Carbon-carbon crucible for melting siliconizing of carbon-ceramic brake disc and preparation method of carbon-carbon crucible

By adopting alternating laying and three-dimensional needle-punching knitting technology in carbon-carbon crucibles, combined with CVI and graphitization treatment, the problems of uneven density and short life of carbon-carbon crucibles are solved, and high-performance and low-cost carbon ceramic brake discs are realized Production.

CN119039031APending Publication Date: 2024-11-29SHANDONG STOP ART BRAKING MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411215421.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing carbon-carbon crucibles have short service life, uneven density and poor thermal conductivity in ultra-high temperature environments, resulting in the failure of carbon ceramic brake disc performance and high production costs.

Method used

A layer of long fiber weft-free carbon cloth and a layer of short fiber mesh are alternately laid, and a carbon fiber prefabricated body is formed by three-dimensional needle-branching and CVI1-machine-CVI2 two chemical vapor deposition and high-temperature graphitization heat treatment are carried out to form High-density, uniform-density carbon-carbon crucible.

Benefits of technology

The high density and uniform density of carbon-carbon crucibles are achieved, the bending strength, compressive strength, impact toughness and service life are improved, the production cost is reduced, and the performance of carbon ceramic brake discs is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039031A_ABST
    Figure CN119039031A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ultrahigh-temperature composite materials, and relates to a carbon-carbon crucible for melting siliconizing of a carbon-ceramic brake disc and a preparation method of the carbon-carbon crucible, and the preparation method comprises the following steps: S1, alternately paving a layer of long-fiber weftless carbon cloth and a layer of short-fiber net tire to form a composite layer as raw materials of the carbon-carbon crucible; s2, needling the multiple composite layers in a three-dimensional needling weaving mode to form a carbon fiber preform; s3, the carbon fiber preform is placed in a high-temperature furnace to be subjected to chemical vapor deposition twice and densification twice, and a high-density carbon-carbon crucible preform is prepared; s4, high-temperature graphitization heat treatment is carried out, the graphitization degree of the carbon-carbon crucible is increased, and the overall structure and performance stability of the crucible are improved; and S5, machining treatment forming is conducted. The carbon-carbon crucible obtained by the method disclosed by the invention has the mechanical properties of high density, excellent bending strength, compressive strength, interlaminar shear strength, impact toughness, tensile strength and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ultra-high temperature composite materials and relates to a carbon-carbon crucible used for melting and siliconizing a carbon-ceramic brake disc and a preparation method thereof. Background Art

[0002] Carbon-ceramic brake discs have great market prospects due to their excellent performance, but their manufacturing process is extremely complex, including three steps: CVI (chemical vapor deposition), RMI (molten siliconization), and post-processing. The molten siliconization process requires the carbon-ceramic disc to be placed in a high-temperature furnace above 1700°C, and the silicon material is melted and infiltrated into the carbon-ceramic disc by high temperature, thereby increasing the density of the carbon-ceramic disc to obtain a carbon-ceramic brake disc with excellent performance. This requires the use of special vessels to carry the carbon-ceramic disc and the silicon material so that the two can be fully integrated. The carbon-carbon material crucible is the best solution.

[0003] However, there are many problems in the use of ordinary carbon-carbon crucibles today: due to the disadvantages of materials and manufacturing processes, carbon-carbon crucibles are mostly used once for CVI production. When the crucible preform is produced in CVI, the carbon deposition effect is best at a depth of 1-2mm on the surface of the preform. As time goes by, the surface deposited carbon content is much greater than the internal deposited carbon content. The surface depth of 1-2mm has a high density, resulting in low porosity. Therefore, the speed at which gas enters the interior of the preform from the surface of the preform is getting slower and slower, resulting in a much lower density inside the preform than the surface of the preform. As time goes by, the gas content entering the interior of the preform is negligible, and the deposited carbon content inside the preform is also low. The prepared carbon-carbon crucible has uneven density (external density 1.70g / cm 3 、Internal density 1.50g / cm 3 ) results in lower performance. And due to the drawbacks of this process, the CVI process time of carbon-carbon crucible is too long, resulting in high production costs. When the crucible is used in an ultra-high temperature environment, the service life is short due to poor thermal conductivity, and the matrix will break and become unusable after producing dozens of batches; and ordinary crucibles have poor thermal shock resistance. Carbon-ceramic brake discs require a faster heating rate at ultra-high temperatures. After experiencing multiple rapid heating, the matrix of ordinary crucibles will be damaged; and the matrix of ordinary crucibles is brittle, and cracks will appear during use, resulting in scrapping and high production costs; and because the RMI (molten siliconization) environment of carbon-ceramic discs is above 1700°C, the poor thermal conductivity of ordinary crucibles results in poor molten siliconization effect, and the performance of the produced carbon-ceramic discs does not meet the standards. Summary of the invention

