Green low-carbon recycled concrete material as well as preparation method and application thereof
By using volcanic ash active industrial solid waste, alkali triggers and composite modified materials in concrete, high-performance green and low-carbon recycled concrete is formed, which solves the contradiction between high-performance and low-carbon emissions in the existing technology, and achieves efficient carbon sequestration and Improved mechanical properties.
Patent Information
- Application Number
- CN202411264003.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
AI Technical Summary
The lack of high-performance green, low-carbon recycled concrete materials in the prior art makes it difficult to meet the requirements of high-performance and green, low-carbon emissions at the same time.
Using industrial solid waste, alkali triggers, fine aggregates, crude aggregates and composite modified materials with volcanic ash activity, including modified biochar and modified montmorillonite, gelled substances are formed through high-temperature calcination and alkali triggers. , replace cement, improve the mechanical properties of concrete and reduce carbon emissions.
Achieve high-performance concrete materials, while significantly reducing carbon emissions. Through the storage effect of modified biochar and the regulation of modified montmorillonite, compressive strength and acid corrosion resistance are improved, and the requirements of green and low carbon are met. .
Smart Images

Figure CN119038938A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of building materials technology, and in particular relates to a green, low-carbon recycled concrete material and a preparation method and application thereof. Background Art
[0002] The construction industry currently mainly uses cement concrete as a structural building material. Cement concrete includes ingredients such as aggregates, cement binders, and water. However, the production and use of cement concrete will cause a large amount of carbon dioxide emissions. With the development of the economy, the output of cement concrete has also increased, seriously affecting the green and sustainable development of the environment and society.
[0003] In addition to traditional cement binders, some scholars have found that some industrial solid wastes with volcanic ash activity, such as slag, fly ash and other industrial solid wastes, can produce binders under the stimulation of alkali activators to replace cement in traditional concrete to prepare concrete materials. Slag, fly ash and other industrial solid wastes can achieve the purpose of reducing carbon emissions by replacing cement; however, concrete materials as structural building materials have high requirements for mechanical properties. Slag, fly ash and other industrial solid wastes have low reaction activity, which leads to the fact that concrete materials often require high-temperature steam curing and other means to promote the reaction in order to improve their mechanical properties. In addition to improving the curing methods, the mechanical properties can also be improved by improving the raw material formula in concrete, such as increasing the concentration of alkali activators or reducing the particle size of fly ash.
[0004] Although improvements such as high-temperature steam curing of concrete materials, increasing the concentration of alkali activators or reducing the particle size of fly ash can improve the performance of concrete materials and prepare concrete materials with better performance, they cannot reduce carbon emissions very well, which is inconsistent with the purpose of green and low-carbon recycled concrete to reduce carbon emissions. There is currently a lack of high-performance green and low-carbon recycled concrete materials, and further research on concrete materials is needed to meet the requirements of both high performance and green and low-carbon. Summary of the invention
[0005] In view of this, the present application provides a green low-carbon recycled concrete material and a preparation method and application thereof, which are used to solve the technical problem of the lack of high-performance green low-carbon recycled concrete in the prior art.
[0006] The first aspect of the present application provides a green low-carbon recycled concrete material, comprising: industrial solid waste with volcanic ash activity, an alkali activator, fine aggregate, coarse aggregate, and a composite modified material; The composite modified material is selected from modified biochar and modified montmorillonite.
[0007] Preferably, the industrial solid waste with pozzolanic activity is selected from slag and fly ash; The alkaline activator is selected from sodium silicate and tetrasodium 3-hydroxy-2,2′-iminodisuccinate; The fine aggregate is selected from river sand; The coarse aggregate is selected from gravel.
[0008] Preferably, calculated by mass, the green low-carbon recycled concrete material includes 100-300 parts by mass of slag, 200-400 parts by mass of fly ash, 70-100 parts by mass of sodium silicate, 10-30 parts by mass of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, 500-600 parts by mass of river sand, 900-1200 parts by mass of gravel, 100-200 parts by mass of modified biochar, 100-200 parts by mass of modified montmorillonite and 200-300 parts by mass of water.
[0009] Preferably, the sodium silicate includes 4 to 10 parts by mass of Na 2 O·SiO 2 and 60~70 parts by mass of Na 2 O·2SiO 2 .
[0010] The second aspect of the present application provides a method for preparing a green low-carbon recycled concrete material, the preparation method comprising the steps of: Step S1, mixing industrial solid waste with volcanic ash activity, fine aggregate, coarse aggregate and modified montmorillonite in the composite modified material and calcining at high temperature to obtain calcined clinker; Step S2, mixing the calcined clinker, the modified biochar in the composite modified material and the alkali activator evenly to obtain a green low-carbon recycled concrete material precursor; Step S3: Evenly mix the green low-carbon recycled concrete material precursor and water, and cast to obtain the green low-carbon recycled concrete material.
[0011] Preferably, in step S1, the method for preparing the modified montmorillonite comprises: Step A1, soaking montmorillonite with a hydrochloric acid solution and then drying to obtain montmorillonite treated with an acid reagent; Step A2, mixing the montmorillonite treated with an acid reagent and the composite modified liquid to obtain modified montmorillonite; The composite modified liquid is selected from a mixed solution of ammonium monohydrogen phosphate and tetradecyltrimethylammonium bromide.
