Preparation method of pesticide intermediate ethyl difluoroacetate

By reacting the modified catalyst with ethyl difluoroacetic acid, the problems of low atom utilization rate and poor economicality prepared by difluoroacetic acid in the prior art are solved, and high yield, low cost and environmentally friendly ethyl difluoroacetic acid is achieved. Preparation, suitable for industrial applications.

CN119039141APending Publication Date: 2024-11-29HUNAN SPARK SCI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411313531.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, the preparation process of difluoroacetic acid has problems such as low atom utilization rate, poor economics, high reaction risk, serious environmental pollution, complex equipment and high cost.

Method used

Using ethyl difluorochloroacetate as raw material, the reaction is carried out by using a modified catalyst in a fixed bed. The catalyst is made of microcrystalline cellulose, starch and carboxymethyl chitosan, combined with nickel and copper as the main catalyst, and passed Doping of Ca/Mg ions and lanthanum regulates the pore structure and electron density of the catalyst, reduces the reaction activation energy, improves yield and reaction control.

Benefits of technology

The high yield, low cost and environmentally friendly preparation of ethyl difluoroacetate is achieved, the reaction conditions are mild, easy to be industrially applied, and the catalyst has high activity and reusability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a preparation method of a pesticide intermediate ethyl difluoroacetate, and belongs to the technical field of organic synthesis. The method comprises the following steps: adding a catalyst into a fixed bed, replacing air with inert gas, heating, introducing hydrogen and ethyl difluorochloroacetate gas, and collecting a product while reacting, thereby obtaining the pesticide intermediate ethyl difluoroacetate. The ethyl difluoroacetate is prepared by taking the ethyl difluorochloroacetate as the raw material, the method has the advantages of high yield, easiness in reaction control, small environmental pollution and the like, the reaction condition is mild, the cost is relatively low, and industrial application is easy to realize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic synthesis, and in particular to a method for preparing ethyl difluoroacetate, a pesticide intermediate. Background Art

[0002] Ethyl difluoroacetate is an important organic intermediate, mainly used in medicine, pesticides, organic synthesis and other fields. It has a very broad market prospect and a very high development value. Ethyl difluoroacetate is prepared by esterification of difluoroacetic acid. At present, the preparation process of difluoroacetic acid is usually divided into the following types: One is to use tetrafluoroethylene as a raw material and react it with inorganic bases, ammonia or amines, sodium bisulfite, etc. to prepare difluoroacetic acid. In this process, tetrafluoroethylene is prone to self-polymerization under high temperature conditions, resulting in low atomic utilization; at the same time, tetrafluoroethylene often participates in the reaction in the form of difluorocarbene, which has only a 50% utilization rate, and the atomic utilization rate is not high, resulting in poor economic efficiency; The second method is to use acyl compounds as substrates, react with potassium fluoride, and then hydrolyze and distill to prepare difluoroacetic acid. In this process, when the acyl compound is difluoroacetyl chloride or difluoroacetyl fluoride, the selectivity of the reaction is poor; in addition, fluorides such as hydrogen fluoride are easily produced during the reaction, resulting in high risk of the reaction and impact on the environment; The third is to use halogenated acetic acid (at least one halogen atom is not a fluoride ion) as a raw material and react with a fluorinating agent to prepare difluoroacetic acid. In this process, the use of fluorinating agents has high requirements for reaction equipment, and the cost of customizing special equipment is high; in addition, fluoride ions are very harmful to the environment; and after the exchange reaction, a large amount of halogen inorganic salts will be produced, resulting in a high amount of three wastes; Fourth, hydrogen peroxide reacts with 2-chloro-1,1-difluoroethane, 1,1-difluoroethane and other raw materials to prepare difluoroacetic acid. This process uses a fixed bed as the reaction equipment, and uses KMnO4 / C, strong acid ion exchange resin, tungstic acid complex, heteropoly acid and the like as catalysts. The equipment structure is complex and the cost is high, resulting in high production costs and poor economic efficiency. In addition, hydrogen peroxide reacts and decomposes rapidly in a closed pressure vessel at a high temperature of 140°C, resulting in greater risks. Fifth, using chlorodifluoromethane and sodium cyanide as raw materials, a cyanation reaction is carried out in a metal hydroxide aqueous solution at 50-120°C and 10-150°C for 2-8h to prepare difluoroacetonitrile, and then a hydrolysis reaction is carried out under strong alkaline conditions to prepare difluoroacetamide and difluoroacetic acid. In this process, in an aqueous solvent system, the cyano group is easily attacked by water, resulting in poor reaction selectivity; in addition, difluorocarbene is also attacked by a metal hydroxide aqueous solution to generate by-products, resulting in low atomic utilization; furthermore, the reaction temperature of this process is high and the reaction time is long, which is easy to cause polymerization of intermediate products, resulting in poor reaction economy. Summary of the invention