[0004] The object of the present invention is to solve the above-mentioned problem and to provide a carbon-carbon crucible for molten siliconization of carbon-ceramic brake discs and a preparation method thereof.

[0005] In order to achieve the above object, the present invention adopts the following scheme:

[0006] A method for preparing a carbon-carbon crucible for melt siliconizing of a carbon-ceramic brake disc comprises the following steps:

[0007] S1. The raw materials of the carbon-carbon crucible are a layer of long-fiber non-weft carbon cloth and a layer of short-fiber mesh tire alternately laid to form a composite layer. In each composite layer, the angle between the long-fiber non-weft carbon cloth and the short-fiber mesh tire is 90°;

[0008] S2, using a three-dimensional needle-punching weaving method to needle-punch multiple composite layers to form a carbon fiber preform;

[0009] S3, placing the carbon fiber preform in a high temperature furnace for CVI1-machining-CVI2 to obtain a high-density carbon-carbon crucible preform;

[0010] S4, performing high-temperature graphitization heat treatment on the carbon-carbon crucible preform prepared in S3;

[0011] S5, machining the crucible preform prepared in S4 into a shape.

[0012] Furthermore, in S1, the raw material long fiber lay carbon cloth is made of T700SC or HTS40 polyacrylonitrile carbon fiber; and the short fiber web is made of T700SC polyacrylonitrile carbon fiber.

[0013] Further, in S2, the acupuncture density is 20-24 needles / cm 2 The weight percentage of the long fiber non-woven carbon cloth in the preform is ≥65%, the weight percentage of the short fiber web is ≤35%, and the interlayer density is (12±2) layers / cm.

[0014] Furthermore, the short fiber web tire adopts carbon fiber with a length of (60±2) mm.

[0015] Furthermore, in S2, the carbon fiber preform has a density of (0.46±0.02) g / cm 3 .

[0016] Furthermore, the S3 includes:

[0017] Step 1: Place the carbon fiber preform in a high temperature furnace for CVI1 to a density of (1.1-1.2) g / cm 3 between;

[0018] Step 2: The preform prepared by the CVI1 process is subjected to shelling treatment, and the overall shape of the preform is subjected to rough processing, with a processing amount of (2±0.2) mm;

[0019] Step 3: Place the preform obtained by shelling treatment in a high temperature furnace for CVI2 treatment to obtain a uniform internal and external density of (1.70±0.05) g / cm 3of prefabricated bodies.

[0020] Furthermore, the process time of CVI1 is (100±5) h, and the process temperature is (1100±50)°C; the process time of CVI2 is (130±5) h, and the process temperature is (1100±50)°C.

[0021] Furthermore, in S4, the temperature of the high temperature graphitization treatment is (2200±50)°C, and the process time is (180-200)h.

[0022] In addition, the present invention also provides a carbon-carbon crucible for molten siliconization of carbon-ceramic brake discs, which is prepared by the above preparation method.

[0023] The beneficial effects of the present invention are as follows:

[0024] (1) The method of the present invention, wherein the deposition process adopts CVI 1 (pre-deposition) - machining - CVI 2, and two chemical vapor deposition and two densification methods are carried out continuously. The secondary deposition + process shelling treatment can shorten the deposition time, which is about 3 / 4 of the time of the existing ordinary one-time deposition process, greatly reducing the production cost and saving the amount of raw materials (gas); and the uniform density inside and outside the prepared carbon-carbon crucible avoids the problem of uneven density inside and outside the crucible caused by the one-time deposition process.

