz sand with a particle size between 100 and 200 meshes.
[0064] Example 2 The preparation method of low-hydroxyl and low-inclusion quartz sand in Example 2 is basically the same as that in Example 1, except that the time t in step 4) is 1.0 times t max-t0, that is, 1.0×1h=1.0h.
[0065] Example 3 The preparation method of low-hydroxyl and low-inclusion quartz sand in Example 3 is basically the same as that in Example 1, except that the time t in step 4) is 1.2 times t max -t0, that is, 1.2×1h=1.2h.
[0066] Example 4 The preparation method of low-hydroxyl and low-inclusion quartz sand in Example 4 is basically the same as that in Example 1, except that the ultrasonic treatment time in step 5) is 0.3 (t max -t0)=0.3h.
[0067] Example 5 The preparation method of low-hydroxyl and low-inclusion quartz sand in Example 5 is basically the same as that in Example 1, except that the ultrasonic treatment time in step 5) is 0.6 (t max -t0)=0.6h.
[0068] Example 6 The preparation method of low-hydroxyl and low-inclusion quartz sand in Example 6 is basically the same as that in Example 1, except that the aging treatment time in step 5) is 1 (t max -t0)=1h.
[0069] Example 7 The preparation method of low-hydroxyl and low-inclusion quartz sand in Example 7 is basically the same as that in Example 1, except that the aging treatment time in step 5) is 3 (t max -t0)=3h.
[0070] Example 8 The preparation method of low-hydroxyl and low-inclusion quartz sand in Example 8 is basically the same as that in Example 1, except that the drying treatment temperature in step 6) is 150° C. and the time is 10 h.
[0071] Example 9 The preparation method of the low-hydroxyl and low-inclusion quartz sand of the present embodiment comprises the following steps: 1) Mix 30 kg of methyl orthosilicate, 60 kg of deionized water, and 30 kg of methanol, add 5 kg of 1 mol / L hydrochloric acid as an acid catalyst, heat to 60°C and stir for 1.5 hours to completely hydrolyze the methyl orthosilicate to obtain a hydrolysis product.
[0072] 2) Adding aqueous ammonia to the hydrolyzate at a rate of 150 g / min until the pH value reaches 9.5 to obtain a sol.
[0073] 3) Keep the sol at a pH of 9.5 and place it in a constant temperature environment of 80°C. Take samples every 0.5 h for DLS light scattering intensity analysis. Differentiate the data curve to obtain a differential curve, such as Figure 2 As shown, from Figure 2 From the curve, we can see that the time when the differential curve begins to peak is the critical time for gelation, t0=3h, and the time when the peak value appears is the time when the maximum gelation rate appears, t max =4h, then t max -t0=1h.
[0074] 4) From the moment when the maximum gelation speed appears t max = 4h, after t time, ultrasonic treatment was performed and vacuum was simultaneously applied to promote the rapid detachment of bubbles in the gel fragments. Time t is 1.1 times t max -t0, that is, 1.1×1h=1.1h.
[0075] 5) Ultrasonic treatment 0.5 (t max After t0 = 0.5 h, turn off the ultrasound and continue to maintain the vacuum to allow the gel to continue aging for 2 (t max -t0) = 2h, and the aged product was obtained.
[0076] 6) The aged product was washed with deionized water, separated and dried at 120°C for 8 hours to obtain a dried product.
[0077] 7) Under air atmosphere, the dried product is subjected to a first calcination treatment at a heating rate of 2°C / min, a temperature of 550°C, and a time of 6 hours to obtain a first calcined product.
[0078] 8) Evacuate to an absolute pressure of 5 Pa, perform a second calcination treatment on the first calcined product, and heat up at a rate of 2°C / min. The temperature of the second calcination treatment is 1400°C for 24 hours to obtain a second calcined product.
[0079] 9) Cooling the second calcined product, taking out the cooled material, crushing it into coarse-grained quartz sand, and passing the crushed quartz sand through a screening device to separate quartz sand with a particle size between 100 and 200 meshes.