[0003] The invention aims to provide a method for preparing ethyl difluoroacetate, a pesticide intermediate, by using ethyl difluorochloroacetate as a raw material to prepare ethyl difluoroacetate, which has the advantages of high yield, easy reaction control, low environmental pollution, mild reaction conditions, low cost and easy industrial application.

[0004] The technical solution of the present invention is achieved in this way: The invention provides a method for preparing ethyl difluoroacetate, a pesticide intermediate. The method comprises the following steps: placing a catalyst in a fixed bed, replacing air with an inert gas, heating the bed, introducing hydrogen and ethyl difluorochloroacetate gas, reacting and collecting products to obtain the pesticide intermediate ethyl difluoroacetate.

[0005] As a further improvement of the present invention, the molar ratio of the hydrogen to the ethyl chlorodifluoroacetate gas is 25-35:1.

[0006] As a further improvement of the present invention, the temperature is raised to 180-190°C.

[0007] As a further improvement of the present invention, the preparation method of the catalyst is as follows: S1. Preparation of wrinkled nanospheres: Dissolve microcrystalline cellulose, starch and carboxymethyl chitosan in water to form a uniform solution, spray dry and carbonize to obtain wrinkled nanospheres; S2. Preparation of carrier: adding wrinkled nanospheres to ethanol, adding aluminum isopropoxide, tetraethyl orthosilicate and tetrabutyl titanate, stirring and mixing, adding ammonia water to adjust the pH value of the solution, stirring the reaction, centrifuging, washing, drying, and calcining to obtain a carrier; S3. Ni / Cu loading: adding the carrier to water, adding nickel salt and copper salt, stirring for adsorption, evaporating the solvent, washing, and drying to obtain a Ni / Cu loaded catalyst; S4. Regulation of Ca / Mg ions: Add the Ni / Cu loaded catalyst into water, add calcium salt and magnesium salt, heat and stir to react, filter, wash, and dry to obtain a modified Ni / Cu loaded catalyst; S5. La doping: dissolve lanthanum salt in water, add modified Ni / Cu loaded catalyst, impregnate, filter, wash and dry to obtain the catalyst.

[0008] As a further improvement of the present invention, in step S1, the mass ratio of microcrystalline cellulose, starch and carboxymethyl chitosan is 1-2:7-10:4-6, the carbonization temperature is 750-850° C., and the time is 1-3 h.

[0009] As a further improvement of the present invention, the mass ratio of the wrinkled nanospheres, aluminum isopropoxide, tetraethyl orthosilicate and tetrabutyl titanate in step S2 is 10:1-2:3-4:1-2, the pH value of the adjusted solution is 9-10, the stirring reaction time is 3-5h, the calcination temperature is 300-400°C, and the time is 2-3h.

[0010] As a further improvement of the present invention, the mass ratio of the carrier, nickel salt and copper salt in step S3 is 5:1-2:0.4-0.9, the stirring adsorption time is 0.5-1h, the nickel salt is at least one of nickel chloride, nickel nitrate and nickel sulfate, and the copper salt is at least one of copper chloride, copper sulfate and copper nitrate.