[0012] Preferably, the method for preparing the modified biochar comprises: Step B1, crushing the agricultural and forestry biomass to obtain agricultural and forestry biomass powder; Step B2, soaking the agricultural and forestry biomass powder with a sodium hydroxide solution and then drying it to obtain the agricultural and forestry biomass treated with an alkaline reagent; Step B3, soaking the agricultural and forestry biomass treated with the alkaline reagent with a ferric nitrate solution and then drying to obtain modified agricultural and forestry biomass; Step B4: pyrolyzing the modified agricultural and forestry biomass to obtain modified biochar.
[0013] Preferably, the agricultural and forestry biomass is selected from agricultural and forestry wastes and / or agricultural and forestry crops.
[0014] Preferably, the agricultural and forestry waste is selected from straw, fruit peel, rice husk, tree bark or peanut shell.
[0015] Preferably, the agricultural and forestry crops are selected from sisal, flax, trees or shrubs.
[0016] Preferably, in step S1, the high temperature calcination is carried out at a temperature of 1000-1200° C. for a time of 3-4 hours.
[0017] Preferably, in step S2, the uniform mixing is performed by stirring for 3 to 4 minutes.
[0018] Preferably, in step S3, the uniform mixing method is stirring for 3 to 4 minutes, and the pouring time is 1 to 30 minutes.
[0019] The third aspect of the present application provides an application of a green and low-carbon recycled concrete material in engineering construction.
[0020] In summary, the present application provides a green and low-carbon recycled concrete material, a preparation method and application thereof. The green and low-carbon recycled concrete material provided by the present application includes industrial solid waste with volcanic ash activity, an alkali activator, fine aggregate, coarse aggregate and a composite modified material; the cementitious material produced by the industrial solid waste with volcanic ash activity under the stimulation of the alkali activator can replace cement, firmly bond the fine aggregate and the coarse aggregate together to obtain a concrete material and reduce carbon emissions, and the composite modified material composed of modified montmorillonite and biochar can improve the mechanical properties of the concrete material, and at the same time, the biochar can seal carbon into the concrete to further reduce carbon emissions, thereby solving the technical problem of the lack of high-performance green and low-carbon recycled concrete in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0022] Figure 1 The gradation distribution diagram of slag and fly ash provided in Example 1 of the present application; Figure 2 X-ray diffraction patterns of slag and fly ash provided in Example 1 of the present application; Figure 3 This is a test result diagram of the slump of the green low-carbon recycled concrete material provided in Example 2, Example 6, Example 7 and Example 1 of the present application; Figure 4 A schematic diagram of the preparation process of the green low-carbon recycled concrete material provided in the embodiment of the present application; Figure 1 and 2 In the table, slag means slag and Fly ash means fly ash. DETAILED DESCRIPTION
[0023] The present application provides a green low-carbon recycled concrete material and a preparation method and application thereof, which are used to solve the technical problem of the lack of high-performance green low-carbon recycled concrete in the prior art.
[0024] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0025] In view of the current lack of high-performance green and low-carbon recycled concrete materials, the present application provides a green and low-carbon recycled concrete material. The raw material composition of the green and low-carbon recycled concrete material provided by the present application includes industrial solid waste with volcanic ash activity, alkali activator, fine aggregate, coarse aggregate and composite modified material; in the raw material composition, the cementitious material produced by the industrial solid waste with volcanic ash activity under the stimulation of the alkali activator can replace cement, and the fine aggregate and the coarse aggregate are firmly bonded together to obtain a concrete material. At the same time, the industrial solid waste with volcanic ash activity is used as a renewable resource to replace cement to reduce carbon emissions. The prepared concrete material is a green and low-carbon emission renewable concrete material; In addition, the modified biochar in the composite modified material is obtained by pyrolysis of agricultural and forestry biomass, which is rich in plant fiber components. The amorphous silicon of plant fiber gradually transforms into a crystalline state during high-temperature pyrolysis, and the biochar formed by pyrolysis is more stable. Experimental results show that adding it to concrete can enhance the compressive strength and other mechanical properties of concrete materials. At the same time, the modified montmorillonite in the composite modified material can also regulate the hydration process of the cementitious material in the concrete material, improve the defect of concrete's later strength shrinkage, and improve the mechanical strength of the concrete material. In addition to improving the compressive strength and other mechanical properties, adding modified biochar to the concrete material can also seal carbon into the concrete in the form of biochar to reduce carbon emissions. Since the life of concrete can reach 100 years, these carbons will form carbon sinks for a long time and will no longer exchange carbon with the carbon source, so they can be sealed for a long time, thereby effectively reducing carbon emissions and meeting the purpose of reducing carbon emissions. This enables the green and low-carbon recycled concrete material provided by the present application to meet the requirements of both high performance and green and low carbon, thereby overcoming the current lack of high-performance green and low-carbon recycled concrete materials.
[0026] Preferably, in the green and low-carbon recycled concrete material provided in the present application, the industrial solid waste with volcanic ash activity is selected from slag and fly ash with better activity; and the alkali activator is selected from a composite alkali activator of sodium silicate and tetrasodium 3-hydroxy-2,2′-iminodisuccinate.
