Low-carbon pervious concrete based on modified recycled aggregate and preparation method of low-carbon pervious concrete
Through the water-permeable concrete preparation method of modified regenerated aggregate, the problem of the difference in carbonization degree of permeable concrete of low-carbon cementitious materials is solved, the carbonization homogeneity and the compactness of the internal structure of concrete are improved, and the low-carbon and environmentally friendly water-permeable concrete preparation is realized. Promote the green development of the cement industry.
Patent Information
- Application Number
- CN202411245808.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-06
AI Technical Summary
Preparation of water-permeable concrete for low-carbon gelling materials has a problem of large differences in the degree of carbonization during carbonization curing, which leads to inconsistent internal and external strengths and affects service life.
The permeable concrete preparation method of modified regenerated aggregate is used to improve the carbonization homogeneity and compactness of the internal structure of the concrete by mechanical crushing of building demolitions, removing impurities, soaking in aqueous acetic acid solution, immersion of calcium source solution and microbial suspension.
Improve the defects of recycled aggregates, improve the carbonization homogeneity and robustness of low-carbon permeable concrete, reduce voids, reduce the CO2 purification process for carbonization curing, reduce industrial energy consumption, and promote the green and healthy development of the cement industry. .
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and particularly relates to permeable concrete and a preparation method thereof. Background Art
[0002] With the huge emissions of traditional cement and concrete industries, there is no doubt that they need to take on greater responsibility for emission reduction. Low-carbon concrete not only uses low-carbon cement with lower carbon emissions, but also fixes a portion of carbon dioxide during the carbonation curing process, which has an important impact on carbon reduction and emission reduction in the building materials industry. At present, research on low-carbon concrete has become a hot topic. At present, how to deepen the depth of carbonation is the focus and difficulty of low-carbon concrete research. Researchers mainly study carbonation curing system, mix design, and carbonation enhancers, but there is little research on the carbonation situation inside low-carbon concrete. There are a large amount of construction and demolition waste in the world, which pollutes the environment; the consumption and mining of natural sand and gravel on the ecological environment is also a problem that needs to be solved urgently. Therefore, the use of construction waste as recycled aggregate is also one of the research hotspots; however, recycled aggregates have the disadvantages of large porosity, high water absorption, and low strength.
[0003] Carbonation curing is inevitable when using low-carbon cementitious materials to prepare permeable concrete. Although permeable concrete has certain air permeability due to its own characteristics, there is still a large difference in the degree of carbonization between the surface and the interior during the actual preparation process, which leads to inconsistent internal and external strength and seriously affects the service life. Summary of the invention
[0004] In view of the problem that there is a large difference in the degree of carbonization during the carbonization curing process of permeable concrete prepared from low-carbon cementitious materials, the present invention provides a permeable concrete based on modified recycled aggregate and a preparation method thereof. By modifying the recycled aggregate, not only the defects of the recycled aggregate itself can be improved, but also the carbonization homogeneity of the low-carbon permeable concrete can be improved.
[0005] In order to achieve the above purpose, the technical solutions adopted are as follows:
[0006] The permeable concrete based on modified recycled aggregate has the following composition by weight:
[0007] 260-500 parts of low-carbon cementitious materials, 900-1600 parts of modified recycled coarse aggregate, 50-200 parts of fine aggregate, 90-180 parts of water, and 9-30 parts of water reducer;
[0008] The modified recycled aggregate preparation method comprises the following steps:
[0009] (1) Mechanically crushing the demolished building materials to remove impurities and obtain 5-10 mm recycled coarse aggregate;
[0010] (2) the recycled coarse aggregate is soaked or sprayed with an acetic acid aqueous solution;
[0011] (3) Under vacuum conditions, the mixture is sequentially impregnated with a calcium source solution and a nutrient solution; and finally, the mixture is impregnated with a microbial suspension.
[0012] According to the above scheme, the concentration of the acetic acid aqueous solution in step 2 is 1% to 3%, and the treatment time is 12h to 24h.
[0013] According to the above scheme, the calcium source solution in step 3 is a calcium lactate solution, or a mixed solution of calcium lactate and calcium formate, with a concentration of 60-80 g / l.
[0014] According to the above scheme, the nutrient solution in step 3 is a yeast extract solution or a glucose solution with a concentration of 1 to 3 g / l.