[0011] As a further improvement of the present invention, the mass ratio of the Ni / Cu loaded catalyst, calcium salt and magnesium salt in step S4 is 100:1-2:0.7-1.2, the temperature of the heating and stirring reaction is 40-50°C, the time is 1-2h, the calcium salt is calcium chloride or calcium nitrate, and the magnesium salt is magnesium chloride, magnesium sulfate or magnesium nitrate.

[0012] As a further improvement of the present invention, in step S5, the mass ratio of the lanthanum salt to the modified Ni / Cu loaded catalyst is 0.5-1:100, the impregnation time is 3-5h, and the lanthanum salt is lanthanum chloride.

[0013] As a further improvement of the present invention, the preparation method of the catalyst is specifically as follows: S1. Preparation of wrinkled nanospheres: 1-2 parts by weight of microcrystalline cellulose, 7-10 parts by weight of starch and 4-6 parts by weight of carboxymethyl chitosan are dissolved in water to form a uniform solution, spray dried, and carbonized at 750-850° C. for 1-3 h to obtain wrinkled nanospheres; S2. Preparation of a carrier: 10 parts by weight of wrinkled nanospheres were added to ethanol, 1-2 parts by weight of aluminum isopropoxide, 3-4 parts by weight of ethyl orthosilicate and 1-2 parts by weight of tetrabutyl titanate were added, and the mixture was stirred and mixed uniformly, and ammonia was added dropwise to adjust the pH value of the solution to 9-10, and the reaction was stirred for 3-5 hours, centrifuged, washed, dried, and calcined at 300-400°C for 2-3 hours to obtain a carrier; S3 Ni / Cu loading: 5 parts by weight of the carrier was added to water, 1-2 parts by weight of nickel salt and 0.4-0.9 parts by weight of copper salt were added, and the adsorption was stirred for 0.5-1h, the solvent was evaporated, washed, and dried to obtain a Ni / Cu loaded catalyst; S4. Regulation of Ca / Mg ions: 10 parts by weight of a Ni / Cu-loaded catalyst is added to water, 0.1-0.2 parts by weight of a calcium salt and 0.07-0.12 parts by weight of a magnesium salt are added, heated to 40-50° C., stirred for reaction for 1-2 hours, filtered, washed, and dried to obtain a modified Ni / Cu-loaded catalyst; S5. La doping: 0.05-0.1 parts by weight of lanthanum salt is dissolved in water, 10 parts by weight of modified Ni / Cu loaded catalyst is added, and the mixture is immersed for 3-5 hours, filtered, washed, and dried to obtain a catalyst.

[0014] The present invention has the following beneficial effects: The present invention prepares a catalyst. First, hydrogen bonds and self-assembly between microcrystalline cellulose, starch and carboxymethyl chitosan are used to form microspheres during spray drying. Due to the rapid volatilization of water, wrinkled microspheres are formed. After high-temperature carbonization, the original morphology structure can still be maintained without structural collapse and damage. The wrinkled nanospheres prepared by the method have a large specific surface area, which is convenient for the subsequent preparation of carriers and has the effects of increasing the specific surface area of ​​the carriers.

[0015] Through the sol-gel reaction, the aluminum oxide / silicon oxide / titanium oxide composite is in situ deposited on the surface of the obtained wrinkled nanospheres. Through the appropriate mass ratio of the three, the interaction between the metal and the carrier is effectively adjusted, and the subsequent electron density of the nickel and copper species is changed, thereby improving the catalyst's adsorption of H2 and ethyl difluorochloroacetate, providing abundant sites for the reaction of the two. At the same time, under the synergistic catalytic action of the composite catalyst nickel and copper species, the reaction efficiency can be significantly improved, the reaction activation energy can be reduced, the reaction temperature is reduced to a certain extent, and the yield of the product is also improved.