[0027] At the same time, in the green and low-carbon recycled concrete material provided by this application, the fine aggregate is selected from river sand, and the coarse aggregate is selected from gravel; river sand and gravel are traditional concrete aggregates with good performance.
[0028] As a preference, due to the porous structure of the modified biochar in the composite modified material, excessive doping can easily lead to a decrease in the density of the concrete material. At the same time, too much modified biochar may also agglomerate, thereby reducing the splitting tensile strength and toughness of the concrete material. In addition, the ratio of water to slag, fly ash, sodium silicate, tetrasodium 3-hydroxy-2,2′-iminodisuccinate, modified biochar, modified montmorillonite and other raw materials will also affect the workability of the concrete material. Therefore, in the green and low-carbon recycled concrete material provided by the present application, green Specific improvements have been made to the amount of raw materials in the low-carbon recycled concrete materials. The green low-carbon recycled concrete materials provided include 100~300 parts by mass of slag, 200~400 parts by mass of fly ash, 70~100 parts by mass of sodium silicate, 10~30 parts by mass of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, 500~600 parts by mass of river sand, 900~1200 parts by mass of gravel, 100~200 parts by mass of modified biochar, 100~200 parts by mass of modified montmorillonite and 200-300 parts by mass of water.
[0029] The green and low-carbon recycled concrete material provided by this application will be specifically described below in combination with embodiments and experimental examples.
[0030] Example 1 Example 1 of the present application provides a method for preparing a green and low-carbon recycled concrete material, the preparation method comprising the steps of preparing clinker, preparing a precursor, and a volcanic ash reaction.
[0031] The steps of preparing clinker include: 25 kg of fly ash, 12.5 kg of slag, 11.25 kg of modified montmorillonite, 42 kg of river sand and 77.4 kg of gravel were mixed and calcined at 1100° C. for 3 hours to obtain calcined clinker.
[0032] The steps of preparing the precursor include: The obtained cement clinker was mixed with 7.5 kg modified biochar and 0.4 kg activator A (sodium silicate with modulus 1, Na 2 O·SiO 2 )、6.5kg activator B (modulus 2 sodium silicate, Na 2 O·2SiO 2 ), 1.3 kg of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, poured into a mixer and stirred for 3 minutes to obtain a green and low-carbon recycled concrete material precursor.
[0033] The steps of the pozzolanic reaction include: Then, 20 kg of water was added to the green low-carbon recycled concrete material precursor and stirred for 3 minutes using a mixer. The green low-carbon recycled concrete material was poured out of the pot, and the pouring, vibrating and leveling were completed within 30 minutes to obtain the green low-carbon recycled concrete material.
[0034] In this embodiment, the preparation process of the modified biochar used includes: washing, drying and then crushing 10 kg of sisal to obtain fiber powder; immersing the 10 kg of fiber powder in 50 kg of 1 mol / L sodium hydroxide solution for 0.5 h, taking out and drying; immersing the treated fiber powder in 70 kg of 0.5 mol / L ferric nitrate solution for 1 h, drying it and placing it in an oxygen-free environment at 900 ° C for 4 h, and grinding it to obtain modified biochar with a particle size of 50-100 μm.
[0035] The preparation process of the modified montmorillonite used includes: immersing 14 kg of montmorillonite in 40 kg of hydrochloric acid solution with a concentration of 0.5 mol / L for 1 hour, taking out and drying; mixing the treated montmorillonite with 16 kg of saturated ammonium monohydrogen phosphate solution and 24 kg of saturated tetradecyltrimethylammonium bromide solution for 2 hours to obtain the modified montmorillonite; the solubility of ammonium monohydrogen phosphate is 58 g / 100 mL, and the solubility of tetradecyltrimethylammonium bromide is 20 g / 100 mL.
[0036] The composition of slag and fly ash used is shown in Table 1, and the gradation distribution diagram is shown in Figure 1 The X-ray diffraction pattern is shown in Figure 2 shown.
[0037]
[0038] Table 1
[0039] Example 2 Example 2 of the present application provides a method for preparing a green and low-carbon recycled concrete material, the preparation method comprising the steps of preparing clinker, preparing a precursor, and a volcanic ash reaction.
[0040] The steps of preparing clinker include: 22.5 kg of fly ash, 12 kg of slag, 11.5 kg of modified montmorillonite, 37.5 g of river sand and 67.5 kg of gravel were mixed and calcined at 1000° C. for 3 hours to obtain calcined clinker.
[0041] The steps of preparing the precursor include: The obtained clinker was mixed with 7.5 kg modified biochar, 0.4 kg activator A (modulus 1 sodium silicate, Na 2 O·SiO 2 )、7kg activator B (modulus 2 sodium silicate, Na 2 O·2SiO 2 ), 1.5kg of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, poured into a mixer and stirred for 3 minutes to obtain a green and low-carbon recycled concrete material precursor.
[0042] The steps of the pozzolanic reaction include: Then, 15 kg of water was added to the green low-carbon recycled concrete material precursor and stirred for 3 minutes using a mixer. The green low-carbon recycled concrete material was poured out of the pot, and the pouring, vibrating and leveling were completed within 30 minutes to obtain the green low-carbon recycled concrete material.