[0080] Example 10 The preparation method of low-hydroxyl and low-inclusion quartz sand in Example 10 is basically the same as that in Example 1, except that the temperature of the first calcination treatment in step 7) is 500° C. and the time is 12 hours.
[0081] Embodiment 11 The preparation method of low-hydroxyl and low-inclusion quartz sand in Example 11 is basically the same as that in Example 1, except that the temperature of the second calcination treatment in step 8) is 1200° C. and the time is 18 hours.
[0082] Example 12 The preparation method of low-hydroxyl and low-inclusion quartz sand in Example 12 is basically the same as that in Example 1, except that the pH value in step 2) and step 3) is 10.5.
[0083] Comparative Example 1 The preparation method of the low-hydroxyl and low-inclusion quartz sand of this comparative example comprises the following steps: 1) Mix 30 kg of tetraethyl orthosilicate, 60 kg of deionized water, and 30 kg of ethanol, add 5 kg of 1 mol / L hydrochloric acid as an acid catalyst, heat to 60°C and stir for 1.5 hours to completely hydrolyze the tetraethyl orthosilicate to obtain a hydrolysis product.
[0084] 2) Adding aqueous ammonia to the hydrolyzate at a rate of 150 g / min until the pH value reaches 9.5 to obtain a sol.
[0085] 3) Keep the sol at a pH of 9.5 and place it in a constant temperature environment of 80°C for 6.1 hours to form a gel. Allow the gel to continue aging for 2 (t max -t0) = 2h, and the aged product was obtained.
[0086] 4) The aged product was washed with deionized water, separated and dried at 120°C for 8 hours to obtain a dried product.
[0087] 5) Under air atmosphere, the dried product is subjected to a first calcination treatment at a heating rate of 2°C / min, a temperature of 550°C, and a time of 6 hours to obtain a first calcined product.
[0088] 6) Evacuate to an absolute pressure of 5 Pa, perform a second calcination on the first calcined product, and heat up at a rate of 2°C / min. The temperature of the second calcination is 1400°C for 24 hours to obtain a second calcined product.
[0089] 7) Cooling the second calcined product, taking out the cooled material, crushing it into coarse-grained quartz sand, and passing the crushed quartz sand through a screening device to separate quartz sand with a particle size between 100 and 200 meshes.
[0090] Comparative Example 2 The preparation method of low-hydroxyl and low-inclusion quartz sand in Comparative Example 2 is basically the same as that in Example 1, except that the time t in step 4) is 0.5 times t max-t0, that is, 0.5×1h=0.5h.
[0091] Comparative Example 3 The preparation method of low-hydroxyl and low-inclusion quartz sand in Comparative Example 3 is basically the same as that in Example 1, except that the time t in step 4) is twice that of t max -t0, that is, 2×1h=2h.
[0092] Test example 1. Measure the hydroxyl content of the sample using the following method: 1) Accurately weigh 0.02g of sample and 0.8g of KBr, and grind them in an agate mortar for at least 5 minutes until there is no obvious granularity after grinding; 2) Accurately weigh 0.2 g of the ground and diluted sample and spread it on the tableting mold as evenly as possible. The pressure is 3.0 MPa. After reaching 3.0 MPa, hold it for 60 seconds and then release the pressure. 3) First analyze under empty sample to obtain the instrument background value, then put the sample into the infrared spectrometer for testing, repeat three times, select two parallel results and take the average value, the results are shown in Table 1.
[0093] 2. Measure the number of inclusions in the sample using the following method: 1) Take 10g of the prepared quartz sand powder, put it into a straight barrel molybdenum crucible, put it into a vacuum graphite furnace after compaction, and treat it at 1850℃ for 2h under vacuum environment; 2) Take out the melted quartz slice, and go through the process of slicing, coarse grinding, fine grinding, polishing, and gluing. After gluing, grind the other side of the slice according to the above grinding and polishing process, and grind it into a slice with a thickness of 0.3-0.5mm. Put the prepared slice under a microscope and observe it at a magnification of 400-500 times. The area in the field of view can be determined through the ruler sample, and the number of inclusions per square centimeter can be calculated. The results are shown in Table 1.