[0016] The present invention uses nickel and copper as main catalysts for the reaction, effectively avoiding the use of precious metal catalysts such as Pt, Au, etc., greatly reducing the cost of the reaction, improving the reaction yield, and thus improving the industrial application of the product.

[0017] The present invention can effectively regulate the pore structure of the carrier by doping with Ca and Mg ions, so that the pores of the catalyst carrier shrink to a certain extent and are not easily blocked by carbon deposition, thereby improving the catalytic activity and enabling the catalyst to be used multiple times without being easily poisoned.

[0018] The present invention further improves the electron density on the catalyst surface by doping with lanthanide metal La due to its special outer electron distribution, and can also improve the catalyst follow-up to a certain extent and improve the reaction efficiency.

[0019] The invention uses ethyl difluoroacetate as a raw material to prepare ethyl difluoroacetate, has the advantages of high yield, easy reaction control, small environmental pollution, mild reaction conditions, low cost, and easy industrial application. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Preparation Example 1 Preparation of Catalyst The specific method is as follows: S1. Preparation of wrinkled nanospheres: 1 g of microcrystalline cellulose, 7 g of starch and 4 g of carboxymethyl chitosan were dissolved in 500 mL of water to form a uniform solution, which was spray dried and carbonized at 750 °C for 1 h to obtain wrinkled nanospheres; S2. Preparation of the carrier: 10 g of wrinkled nanospheres were added to 500 mL of ethanol, 1 g of aluminum isopropoxide, 3 g of tetraethyl orthosilicate and 1 g of tetrabutyl titanate, and the mixture was stirred for 30 min. Ammonia was added dropwise to adjust the pH value of the solution to 9, and the mixture was stirred for 3 h. The mixture was centrifuged, washed, dried and calcined at 300 ° C for 2 h to obtain the carrier. S3. Ni / Cu loading: 5 g of the carrier was added to 200 mL of water, 1 g of nickel chloride and 0.4 g of copper chloride were added, and the mixture was stirred and adsorbed for 0.5 h, the solvent was evaporated, washed, and dried to obtain a Ni / Cu loaded catalyst; S4. Regulation of Ca / Mg ions: 10 g of Ni / Cu-loaded catalyst was added to 200 mL of water, and 0.1 g of calcium chloride and 0.07 g of magnesium chloride were added. The mixture was heated to 40°C, stirred for 1 h, filtered, washed, and dried to obtain a modified Ni / Cu-loaded catalyst. S5. La doping: 0.05 g of lanthanum chloride was dissolved in 100 mL of water, 10 g of the modified Ni / Cu loaded catalyst was added, and the mixture was immersed for 3 h, filtered, washed, and dried to obtain a catalyst.

[0022] Preparation Example 2 Preparation of Catalyst The specific method is as follows: S1. Preparation of wrinkled nanospheres: 2 g of microcrystalline cellulose, 10 g of starch and 6 g of carboxymethyl chitosan were dissolved in 500 mL of water to form a uniform solution, which was spray dried and carbonized at 850 °C for 3 h to obtain wrinkled nanospheres; S2. Preparation of the carrier: 10 g of wrinkled nanospheres were added to 500 mL of ethanol, 2 g of aluminum isopropoxide, 4 g of tetraethyl orthosilicate and 2 g of tetrabutyl titanate, and the mixture was stirred for 30 min. Ammonia was added dropwise to adjust the pH value of the solution to 10, and the mixture was stirred for 5 h. The mixture was centrifuged, washed, dried and calcined at 400 ° C for 3 h to obtain the carrier. S3. Ni / Cu loading: 5 g of the carrier was added to 200 mL of water, 2 g of nickel sulfate and 0.9 g of copper sulfate were added, and the mixture was stirred and adsorbed for 1 h, the solvent was evaporated, washed, and dried to obtain a Ni / Cu loaded catalyst; S4. Regulation of Ca / Mg ions: 10 g of Ni / Cu-loaded catalyst was added to 200 mL of water, and 0.2 g of calcium nitrate and 0.12 g of magnesium nitrate were added. The mixture was heated to 50°C, stirred for 2 h, filtered, washed, and dried to obtain a modified Ni / Cu-loaded catalyst. S5. La doping: 0.1 g of lanthanum chloride was dissolved in 100 mL of water, 10 g of the modified Ni / Cu loaded catalyst was added, and the mixture was immersed for 5 h, filtered, washed, and dried to obtain a catalyst.