[0015] According to the above scheme, the microorganism in step 3 is an aerobic Bacillus pseudofirmus or Bacillus cohnii.
[0016] According to the above scheme, each immersion time in step 3 is 5 to 8 hours, and drying is required after each immersion.
[0017] According to the above scheme, the low-carbon cementitious material is a mixture of low-carbon clinker and mineral powder, and the ratio of low-carbon clinker to mineral powder is 1:0.25-0.6; the content of CS, C2S and C3S2 in the low-carbon clinker is ≥80%.
[0018] According to the above scheme, the fineness modulus of the fine aggregate is 2.1-3.2, the stone powder content is ≤17%, and the crushing value is ≤20%.
[0019] The method for preparing the permeable concrete based on modified recycled aggregate comprises the following steps:
[0020] 1) Mixing the above raw materials in a mixer to obtain a permeable concrete mixture;
[0021] 2) The obtained permeable concrete mixture is vibrated and pressed into shape, and then placed in a CO2 curing environment for carbonization curing to obtain a permeable concrete product.
[0022] According to the above scheme, the carbonization curing system is: CO2 volume concentration 20-80%, O2 volume concentration 20-80%, curing temperature 20-55°C, curing pressure 0.1-1.0MPa, and curing time 12-48h.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] Recycled aggregates have the characteristics of high water absorption and porosity. In a vacuum environment, they can absorb more microorganisms and calcium source substrates, which helps microorganisms decompose to produce more CO2 and CaCO3, making the internal structure of concrete more compact.
[0025] During the modification process of the recycled aggregate of the present invention, calcium lactate and calcium formate are adsorbed, wherein calcium lactate reacts with O2 to generate CaCO3 and CO2; calcium formate reacts with Ca(OH)2 and O2 to generate CaCO3; carbonization active components in the low-carbon cementitious material and unhydrated cement minerals on the surface of the recycled aggregate further react with the generated CO2 to obtain more CaCO3 precipitation, the carbonization degree inside the concrete is more sufficient, and the carbonization homogeneity of the concrete is improved; at the same time, the carbonization effect reduces the voids in the recycled aggregate and improves the firmness.
[0026] In the process of regenerated aggregate modification of the present invention, microorganisms are adsorbed, and after being activated, the microorganisms synthesize acid anhydrase by themselves, and use the calcium source substrate attached to the surface of the modified regenerated coarse aggregate as a deposition precursor to react with substrates such as calcium lactate or calcium formate to generate CaCO3. The reaction mechanism is as follows:
[0027] CaC6H 10 O6+6O2→CaCO3↓+5CO2↑+5H2O;
[0028] Ca(CHO2)2+Ca(OH)2+O2→2CaCO3↓ + 2H2O.
[0029] The present invention requires that the carbonization curing CO2 concentration be 20-80% VOL, and the fume concentration at the kiln tail can meet the requirement, thereby reducing the CO2 purification process in production and reducing industrial energy consumption.
[0030] Low-carbon cementitious materials and recycled aggregates pretreated with acetic acid are suitable for the survival of microorganisms, and can improve the survival rate of microorganisms without the need for biological sealing; low-carbon cementitious materials are composed of low-carbon clinker and mineral powder, and the carbon emission factors of both are smaller than those of ordinary silicate clinker. Using low-carbon cementitious materials to replace traditional silicate cement can promote the green and healthy development of the cement industry. DETAILED DESCRIPTION
[0031] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.
[0032] The specific implementation method part provides two kinds of low-carbon cementitious materials, in which the ratio of low-carbon cement to mineral powder in the 1# low-carbon cementitious material is 1:0.3, and the contents of mineral components CS, C2S, and C3S2 are 91% respectively. In the 2# low-carbon cementitious material, the ratio of low-carbon cement to mineral powder is 1:0.5, and the contents of mineral components CS, C2S, and C3S2 are 86%, and the ordinary silicate cement used is PO42.5 cement.
[0033] The recycled coarse aggregate used was obtained by crushing construction waste concrete with a jaw crusher. The recycled coarse aggregate was soaked in acetic acid for 12 hours, and four kinds of modified recycled aggregates were obtained after different modification processes.