[0043] In this embodiment, the preparation process of the modified biochar used includes: washing, drying and then crushing 10 kg of sisal to obtain fiber powder; immersing the 10 kg of fiber powder in 50 kg of 3 mol / L sodium hydroxide solution for 0.25 h, taking out and drying; immersing the treated fiber powder in 70 kg of 1 mol / L ferric nitrate solution for 1.5 h, drying and placing it in an oxygen-free environment at 1000°C for slow pyrolysis for 4 h, and grinding to obtain modified biochar with a particle size of 50-100 μm.
[0044] Example 3 Example 3 of the present application provides a method for preparing a green and low-carbon recycled concrete material, the preparation method comprising the steps of preparing clinker, preparing a precursor, and a volcanic ash reaction.
[0045] The steps of preparing clinker include: 30 kg of fly ash, 15 kg of slag, 15 kg of modified montmorillonite, 45 g of river sand and 90 kg of gravel were mixed and calcined at 1200° C. for 4 hours to obtain calcined clinker.
[0046] The steps of preparing the precursor include: The obtained clinker was mixed with 10 kg modified biochar, 0.4 kg activator A (sodium silicate with modulus 1, Na 2 O·SiO 2 )、7kg activator B (modulus 2 sodium silicate, Na 2 O·2SiO 2 ), 2.25kg of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, poured into a mixer and stirred for 3 minutes to obtain a green and low-carbon recycled concrete material precursor.
[0047] The steps of the pozzolanic reaction include: Then, 22 kg of water was added to the green low-carbon recycled concrete material precursor and stirred in a mixer for 3 minutes. The green low-carbon recycled concrete material was poured out of the pot, and the pouring, vibrating and leveling were completed within 30 minutes to obtain the green low-carbon recycled concrete material.
[0048] In this embodiment, the preparation process of the modified biochar used includes: washing, drying and then crushing 15 kg of sisal to obtain fiber powder; immersing the 15 kg of fiber powder in 50 kg of 3 mol / L sodium hydroxide solution for 0.5 h, taking out and drying; immersing the treated fiber powder in 70 kg of 1 mol / L ferric nitrate solution for 1.5 h, drying and placing it in an oxygen-free environment at 1200°C for slow pyrolysis for 4 h, and grinding to obtain modified biochar with a particle size of 50-100 μm.
[0049] The preparation process of the modified montmorillonite used includes: immersing 20 kg of montmorillonite in 40 kg of 1 mol / L hydrochloric acid solution for 0.5 h, taking it out and drying it; mixing the treated montmorillonite with 18 kg of ammonium monohydrogen phosphate solution and 27 kg of tetradecyltrimethylammonium bromide solution, and stirring for 3 h to obtain the modified montmorillonite.
[0050] The slag and fly ash used are consistent with those in Example 1.
[0051] Example 4 Example 4 of the present application provides a method for preparing a green and low-carbon recycled concrete material, the preparation method comprising the steps of preparing clinker, preparing a precursor, and a volcanic ash reaction.
[0052] The steps of preparing clinker include: 22.5 kg of fly ash, 13.5 kg of slag, 13.5 kg of modified montmorillonite, 37.5 g of river sand and 67.5 kg of gravel were mixed and calcined at 1000° C. for 3 hours to obtain calcined clinker.
[0053] The steps of preparing the precursor include: The obtained clinker was mixed with 7.5 kg modified biochar, 0.4 kg activator A (modulus 1 sodium silicate, Na 2 O·SiO 2 )、7kg activator B (modulus 2 sodium silicate, Na 2 O·2SiO 2 ), 1.5kg of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, poured into a mixer and stirred for 3 minutes to obtain a green and low-carbon recycled concrete material precursor.
[0054] The steps of the pozzolanic reaction include: Then, 15 kg of water was added to the green low-carbon recycled concrete material precursor and stirred for 3 minutes using a mixer. The green low-carbon recycled concrete material was poured out of the pot, and the pouring, vibrating and leveling were completed within 30 minutes to obtain the green low-carbon recycled concrete material.
[0055] In this embodiment, the preparation process of the modified biochar used includes: washing, drying and then crushing 10 kg of sisal to obtain fiber powder; immersing the 10 kg of fiber powder in 50 kg of 3 mol / L sodium hydroxide solution for 0.25 h, taking out and drying; immersing the treated fiber powder in 70 kg of 1 mol / L ferric nitrate solution for 1.5 h, drying and placing it in an oxygen-free environment at 1000°C for slow pyrolysis for 4 h, and grinding to obtain modified biochar with a particle size of 50-100 μm.
[0056] The preparation process of the modified montmorillonite used includes: immersing 15 kg of montmorillonite in 40 kg of 1 mol / L hydrochloric acid solution for 0.5 h, taking it out and drying it; mixing the treated montmorillonite with 16 kg of ammonium monohydrogen phosphate solution and 24 kg of tetradecyltrimethylammonium bromide solution, and stirring for 3 h to obtain the modified montmorillonite.
[0057] The slag and fly ash used are consistent with those in Example 1.