[0023] Preparation Example 3 Preparation of Catalyst The specific method is as follows: S1. Preparation of wrinkled nanospheres: 1.5 g of microcrystalline cellulose, 8 g of starch and 5 g of carboxymethyl chitosan were dissolved in 500 mL of water to form a uniform solution, which was spray dried and carbonized at 800 °C for 2 h to obtain wrinkled nanospheres; S2. Preparation of the carrier: 10 g of wrinkled nanospheres were added to 500 mL of ethanol, 1.5 g of aluminum isopropoxide, 3.5 g of ethyl orthosilicate and 1.5 g of tetrabutyl titanate, and the mixture was stirred for 30 min. Ammonia water was added dropwise to adjust the pH value of the solution to 9.5. The mixture was stirred for 4 h, centrifuged, washed, dried, and calcined at 350 ° C for 2.5 h to obtain the carrier. S3. Ni / Cu loading: 5 g of the carrier was added to 200 mL of water, 1.5 g of nickel nitrate and 0.6 g of copper nitrate were added, and the mixture was stirred and adsorbed for 1 h, the solvent was evaporated, washed, and dried to obtain a Ni / Cu loaded catalyst; S4. Regulation of Ca / Mg ions: 10 g of Ni / Cu-loaded catalyst was added to 200 mL of water, and 0.15 g of calcium nitrate and 0.1 g of magnesium sulfate were added. The mixture was heated to 45°C, stirred for 1.5 h, filtered, washed, and dried to obtain a modified Ni / Cu-loaded catalyst. S5. La doping: 0.07 g of lanthanum chloride was dissolved in 100 mL of water, 10 g of the modified Ni / Cu loaded catalyst was added, and the mixture was immersed for 4 h, filtered, washed, and dried to obtain a catalyst.

[0024] Comparative Preparation Example 1 Compared with Preparation Example 3, the difference is that step S1 is not performed.

[0025] The details are as follows: S1. Preparation of the carrier: 1.5 g of aluminum isopropoxide, 3.5 g of ethyl orthosilicate and 1.5 g of tetrabutyl titanate were added to 500 mL of ethanol, and the mixture was stirred for 30 min. Ammonia was added dropwise to adjust the pH value of the solution to 9.5. The mixture was stirred for 4 h, centrifuged, washed, dried, and calcined at 350 ° C for 2.5 h to obtain a carrier. S2. Ni / Cu loading: 5 g of the carrier was added to 200 mL of water, 1.5 g of nickel nitrate and 0.6 g of copper nitrate were added, and the mixture was stirred and adsorbed for 1 h, the solvent was evaporated, washed, and dried to obtain a Ni / Cu loaded catalyst; S3. Regulation of Ca / Mg ions: 10 g of Ni / Cu-loaded catalyst was added to 200 mL of water, and 0.15 g of calcium nitrate and 0.1 g of magnesium sulfate were added. The mixture was heated to 45°C, stirred for 1.5 h, filtered, washed, and dried to obtain a modified Ni / Cu-loaded catalyst. S4. La doping: 0.07 g of lanthanum chloride was dissolved in 100 mL of water, 10 g of the modified Ni / Cu loaded catalyst was added, and the mixture was immersed for 4 h, filtered, washed, and dried to obtain a catalyst.

[0026] Comparative Preparation Example 2 Compared with Preparation Example 3, the difference is that aluminum isopropoxide is not added in step S2.