[0034] 1# Recycled coarse aggregate: Soak the recycled coarse aggregate in 1% acetic acid for 16 hours, impregnate it twice with 70g / calcium lactate and 1g / L yeast extract solution under vacuum conditions, and then make the final impregnation with Bacillus pseudofirmus spore suspension; each impregnation time is 5 hours, and after impregnation, put it in a drying oven at 35℃ for 1 day;
[0035] 2# Recycled coarse aggregate: Soak the recycled coarse aggregate in 2% acetic acid for 12 hours, impregnate it twice with 60g / L calcium lactate and 2g / L yeast extract solution under vacuum conditions, and then perform the final impregnation with Bacillus pseudofirmus spore suspension; each impregnation time is 5 hours, and after impregnation, put it in a drying oven at 35℃ and dry it for 1 day;
[0036] 3# Recycled coarse aggregate: Soak the recycled coarse aggregate in 2% acetic acid for 12 hours, impregnate twice with 70g / calcium lactate and 1g / L yeast extract solution under vacuum conditions, and then perform the final impregnation with aerobic Bacillus pseudofirmus spore suspension; each impregnation time is 6 hours, and after impregnation, put it in a drying oven at 35℃ for 2 days;
[0037] 4# Recycled coarse aggregate: Soak the recycled coarse aggregate in 1% acetic acid for 16 hours, impregnate it twice with 70g / calcium lactate and 2g / L yeast extract solution under vacuum conditions, and then make the final impregnation with Bacillus cohnii spore suspension; each impregnation time is 5 hours, and after impregnation, put it in a drying oven at 35℃ and dry it for 1 day.
[0038] There are two types of microorganisms: Bacillus pseudofirmus and Bacillus cohnii.
[0039] The fine aggregate used is dolomite machine-made sand, with a fineness modulus of 3.0, a stone powder content of 4.4%, an MB value of 0.25, a crushing value of 22%, and a moisture content of 1%. The admixture is a naphthalene-based water reducer with a water reduction rate of 20%. The raw materials used in the specific implementation method are all purchased from the market unless otherwise specified.
[0040] The specific embodiment also provides a modified natural coarse aggregate, the lithology is dolomite and limestone, the particle size is 5-10mm, the continuous grading, the needle and flake particle content (mass percentage) is 1.8%, the crushing value is 10%, and the saturated surface dry water absorption rate is 0.9%. The modification process is as follows: soak the recycled coarse aggregate in 1% acetic acid for 16 hours, soak it twice with 70g / calcium lactate and 1g / L yeast extract solution under vacuum conditions, and then soak it with Bacillus pseudofirmus spore suspension for the last time; each soaking time is 5 hours, and after soaking, it is placed in a drying oven at 35°C for 1 day;
[0041] Example 1
[0042] A permeable concrete based on modified recycled aggregate and a preparation method thereof, wherein the preparation steps are as follows:
[0043] 1) Weigh each raw material and mix it evenly in a horizontal mixer to obtain a concrete mixture, wherein the mass parts of each raw material are: 360 parts of 1# low-carbon cementitious material, 1600 parts of 1# modified recycled coarse aggregate, 200 parts of fine aggregate, 110 parts of water, and 18 parts of water reducing agent;
[0044] 2) The obtained permeable concrete mixture is vibrated and pressed into shape, and then placed in a CO2 curing environment for carbonization curing to obtain a permeable concrete product, wherein the carbonization system is: curing temperature 35° C., curing pressure 0.4 MPa, curing time 24 h, CO2 volume concentration 60%, and O2 volume concentration 40%.
[0045] Example 2
[0046] A permeable concrete based on modified recycled aggregate and a preparation method thereof are carried out according to the method in Example 1, except that 2# low-carbon cementitious material is used.
[0047] Example 3
[0048] A permeable concrete based on modified recycled aggregate and a preparation method thereof are carried out according to the method in Example 1, except that the coarse aggregate is 2# modified recycled aggregate.
[0049] Example 4
[0050] A permeable concrete based on modified recycled aggregate and a preparation method thereof are carried out according to the method in Example 1, except that the coarse aggregate is 3# modified recycled aggregate.
[0051] Example 5
[0052] A permeable concrete based on modified recycled aggregate is prepared according to the method in Example 1, except that the coarse aggregate is 4# modified recycled aggregate.