[0094] Table 1 Inclusion number and hydroxyl content of Examples 1-12 and Comparative Examples 1-3
[0095] As can be seen from Table 1, compared with the comparative example, the preparation method of low-hydroxyl and low-inclusion quartz sand provided by the present invention can obtain quartz sand with low hydroxyl content and inclusion content by subjecting the system to ultrasonic treatment during the gelation process of the sol, and then aging and calcining the ultrasonic system. At the same time, the ultrasonic treatment has the advantages of simple synthesis process and low energy consumption compared with the prior art.
[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing low-hydroxyl and low-inclusion quartz sand, characterized in that: The following steps are involved: 1) hydrolyzing a mixed system including silicate, deionized water and alcohol to obtain a hydrolysis product; 2) adjusting the pH value of the hydrolyzate to 8-12 to obtain a sol; 3) allowing the sol to stand for gelation, and after a period of time t from the time when the system reaches the maximum gelation speed, subjecting the system to ultrasonic treatment to obtain an ultrasonic system; 4) performing aging treatment and calcination treatment on the ultrasonic system in sequence to obtain the low-hydroxyl and low-inclusion quartz sand; Among them, (t max -t0)≤t≤1.2(t max -t0), t max t0 is the moment when the maximum speed of the gelation process appears during the gelation process; t1 is the critical moment when gel is produced during the gelation process.
2. The preparation method according to claim 1, characterized in that: The ultrasonic treatment time is 0.3-0.6 (t max -t0).
3. The preparation method according to claim 1 or 2, characterized in that: The ultrasonic treatment is performed under vacuum conditions.
4. The preparation method according to claim 3, characterized in that: The aging treatment is carried out under vacuum conditions, and the aging treatment time is 1-3 (t max -t0).
5. The preparation method according to claim 4, characterized in that: Before the calcination treatment, the method further comprises: washing, filtering and drying the product after the aging treatment in sequence; The drying process is carried out at a temperature of 100-180° C. and for a time of more than 6 hours.
6. The preparation method according to claim 5, characterized in that: The roasting process includes a first roasting process and a second roasting process; The temperature of the second calcination treatment is 300-950° C. higher than the temperature of the first calcination treatment.
7. The preparation method according to claim 6, characterized in that: The first calcination treatment is carried out under oxygen-containing conditions, the temperature of the first calcination treatment is 450-600° C., and the time is 6-24 hours.
8. The preparation method according to claim 6 or 7, characterized in that: The second calcination treatment is performed under vacuum conditions, the temperature of the second calcination treatment is 900-1400° C., and the time is 6-24 hours.
9. A low-hydroxyl and low-inclusion quartz sand, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 8.
10. A quartz crucible, characterized in that: The invention comprises the low-hydroxyl and low-inclusion quartz sand as described in claim 9 or the low-hydroxyl and low-inclusion quartz sand prepared by the preparation method as described in any one of claims 1 to 8.
Citation Information
Patent Citations
High-temperature-resistant heteromorphic nanocrystalline aerogel material and preparation method thereof
CN110282958A
High-purity quartz sand and preparation method and application thereof
CN110862091A
Low-hydroxyl low-inclusion quartz sand and preparation method thereof
CN116835866A
Preparation method of high-purity synthetic quartz sand
CN118702112A
Method for preparing high-purity quartz sand from waste quartz crucible, high-temperature furnace and method for preparing high-purity quartz sand and high-purity quartz sand
WO2024093654A1
Cited By
Method and equipment for purifying high-purity quartz sand from granite pegmatite
CN119983788A
Preparation method of quartz sand
CN121377048A