[0027] The details are as follows: S2. Preparation of carrier: 10 g of wrinkled nanospheres were added to 500 mL of ethanol, 3.5 g of ethyl orthosilicate and 1.5 g of tetrabutyl titanate, and the mixture was stirred for 30 min. Ammonia water was added dropwise to adjust the pH value of the solution to 9.5. The mixture was stirred for 4 h, centrifuged, washed, dried, and calcined at 350 °C for 2.5 h to obtain the carrier.

[0028] Comparative Preparation Example 3 Compared with Preparation Example 3, the difference is that tetraethyl orthosilicate is not added in step S2.

[0029] The details are as follows: S2. Preparation of the carrier: 10 g of wrinkled nanospheres were added to 500 mL of ethanol, 1.5 g of aluminum isopropoxide and 1.5 g of tetrabutyl titanate, and the mixture was stirred for 30 min. Ammonia water was added dropwise to adjust the pH value of the solution to 9.5. The mixture was stirred for 4 h, centrifuged, washed, dried, and calcined at 350 °C for 2.5 h to obtain the carrier.

[0030] Comparative Preparation Example 4 Compared with Preparation Example 3, the difference is that tetrabutyl titanate is not added in step S2.

[0031] The details are as follows: S2. Preparation of carrier: 10 g of wrinkled nanospheres were added to 500 mL of ethanol, 1.5 g of aluminum isopropoxide and 3.5 g of tetraethyl orthosilicate, and the mixture was stirred for 30 min. Ammonia water was added dropwise to adjust the pH value of the solution to 9.5. The mixture was stirred for 4 h, centrifuged, washed, dried, and calcined at 350° C. for 2.5 h to obtain the carrier.

[0032] Comparative Preparation Example 5 Compared with Preparation Example 3, the difference is that nickel nitrate is not added in step S3.

[0033] The details are as follows: S3. Cu loading: 5 g of the carrier was added to 200 mL of water, and 2.1 g of copper nitrate was added. The mixture was stirred and adsorbed for 1 h. The solvent was evaporated, washed, and dried to obtain a Cu-loaded catalyst.

[0034] Comparative Preparation Example 6 Compared with Preparation Example 3, the difference is that copper nitrate is not added in step S3.

[0035] The details are as follows: S3. Ni loading: 5 g of the carrier was added to 200 mL of water, and 2.1 g of nickel nitrate was added. The mixture was stirred and adsorbed for 1 h. The solvent was evaporated, washed, and dried to obtain a Ni-loaded catalyst.

[0036] Comparative Preparation Example 7 Compared with Preparation Example 3, the difference is that step S4 is not performed.

[0037] The details are as follows: S1. Preparation of wrinkled nanospheres: 1.5 g of microcrystalline cellulose, 8 g of starch and 5 g of carboxymethyl chitosan were dissolved in 500 mL of water to form a uniform solution, which was spray dried and carbonized at 800 °C for 2 h to obtain wrinkled nanospheres; S2. Preparation of the carrier: 10 g of wrinkled nanospheres were added to 500 mL of ethanol, 1.5 g of aluminum isopropoxide, 3.5 g of ethyl orthosilicate and 1.5 g of tetrabutyl titanate, and the mixture was stirred for 30 min. Ammonia water was added dropwise to adjust the pH value of the solution to 9.5. The mixture was stirred for 4 h, centrifuged, washed, dried, and calcined at 350 ° C for 2.5 h to obtain the carrier. S3. Ni / Cu loading: 5 g of the carrier was added to 200 mL of water, 1.5 g of nickel nitrate and 0.6 g of copper nitrate were added, and the mixture was stirred and adsorbed for 1 h, the solvent was evaporated, washed, and dried to obtain a Ni / Cu loaded catalyst; S4. La doping: 0.07 g of lanthanum chloride was dissolved in 100 mL of water, 10 g of Ni / Cu-loaded catalyst was added, and the mixture was immersed for 4 h. The mixture was filtered, washed, and dried to obtain a catalyst.