[0058] Example 5 Example 5 of the present application provides a method for preparing a green and low-carbon recycled concrete material, the preparation method comprising the steps of preparing clinker, preparing a precursor, and a volcanic ash reaction.
[0059] The steps of preparing clinker include: 22.5 kg of fly ash, 22.5 kg of slag, 11.25 kg of modified montmorillonite, 40 g of river sand and 80 kg of gravel were mixed and calcined at 1000° C. for 3 h to obtain calcined clinker.
[0060] The steps of preparing the precursor include: The obtained cement clinker was mixed with 7.5 kg modified biochar and 0.4 kg activator A (sodium silicate with modulus 1, Na 2 O·SiO 2 )、7kg activator B (modulus 2 sodium silicate, Na 2 O·2SiO 2 ), 1.5kg of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, poured into a mixer and stirred for 3 minutes to obtain a green and low-carbon recycled concrete material precursor.
[0061] The steps of the pozzolanic reaction include: Then, 15 kg of water was added to the green low-carbon recycled concrete material precursor and stirred for 3 minutes using a mixer. The green low-carbon recycled concrete material was poured out of the pot, and the pouring, vibrating and leveling were completed within 30 minutes to obtain the green low-carbon recycled concrete material.
[0062] In this embodiment, the preparation process of the modified biochar used includes: washing, drying and then crushing 10 kg of sisal to obtain fiber powder; immersing the 10 kg of fiber powder in 50 kg of 3 mol / L sodium hydroxide solution for 0.25 h, taking out and drying; immersing the treated fiber powder in 70 kg of 1 mol / L ferric nitrate solution for 1.5 h, drying and placing it in an oxygen-free environment at 1000°C for slow pyrolysis for 4 h, and grinding to obtain modified biochar with a particle size of 50-100 μm.
[0063] The preparation process of the modified montmorillonite used includes: immersing 20 kg of montmorillonite in 40 kg of 1 mol / L hydrochloric acid solution for 0.5 h, taking it out and drying it; mixing the treated montmorillonite with 16 kg of ammonium monohydrogen phosphate solution and 24 kg of tetradecyltrimethylammonium bromide solution, and stirring for 3 h to obtain the modified montmorillonite.
[0064] The slag and fly ash used are consistent with those in Example 1.
[0065] Example 6 Example 6 of the present application provides a method for preparing a green and low-carbon recycled concrete material, the preparation method comprising the steps of preparing clinker, preparing a precursor, and a volcanic ash reaction.
[0066] The steps of preparing clinker include: 24.5 kg of fly ash, 14 kg of slag, 15 kg of modified montmorillonite, 42 kg of river sand and 77.4 kg of gravel were mixed and calcined at 1100° C. for 3 hours to obtain calcined clinker.
[0067] The steps of preparing the precursor include: The obtained clinker was mixed with 7.5 kg modified biochar, 0.4 kg activator A (modulus 1 sodium silicate, Na 2 O·SiO 2 )、6.5kg activator B (modulus 2 sodium silicate, Na 2 O·2SiO 2 ), 1.3 kg of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, poured into a mixer and stirred for 3 minutes to obtain a green and low-carbon recycled concrete material precursor.
[0068] The steps of the pozzolanic reaction include: Then, 18 kg of water was added to the green low-carbon recycled concrete material precursor and stirred for 3 minutes using a mixer. The green low-carbon recycled concrete material was poured out of the pot, and the pouring, vibrating and leveling were completed within 30 minutes to obtain the green low-carbon recycled concrete material.
[0069] In this embodiment, the preparation process of the modified biochar used includes: washing, drying and then crushing 10 kg of sisal to obtain fiber powder; immersing the 10 kg of fiber powder in 50 kg of 3 mol / L sodium hydroxide solution for 0.5 h, taking out and drying; immersing the treated fiber powder in 70 kg of 0.5 mol / L ferric nitrate solution for 1 h, drying and placing it in an oxygen-free environment at 900 ° C for 4 h, and grinding to obtain modified biochar with a particle size of 50-100 μm.
[0070] The preparation process of the modified montmorillonite used includes: immersing 20 kg of montmorillonite in 40 kg of 1 mol / L hydrochloric acid solution for 0.5 h, taking it out and drying it; mixing the treated montmorillonite with 16 kg of ammonium dihydrogen phosphate solution and 24 kg of tetradecyltrimethylammonium bromide solution, and stirring for 2 h to obtain the modified montmorillonite.
[0071] The slag and fly ash used are consistent with those in Example 1.
[0072] Example 7 Example 7 of the present application provides a method for preparing a green and low-carbon recycled concrete material, the preparation method comprising the steps of preparing clinker, preparing a precursor, and a volcanic ash reaction.
[0073] The steps of preparing clinker include: 22.5 kg of fly ash, 22.5 kg of slag, 11.25 kg of modified montmorillonite, 42 kg of river sand and 77.4 kg of gravel were mixed and calcined at 1100° C. for 3 hours to obtain calcined clinker.
[0074] The steps of preparing the precursor include: The obtained clinker was mixed with 7.5 kg modified biochar, 0.4 kg activator A (modulus 1 sodium silicate, Na 2 O·SiO 2 )、6.5kg activator B (modulus 2 sodium silicate, Na 2 O·2SiO 2 ), 1.3 kg of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, poured into a mixer and stirred for 3 minutes to obtain a green and low-carbon recycled concrete material precursor.