[0053] Example 6
[0054] Example 1 was repeated, except that the concrete mix ratio used was different. The mix ratio of this example was: 410 parts of 1# low-carbon cementitious material, 1400 parts of 1# modified recycled coarse aggregate, 200 parts of fine aggregate, 130 parts of water, and 26 parts of water reducer.
[0055] Example 7
[0056] A permeable concrete based on modified recycled aggregate is prepared according to the method in Example 1, except that the carbonation curing CO2 volume concentration is 30% and the O2 volume concentration is 70%.
[0057] Comparative Example 1
[0058] A permeable concrete of modified recycled aggregate and a preparation method thereof are carried out according to the method in Example 1, except that the low-carbon cementitious material in the raw material is replaced by PO42.5 cement, and there is no carbonization curing process.
[0059] Comparative Example 2
[0060] A permeable concrete of modified recycled aggregate and a preparation method thereof are prepared according to the method in Example 1, except that the recycled aggregate used is not treated with acetic acid.
[0061] Comparative Example 3
[0062] A permeable concrete of modified recycled aggregate and a preparation method thereof are carried out according to the method in Example 1, except that the recycled aggregate used is free of calcium lactate and yeast extraction and microbial modification process.
[0063] Comparative Example 4
[0064] A permeable concrete of modified recycled aggregate and a preparation method thereof are carried out according to the method in Example 1, except that the prepared concrete is placed in an environment with a carbon dioxide concentration of 100% VOL for curing.
[0065] Comparative Example 5
[0066] A permeable concrete of modified recycled aggregate and a preparation method thereof are carried out according to the method in Example 1, except that the microorganism used is Bacillus pasteurianus.
[0067] Comparative Example 6
[0068] A permeable concrete with modified recycled aggregate and a preparation method thereof are carried out according to the method in Example 1, except that the coarse aggregate used is natural coarse aggregate modified by microorganisms.
[0069] Performance testing methods
[0070] The recycled aggregate permeable concrete prepared in Examples 1 to 6 and Comparative Examples 1 to 6 was performance tested in accordance with CJJ / T135-2009 "Technical Specification for Permeable Cement Concrete Pavement" and JTG 3420-2020 "Test Procedure for Cement and Cement Concrete for Highway Engineering". The volume of the specimen used for the internal carbonization depth test was 100 mm × 100 mm × 100 mm. The results are shown in Table 1.
[0071] Table 1 Performance test results of permeable concrete obtained from Examples 1 to 6 and Comparative Examples 1 to 6
[0072]
[0073]
[0074] It can be seen from Table 1 that:
[0075] In Comparative Example 1, ordinary silicate PO42.5 cement is used as the cementitious material. The concrete system is strongly alkaline, which is not conducive to the survival of microorganisms. In addition, there are fewer carbonized active minerals involved, which is not conducive to the formation of CaCO3. Therefore, the overall performance of the permeable concrete is weaker than that of Examples 1-7.
[0076] Since the recycled aggregate in Comparative Example 2 has not been acidified, the surface is alkaline, which is not conducive to the survival of loaded microorganisms, and the CO2 and CaCO3 precipitation inside the concrete is reduced. Therefore, the performance of the obtained permeable concrete is weaker than that of Examples 1-7.
[0077] Since the recycled aggregate in Comparative Example 3 has not undergone a microbial modification process, the strength of the permeable concrete comes from the hydration of the mineral components of the low-carbon cementitious material. The surface strength of the recycled aggregate is poor and the bonding with the cement mineral is weak. Therefore, the performance of the obtained permeable concrete is weaker than that of Examples 1-7.
[0078] In Comparative Example 4, the concentration of carbonized CO2 is 100%, and the microorganisms are aerobic bacterial spores that require oxygen to decompose the substrate to generate CO2 and CaCO3 precipitation. Therefore, the performance of the permeable concrete prepared in Comparative Example 4 is weaker than that of Examples 1-7.
[0079] The microorganisms used in Comparative Example 5 do not have the function of decomposing nutrients to generate CO2 and CaCO3 precipitation, so the performance of the permeable concrete prepared in Comparative Example 5 is weaker than that of Examples 1-7.
[0080] The coarse aggregate used in Comparative Example 6 is modified natural coarse aggregate, which has few surface pores and less carbonizable minerals, less absorbable microorganisms and nutrient substrates, is not conducive to the generation of CO2 and CaCO3 precipitation, and the internal aggregate has weak meshing force with the carbonization product. Therefore, the performance of the permeable concrete prepared in Comparative Example 6 is weaker than that of Examples 1-7.