[0025] (2) The carbon-carbon crucible prepared by the method of the present invention has excellent comprehensive performance, high density, excellent bending strength, compressive strength, interlaminar shear strength, impact toughness, tensile strength and other mechanical properties; low porosity, the crucible can be used for high-temperature furnace to continuously prepare hundreds of batches of carbon-ceramic brake discs, so that the prepared carbon-carbon crucible has a longer service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a flow chart of acupuncture of a carbon fiber preform in the method of the present invention;

[0027] Figure 2 This is a picture of the carbon-carbon crucible sample prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0029] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The embodiments cannot be described one by one here, but the embodiments of the present invention are not therefore limited to the following embodiments.

[0030] Example 1

[0031] A method for preparing a carbon-carbon crucible for melt-siliconizing a carbon-ceramic brake disc, referring to Figure 1 As shown, the following steps are included:

[0032] S1. The raw materials of carbon-carbon crucible are a layer of long fiber non-woven carbon cloth and a layer of short fiber mesh tire, which are alternately laid to form a composite layer. The design angle between the long fiber non-woven carbon cloth and the short fiber mesh tire of each composite layer is 90°; among them, the long fiber non-woven cloth adopts T700SC or HTS40 polyacrylonitrile carbon fiber; the short fiber mesh tire adopts T700SC polyacrylonitrile carbon fiber with a length of 60mm;

[0033] Carbon fiber specifications are 12K, carbon content ≥ 95%; tensile strength ≥ 3.9GPa; tensile modulus ≥ 185Gpa; density ≥ 1.75g / cm 3 ;

[0034] S2, using three-dimensional needle-punching weaving to needle-punch multiple composite layers to form a density of 0.48g / cm 3 Carbon fiber preform; wherein the needle punching density is 22 needles / cm 2 , the weight percentage of the non-woven fabric in the preform is ≥70%, the weight percentage of the web is ≤30%, and the interlayer density is 14 layers / cm;

[0035] S3, placing the carbon fiber preform in a high temperature furnace for CVI1 (pre-deposition)-machining-CVI2 to obtain a high-density carbon-carbon crucible preform;

[0036] The specific steps are as follows:

[0037] Step 1: The carbon fiber preform is placed in a high temperature furnace for CVI1 (pre-deposition) for 100 hours at a temperature of 1150°C to obtain a density of 1.2 g / cm 3 The preform;

[0038] Step 2: The preform prepared by CVI1 pre-deposition is processed and shelled, and the overall shape of the preform is roughly processed with a processing amount of 2.0 mm;

[0039] Step 3: Place the preform obtained by shelling treatment in a high temperature furnace for CVI2 (secondary chemical vapor deposition) treatment for 130 hours at a temperature of 1150°C to obtain a uniform internal and external density of 1.77 g / cm 3 Preforms;

[0040] S4, performing high-temperature graphitization heat treatment on the carbon-carbon crucible preform prepared in S3, the temperature is 2200° C., the process time is 200 hours, the graphitization degree of the carbon-carbon crucible is increased, and the overall structure and performance stability of the crucible are improved;

[0041] S5, machining the crucible preform prepared in S4, and processing and shaping it according to the required crucible structure and size, referring to Figure 2 shown.

[0042] Example 2

[0043] A method for preparing a carbon-carbon crucible for melt siliconizing of a carbon-ceramic brake disc comprises the following steps:

[0044] S1. The raw materials of carbon-carbon crucible are a layer of long fiber non-woven carbon cloth and a layer of short fiber mesh tire, which are alternately laid to form a composite layer. The design angle between the long fiber non-woven carbon cloth and the short fiber mesh tire of each composite layer is 90°; among them, the long fiber non-woven cloth adopts T700SC or HTS40 polyacrylonitrile carbon fiber; the short fiber mesh tire adopts T700SC polyacrylonitrile carbon fiber with a length of 58mm;

[0045] Carbon fiber specifications are 12K, carbon content ≥ 90%; tensile strength ≥ 3.9GPa; tensile modulus ≥ 180Gpa; density ≥ 1.70g / cm 3 ;

[0046] S2. Use a three-dimensional needle-punching method to needle-punch multiple composite layers to form a carbon fiber preform with a density of 0.45g / cm3; wherein the needle-punching density is 20 needles / cm 2 , the weight percentage of the non-woven fabric in the preform is ≥65%, the weight percentage of the web is ≤35%, and the interlayer density is 12 layers / cm;

[0047] S3, placing the carbon fiber preform in a high temperature furnace for CVI1 (pre-deposition)-machining-CVI2 to obtain a high-density carbon-carbon crucible preform;