[0075] The steps of the pozzolanic reaction include: Then, 19.7 kg of water was added to the green low-carbon recycled concrete material precursor and stirred for 3 minutes using a mixer. The green low-carbon recycled concrete material was poured out of the pot, and the pouring, vibrating and leveling were completed within 30 minutes to obtain the green low-carbon recycled concrete material.
[0076] In this embodiment, the preparation process of the modified biochar used includes: washing, drying and then crushing 10 kg of sisal to obtain fiber powder; immersing the 10 kg of fiber powder in 50 kg of 1 mol / L sodium hydroxide solution for 0.5 h, taking out and drying; immersing the treated fiber powder in 70 kg of 0.5 mol / L ferric nitrate solution for 1 h, drying it and placing it in an oxygen-free environment at 900 ° C for 4 h, and grinding it to obtain modified biochar with a particle size of 50-100 μm.
[0077] The preparation process of the modified montmorillonite used includes: immersing 14 kg of montmorillonite in 40 kg of 1 mol / L hydrochloric acid solution for 0.5 h, taking it out and drying it; mixing the treated montmorillonite with 16 kg of ammonium monohydrogen phosphate solution and 24 kg of tetradecyltrimethylammonium bromide solution, and stirring for 2 h to obtain the modified montmorillonite.
[0078] The slag and fly ash used are consistent with those in Example 1.
[0079] Example 8 Example 8 of the present application provides a method for preparing a concrete material. As a comparison with Example 1, the preparation method includes the steps of preparing clinker, preparing a precursor, and a pozzolanic reaction. The steps of preparing clinker include: 25 kg of fly ash, 12.5 kg of slag, 11.25 kg of modified montmorillonite, 42 kg of river sand and 77.4 kg of gravel were mixed and calcined at 1100° C. for 3 hours to obtain calcined clinker.
[0080] The steps of preparing the precursor include: The prepared cement clinker was mixed with 0.4 kg of activator A (modulus 1 sodium silicate, Na 2 O·SiO 2 )、6.5kg activator B (modulus 2 sodium silicate, Na 2 O·2SiO 2 ), 1.3 kg of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, were poured into a mixer and stirred for 3 minutes to obtain a concrete material precursor.
[0081] The steps of the pozzolanic reaction include: Then, 20 kg of water was added to the concrete material precursor and stirred for 3 minutes using a mixer. The concrete material was poured out of the pot and poured, vibrated and smoothed within 30 minutes to obtain the concrete material.
[0082] In this embodiment, the preparation process of the modified montmorillonite used includes: immersing 14 kg of montmorillonite in 40 kg of 0.5 mol / L hydrochloric acid solution for 1 hour, taking out and drying; mixing the treated montmorillonite with 16 kg of ammonium monohydrogen phosphate solution and 24 kg of tetradecyltrimethylammonium bromide solution, and stirring for 2 hours to obtain the modified montmorillonite.
[0083] The slag and fly ash used are consistent with those in Example 1.
[0084] Example 9 Example 9 of the present application provides a method for preparing a concrete material. As a comparison with Example 1, the preparation method includes the steps of preparing clinker, preparing a precursor, and conducting a pozzolanic reaction.
[0085] The steps of preparing clinker include: 25 kg of fly ash, 12.5 kg of slag, 42 kg of river sand and 77.4 kg of gravel were mixed and calcined at 1100°C for 3 hours to obtain calcined clinker.
[0086] The steps of preparing the precursor include: The obtained cement clinker was mixed with 7.5 kg modified biochar and 0.4 kg activator A (sodium silicate with modulus 1, Na 2 O·SiO 2)、6.5kg activator B (modulus 2 sodium silicate, Na 2 O·2SiO 2 ), 1.3 kg of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, were poured into a mixer and stirred for 3 minutes to obtain a concrete material precursor.
[0087] The steps of the pozzolanic reaction include: Then, 20 kg of water was added to the concrete material precursor and stirred for 3 minutes using a mixer. The concrete material was poured out of the pot, and the pouring, vibrating and leveling were completed within 30 minutes to obtain the concrete material.
[0088] In this embodiment, the preparation process of the modified biochar used includes: washing, drying and then crushing 10 kg of sisal to obtain fiber powder; immersing the 10 kg of fiber powder in 50 kg of 1 mol / L sodium hydroxide solution for 0.5 h, taking out and drying; immersing the treated fiber powder in 70 kg of 0.5 mol / L ferric nitrate solution for 1 h, drying it and placing it in an oxygen-free environment at 900 ° C for 4 h, and grinding it to obtain modified biochar with a particle size of 50-100 μm.
[0089] The slag and fly ash used are consistent with those in Example 1.
[0090] Example 10 Example 10 of the present application provides a method for preparing a concrete material. As a comparison with Example 1, the preparation method includes the steps of preparing clinker, preparing a precursor, and conducting a pozzolanic reaction.
[0091] The steps of preparing clinker include: 25 kg of fly ash, 12.5 kg of slag, 42 kg of river sand and 77.4 kg of gravel were mixed and calcined at 1100°C for 3 hours to obtain calcined clinker.