[0081] The above results show that the recycled aggregate permeable concrete prepared in Examples 1 to 7 has high compressive strength, good carbonization degree and freeze-thaw resistance; the carbonization curing CO2 concentration is low, the low-carbon cementitious material has low carbon emissions, and has important environmental and economic benefits.
[0082] The above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.
Claims
1. Permeable concrete based on modified recycled aggregate, characterized in that The composition is calculated by weight as follows: 260-500 parts of low-carbon cementitious materials, 900-1600 parts of modified recycled coarse aggregate, 50-200 parts of fine aggregate, 90-180 parts of water, and 9-30 parts of water reducer; Wherein, the modified recycled aggregate preparation method comprises the following steps: (1) Mechanically crushing the demolished building materials to remove impurities and obtain 5-10 mm recycled coarse aggregate; (2) the recycled coarse aggregate is soaked or sprayed with an acetic acid aqueous solution; (3) Under vacuum conditions, the mixture is sequentially impregnated with a calcium source solution and a nutrient solution; and finally, the mixture is impregnated with a microbial suspension.
2. The permeable concrete based on modified recycled aggregate according to claim 1, characterized in that The concentration of the acetic acid aqueous solution in step 2 is 1% to 3%, and the treatment time is 12h to 24h.
3. The permeable concrete based on modified recycled aggregate according to claim 1, characterized in that The calcium source solution in step 3 is a calcium lactate solution, or a mixed solution of calcium lactate and calcium formate, with a concentration of 60-80 g / l.
4. The permeable concrete based on modified recycled aggregate according to claim 1, characterized in that The nutrient solution in step 3 is a yeast extract solution or a glucose solution with a concentration of 1 to 3 g / l.
5. The permeable concrete based on modified recycled aggregate according to claim 1, characterized in that The microorganism in step 3 is aerobic Bacillus pseudofirmus or Bacillus cohnii.
6. The permeable concrete based on modified recycled aggregate according to claim 1, characterized in that In step 3, each immersion time is 5 to 8 hours, and drying is required after each immersion.
7. The permeable concrete based on modified recycled aggregate according to claim 1, characterized in that The low-carbon cementitious material is a mixture of low-carbon clinker and mineral powder, the ratio of the low-carbon clinker to the mineral powder is 1:0.25-0.6; the content of CS, C2S and C3S2 in the low-carbon clinker is ≥80%.
8. The permeable concrete based on modified recycled aggregate according to claim 1, characterized in that The fine aggregate has a fineness modulus of 2.1 to 3.2, a stone powder content of ≤17%, and a crushing value of ≤20%.
9. The method for preparing permeable concrete based on modified recycled aggregate according to claim 1, characterized in that The following steps are involved: 1) Mixing the above raw materials uniformly to obtain a permeable concrete mixture; 2) The obtained permeable concrete mixture is vibrated and pressed into shape, and then placed in a CO2 curing environment for carbonization curing to obtain a permeable concrete product.
10. The method for preparing permeable concrete based on modified recycled aggregate according to claim 1, characterized in that The carbonization curing system is: CO2 volume concentration 20-80%, O2 volume concentration 20-80%, curing temperature 20-55°C, curing pressure 0.1-1.0MPa, and curing time 12-48h.
Citation Information
Patent Citations
Microbiological reinforced recycled aggregate and preparation method thereof
CN107601941A
Method for researching influence of bacillus cohnii mineralization deposition on compressive strength of recycled concrete
CN110398538A
Environment-friendly impermeable high-durability concrete and preparation method thereof
CN112551983A
Preparation method of chitosan immobilized microbial urease in-situ reinforced recycled aggregate
CN113307527A
Method for strengthening recycled concrete aggregate multiple times
CN113582570A
Cited By
Degradable slow-release compound fertilizer and preparation method thereof
CN122212851A
High-strength and high-toughness concrete based on full-solid waste functional aggregate, and application and method of antibacterial self-healing in sewage environment
CN122725747A
High-strength and high-toughness concrete based on full-solid waste functional aggregate, and application and method of antibacterial self-healing in sewage environment
CN122725747B