[0048] The specific steps are as follows:

[0049] Step 1: The carbon fiber preform is placed in a high temperature furnace for CVI1 (pre-deposition) for 95 hours at a temperature of 1100°C to obtain a density of 1.16 g / cm 3 The preform;

[0050] Step 2: The preform prepared by CVI1 pre-deposition is processed and shelled, and the overall shape of the preform is roughly processed with a processing amount of 2.0 mm;

[0051] Step 3: Place the preform obtained by shelling treatment in a high temperature furnace for CVI2 (secondary chemical vapor deposition) treatment for 125 hours at a temperature of 1100°C to obtain a uniform internal and external density of 1.75 g / cm 3 Preforms;

[0052] S4, subjecting the carbon-carbon crucible preform prepared in S3 to a high-temperature graphitization heat treatment at a temperature of 2230° C. for a process time of 180 h, thereby increasing the graphitization degree of the carbon-carbon crucible and improving the overall structure and performance stability of the crucible;

[0053] S5, machining the crucible preform prepared in S4, and processing and shaping it according to the required crucible structure and size.

[0054] Comparative Example 1

[0055] A method for preparing a carbon-carbon crucible for melting siliconization of carbon-ceramic brake discs,

[0056] Compared with Example 1, the difference of Comparative Example 1 is:

[0057] S3, placing the carbon fiber preform in a high temperature furnace for chemical vapor deposition for 200 hours at a temperature of 1150°C, and obtaining a density of 1.40 g / cm 3 A carbon-carbon crucible preform;

[0058] Other operation and process parameters are the same as those in Example 1.

[0059] Comparative Example 2

[0060] A method for preparing a carbon-carbon crucible for melting siliconization of carbon-ceramic brake discs,

[0061] Compared with Example 1, the difference of Comparative Example 1 is:

[0062] S3, placing the carbon fiber preform in a high temperature furnace for CVI1 (pre-deposition)-machining-CVI2 to obtain a high-density carbon-carbon crucible preform;

[0063] The specific steps are as follows:

[0064] Step 1: The carbon fiber preform is placed in a high temperature furnace for CVI1 (pre-deposition) for 90 hours at a temperature of 1050°C to obtain a density of 1.05 g / cm 3 The preform;

[0065] Step 2: The preform prepared by CVI1 pre-deposition is processed and shelled, and the overall shape of the preform is roughly processed with a processing amount of 2.0 mm;

[0066] Step 3: Place the preform obtained by shelling treatment in a high temperature furnace for CVI2 (secondary chemical vapor deposition) treatment for 130 hours at a temperature of 1150°C to obtain a uniform internal and external density of 1.60 g / cm 3 Preforms;

[0067] Other operation and process parameters are the same as those in Example 1.

[0068] Comparative Example 3

[0069] A method for preparing a carbon-carbon crucible for melting siliconization of carbon-ceramic brake discs,

[0070] Compared with Example 1, the difference of Comparative Example 1 is:

[0071] S3, placing the carbon fiber preform in a high temperature furnace for CVI1 (pre-deposition)-machining-CVI2 to obtain a high-density carbon-carbon crucible preform;

[0072] The specific steps are as follows:

[0073] Step 1: The carbon fiber preform is placed in a high temperature furnace for CVI1 (pre-deposition) for 100 hours at a temperature of 1150°C to obtain a density of 1.2 g / cm 3 The preform;

[0074] Step 2: The preform prepared by CVI1 pre-deposition is processed and shelled, and the overall shape of the preform is roughly processed with a processing amount of 2.0 mm;

[0075] Step 3: Place the preform obtained by shelling treatment in a high temperature furnace for CVI2 (secondary chemical vapor deposition) treatment for 130 hours at a temperature of 1150°C to obtain a uniform internal and external density of 1.75 g / cm 3 Preforms;

[0076] S4. Performing a high-temperature graphitization heat treatment on the carbon-carbon crucible preform prepared in S3, the temperature being 1900° C. and the process time being 200 h.

[0077] Test Examples The products obtained from Examples 1-2 and Comparative Examples 1-3 of the present invention were tested for relevant properties:

[0078] The product adopts the group standard "Passenger Car Carbon Ceramic Brake Disc Product Standard and Test Method" to conduct relevant performance testing. The specific test results are shown in Table 1.