[0092] The steps of preparing the precursor include: The prepared cement clinker was mixed with 0.4 kg of activator A (modulus 1 sodium silicate, Na 2 O·SiO 2 )、6.5kg activator B (modulus 2 sodium silicate, Na 2 O·2SiO 2 ), 1.3 kg of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, were poured into a mixer and stirred for 3 minutes to obtain a concrete material precursor.
[0093] The steps of the pozzolanic reaction include: Then, 20 kg of water was added to the concrete material precursor and stirred for 3 minutes using a mixer. The concrete material was poured out of the pot and poured, vibrated and smoothed within 30 minutes to obtain the concrete material.
[0094] The slag and fly ash used are consistent with those in Example 1.
[0095] Experimental Example 1 Experimental Example 1 of the present application performs performance tests on the concrete materials provided in Examples 1-7 and Examples 8-10 as comparative examples of Example 1.
[0096] The compositions of slag and fly ash used in Examples 1-10 are shown in Table 1, and the gradation distribution diagram is shown in Figure 1 The X-ray diffraction pattern is shown in Figure 2 As shown in Table 1, Figure 1~2 It can be seen that the crystal composition of slag and fly ash is similar, and both contain more SiO 2 、Al 2 O 3 The volcanic ash has high activity and is conducive to producing more cementitious substances under the stimulation of alkali activators, thereby improving the strength of concrete materials. Half of the slag particles have a particle size less than 8.68 microns, and 90% of the particles have a particle size less than 24.1 microns. Half of the fly ash particles have a particle size less than 14.5 microns, and 90% of the particles have a particle size less than 58.9 microns. The particle sizes of slag and fly ash are small, and the specific surface area is large, which is conducive to the volcanic ash reaction.
[0097] The slump of the green low-carbon recycled concrete material provided in Example 2, Example 6, Example 7 and Example 1, including different proportions of water and slag, fly ash, sodium silicate, tetrasodium 3-hydroxy-2,2′-iminodisuccinate, modified biochar, modified montmorillonite and other raw materials, is as follows: Figure 3 As shown, from Figure 3 It can be seen that the green low-carbon recycled concrete material provided in the embodiment of the present application has a slump between 90 mm and 140 mm, and has good workability, indicating that the green low-carbon recycled concrete material provided in the present application has good cohesiveness and water retention, and is easy to carry out construction operations such as pouring.
[0098] Experimental Example 2 Experimental Example 2 of the present application performs performance tests on the concrete materials provided in Examples 1-7 and Examples 8-10 as comparative examples of Example 1.
[0099] Among them, the test results of the compressive strength of the concrete materials provided by Examples 8-10 of the green low-carbon recycled concrete materials provided by Examples 1-7 are shown in Table 2.
[0100]
[0101] Table 2 As can be seen from Table 2, the compressive strength of the concrete material provided by Example 8 in which modified biochar is not added to the raw materials is 25.1 MPa, the compressive strength of the concrete material provided by Example 9 in which modified montmorillonite is not added to the raw materials is 24.1 MPa, and the compressive strength of the concrete material provided by Example 10 in which modified biochar and montmorillonite are not added to the raw materials is 20.1 MPa. The average compressive strength of the green and low-carbon recycled concrete materials provided by Examples 1-7 in which modified biochar and montmorillonite are added is 34.8 MPa, which is more than 38% higher than the concrete material without modified biochar / modified montmorillonite. This shows that the green and low-carbon recycled concrete material provided in the present application can enhance the compressive strength of the concrete material by doping with concrete, and doping with modified montmorillonite also improves the defect of concrete's later strength shrinkage, thereby increasing the compressive strength by more than 38%.
[0102] Compared with the concrete materials provided in Examples 8-10, the green and low-carbon recycled concrete materials provided in Examples 1-7 have better anti-carbonation performance. At the same time, compared with ordinary cement concrete, the green and low-carbon recycled concrete materials provided in Examples 1-7 have a large amount of Al-O and Si-O structures formed by the volcanic ash reaction, which makes the green and low-carbon recycled concrete materials provided in this application have better acid corrosion resistance.
[0103] Experimental Example 3 Experimental Example 3 of the present application evaluates the environmental friendliness of the green low-carbon recycled concrete material and ordinary cement concrete provided in Example 1.
[0104] Environmental assessment based on CO 2 Total emissions are calculated, including the CO2 emissions of green low-carbon recycled concrete materials and ordinary cement concrete. 2 The total emissions are calculated as shown in Formula I.
[0105] Formula I.
[0106] In formula I, Q is the amount of fuel consumed to carry out the activity (kg), EC is the energy content of the fuel used to carry out the activity (J / kg), and GWP is the global warming potential of the fuel (kg CO 2 -e / J), EC × GWP is CO 2 Emission factor (kg CO 2 -e / kg).
[0107] Among them, the CO2 content of raw materials in green low-carbon recycled concrete materials and ordinary cement concrete is 2 The emission factors are shown in Table 3.
[0108]
[0109] Table 3 Taking ordinary cement concrete and the green low-carbon recycled concrete material provided in Example 1 as examples, the raw material composition of ordinary cement concrete is shown in Table 4.
[0110]
[0111] Table 4 As can be seen from Table 3, the CO 2 The emission factor is extremely large, at 0.82. However, this application uses slag, fly ash and other industrial solid wastes with volcanic ash activity to replace cement. 2 The emission factors are reduced to 0.019 and 0.009, indicating that the green low-carbon recycled concrete provided by this application can reduce CO 2 The total amount of emissions is discharged to a lower level. Through calculation, it can be known that the green low-carbon recycled concrete provided by the embodiment of the present application is CO2-free compared with ordinary concrete. 2 The total emissions have been reduced by more than 40%, which has a significant environmental impact.
[0112] Through the performance test of the green low-carbon recycled concrete material and concrete material provided in Examples 1-10 of the present application, it can be found that the green low-carbon recycled concrete material provided in the embodiments of the present application has good workability and is easy to perform construction operations such as pouring. At the same time, by adding a certain amount of modified montmorillonite and biochar, the compressive strength, carbonization resistance and acid corrosion resistance of the green low-carbon recycled concrete material can be improved; and due to the use of low CO 2 Slag, fly ash and other industrial solid wastes with volcanic ash activity can replace high CO 2 The cement with a low emission factor can significantly reduce the total carbon emissions. The green and low-carbon recycled concrete material provided in this application can meet the requirements of high performance and green and low-carbon at the same time.
[0113] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A green low-carbon recycled concrete material, characterized in that: include: Industrial solid waste with pozzolanic activity, alkali activators, fine aggregates, coarse aggregates and composite modified materials; The composite modified material is selected from modified biochar and modified montmorillonite.
2. A green low-carbon recycled concrete material according to claim 1, characterized in that: The industrial solid waste with pozzolanic activity is selected from slag and fly ash; The alkaline activator is selected from sodium silicate and tetrasodium 3-hydroxy-2,2′-iminodisuccinate; The fine aggregate is selected from river sand; The coarse aggregate is selected from gravel.
3. The green low-carbon recycled concrete material according to claim 2, characterized in that: Calculated in parts by mass, the green and low-carbon recycled concrete material includes 100-300 parts by mass of slag, 200-400 parts by mass of fly ash, 70-100 parts by mass of sodium silicate, 10-30 parts by mass of tetrasodium 3-hydroxy-2,2′-iminodisuccinate, 500-600 parts by mass of river sand, 900-1200 parts by mass of gravel, 100-200 parts by mass of modified biochar, 100-200 parts by mass of modified montmorillonite and 200-300 parts by mass of water.
4. The green low-carbon recycled concrete material according to claim 3, characterized in that: The sodium silicate comprises 4-10 parts by mass of Na2O·SiO2 and 60-70 parts by mass of Na2O·2SiO2.
5. The method for preparing a green low-carbon recycled concrete material according to any one of claims 1 to 4, characterized in that: Includes steps: Step S1, mixing industrial solid waste with volcanic ash activity, fine aggregate, coarse aggregate and modified montmorillonite in the composite modified material and calcining at high temperature to obtain calcined clinker; Step S2, mixing the calcined clinker, the modified biochar in the composite modified material and the alkali activator evenly to obtain a green low-carbon recycled concrete material precursor; Step S3: Evenly mix the green low-carbon recycled concrete material precursor and water, and cast to obtain the green low-carbon recycled concrete material.
6. The method for preparing a green low-carbon recycled concrete material according to claim 5, characterized in that: In step S1, the preparation method of the modified montmorillonite comprises: Step A1, soaking montmorillonite with a hydrochloric acid solution and then drying to obtain montmorillonite treated with an acid reagent; Step A2, mixing the montmorillonite treated with an acid reagent and the composite modified liquid to obtain modified montmorillonite; The composite modified liquid is selected from a mixed solution of ammonium monohydrogen phosphate and tetradecyltrimethylammonium bromide.
7. The method for preparing a green low-carbon recycled concrete material according to claim 5, wherein The characteristic is that In step S2, the method for preparing modified biochar comprises: Step B1, crushing the agricultural and forestry biomass to obtain agricultural and forestry biomass powder; Step B2, soaking the agricultural and forestry biomass powder with a sodium hydroxide solution and then drying it to obtain the agricultural and forestry biomass treated with an alkaline reagent; Step B3, soaking the agricultural and forestry biomass treated with the alkaline reagent with a ferric nitrate solution and then drying to obtain modified agricultural and forestry biomass; Step B4: pyrolyzing the modified agricultural and forestry biomass to obtain modified biochar.
8. The method for preparing a green and low-carbon recycled concrete material according to claim 7, characterized in that: The agricultural and forestry biomass is selected from agricultural and forestry wastes and / or agricultural and forestry crops.
9. The method for preparing a green and low-carbon recycled concrete material according to claim 7, characterized in that: The agricultural and forestry waste is selected from straw, fruit peel, rice husk, tree bark or peanut shell.
10. Application of the green, low-carbon recycled concrete material according to any one of claims 1 to 4 in engineering construction.
Citation Information
Cited By
Fiber-reinforced building solid waste recycled aggregate concrete and preparation method thereof
CN119430781A