[0079] Table 1 Performance test results of products obtained from Examples 1-2 and Comparative Examples 1-3

[0080]

[0081] From the data in Table 1, we can see that

[0082] In both Example 1 and Example 2, the primary deposition density reached 1.15 g / cm 3 Above, the secondary deposition density has reached 1.75g / cm 3 In contrast, the densification effect of Example 1 is better; in Example 1 and Example 2, the bending strength is greater than 120Mpa, the compressive strength is greater than 240Mpa, the interlaminar shear strength is greater than 12Mpa, and the impact toughness is greater than 20KJ / m 2 , tensile strength greater than 80Mpa, and porosity less than 9%. The performance of the samples prepared in the two examples is excellent. In contrast, the average performance of the samples prepared in Example 1 is better than that in Example 2, which is the best example of this solution. The final product obtained in the comparative example is lower than the product obtained in the embodiment of the present invention in terms of bending strength, interlaminar shear strength, tensile strength, porosity, etc.

[0083] The above is only one embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a carbon-carbon crucible for melt siliconization of carbon-ceramic brake discs, characterized in that: The following steps are involved: S1. The raw materials of the carbon-carbon crucible are a layer of long-fiber non-weft carbon cloth and a layer of short-fiber mesh tire alternately laid to form a composite layer. In each composite layer, the angle between the long-fiber non-weft carbon cloth and the short-fiber mesh tire is 90°; S2, using a three-dimensional needle-punching weaving method to needle-punch multiple composite layers to form a carbon fiber preform; S3, placing the carbon fiber preform in a high temperature furnace for CVI1-machining-CVI2 to obtain a high-density carbon-carbon crucible preform; S4, performing high-temperature graphitization heat treatment on the carbon-carbon crucible preform prepared in S3; S5, machining the crucible preform prepared in S4 into a shape.

2. The method for preparing a carbon-carbon crucible according to claim 1, characterized in that: In S1, the raw material long fiber non-woven carbon cloth is made of T700SC or HTS40 polyacrylonitrile carbon fiber; the short fiber web is made of T700SC polyacrylonitrile carbon fiber.

3. The method for preparing a carbon-carbon crucible according to claim 1, characterized in that: In S2, the acupuncture density is 20-24 needles / cm 2 The weight percentage of the long fiber non-woven carbon cloth in the preform is ≥65%, the weight percentage of the short fiber web is ≤35%, and the interlayer density is (12±2) layers / cm.

4. The method for preparing a carbon-carbon crucible according to claim 2, characterized in that: The short fiber web tire uses carbon fiber with a length of (60±2) mm.

5. The method for preparing a carbon-carbon crucible according to claim 1, characterized in that: In S2, the carbon fiber preform density is (0.46±0.02) g / cm 3 .

6. The method for preparing a carbon-carbon crucible according to claim 1, characterized in that: The S3 includes: Step 1: Place the carbon fiber preform in a high temperature furnace for CVI1 to a density of (1.1-1.2) g / cm 3 between; Step 2: The preform prepared by the CVI1 process is subjected to shelling treatment, and the overall shape of the preform is subjected to rough processing, with a processing amount of (2±0.2) mm; Step 3: Place the preform obtained by shelling treatment in a high temperature furnace for CVI2 treatment to obtain a uniform internal and external density of (1.70±0.05) g / cm 3 of prefabricated bodies.

7. The method for preparing a carbon-carbon crucible according to claim 6, characterized in that: The process time of CVI1 (pre-deposition) is (100±5)h, and the process temperature is (1100±50)℃; the process time of CVI2 is (130±5)h, and the process temperature is (1100±50)℃.

8. The method for preparing a carbon-carbon crucible according to claim 1, characterized in that: In S4, the temperature of the high temperature graphitization treatment is (2200±50)°C, and the process time is (180-200)h.

9. A carbon-carbon crucible for melt siliconizing of carbon-ceramic brake discs, prepared according to the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of carbon / carbon throat liner

    CN115448744A

  • Method for rapidly preparing carbon / carbon composite material brake disc

    CN115819101A

  • Preparation method of low-cost high-thermal-conductivity carbon / carbon composite material

    CN115849930A

  • Preparation method of high-carbon-yield carbon / carbon composite material brake disc

    CN117550908A

  • Carbon-ceramic crucible for siliconizing carbon-ceramic brake disc and preparation method of carbon-ceramic crucible