[0038] Comparative Preparation Example 8 Compared with Preparation Example 3, the difference is that step S5 is not performed.

[0039] The details are as follows: S1. Preparation of wrinkled nanospheres: 1.5 g of microcrystalline cellulose, 8 g of starch and 5 g of carboxymethyl chitosan were dissolved in 500 mL of water to form a uniform solution, which was spray dried and carbonized at 800 °C for 2 h to obtain wrinkled nanospheres; S2. Preparation of the carrier: 10 g of wrinkled nanospheres were added to 500 mL of ethanol, 1.5 g of aluminum isopropoxide, 3.5 g of ethyl orthosilicate and 1.5 g of tetrabutyl titanate, and the mixture was stirred for 30 min. Ammonia water was added dropwise to adjust the pH value of the solution to 9.5. The mixture was stirred for 4 h, centrifuged, washed, dried, and calcined at 350 ° C for 2.5 h to obtain the carrier. S3. Ni / Cu loading: 5 g of the carrier was added to 200 mL of water, 1.5 g of nickel nitrate and 0.6 g of copper nitrate were added, and the mixture was stirred and adsorbed for 1 h, the solvent was evaporated, washed, and dried to obtain a Ni / Cu loaded catalyst; S4. Regulation of Ca / Mg ions: Add 10 g of Ni / Cu loaded catalyst into 200 mL of water, add 0.15 g of calcium nitrate and 0.1 g of magnesium sulfate, heat to 45°C, stir to react for 1.5 h, filter, wash, and dry to obtain a modified Ni / Cu loaded catalyst, namely the catalyst.

[0040] Test Example 1 The specific surface area and pore volume of the catalyst samples prepared in Preparation Examples 1-3 and Comparative Preparation Examples 1-7 were measured using an ASAP2460 fully automatic specific surface area analyzer produced by Micromeritics Instruments. The results are shown in Table 1.

[0041] Table 1 Group <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Pore volume (cm 3 / g)]]> Preparation Example 1 442.1 0.410 Preparation Example 2 445.9 0.411 Preparation Example 3 447.5 0.412 Comparative Preparation Example 1 268.2 0.236 Comparative Preparation Example 2 402.1 0.366 Comparative Preparation Example 3 410.5 0.370 Comparative Preparation Example 4 396.3 0.361 Comparative Preparation Example 5 422.1 0.401 Comparative Preparation Example 6 429.6 0.395 Comparative Preparation Example 7 384.5 0.345 Comparative Preparation Example 8 400.9 0.369 It can be seen from the above table that the catalysts prepared in Preparation Examples 1-3 of the present invention have a higher specific surface area and a larger pore volume.

[0042] Example 1 This example provides a method for preparing ethyl difluoroacetate, a pesticide intermediate. 1 g of the catalyst prepared in Preparation Example 1 is put into a fixed bed. After nitrogen replaces the air, the temperature is raised to 180° C., hydrogen and ethyl difluorochloroacetate gas are introduced at a molar ratio of 25:1, the reaction is carried out for 4 hours, and the product is collected to obtain ethyl difluoroacetate, a pesticide intermediate.

[0043] Example 2 This example provides a method for preparing ethyl difluoroacetate, a pesticide intermediate. 1 g of the catalyst prepared in Preparation Example 2 is placed in a fixed bed. After nitrogen replaces the air, the bed is heated to 190° C., hydrogen and ethyl difluorochloroacetate gas are introduced at a molar ratio of 35:1, and the reaction is carried out for 4 hours. The product is collected to obtain ethyl difluoroacetate, a pesticide intermediate.

[0044] Example 3 This example provides a method for preparing ethyl difluoroacetate, a pesticide intermediate. 1 g of the catalyst prepared in Preparation Example 3 is placed in a fixed bed. After nitrogen replaces the air, the bed is heated to 185° C., hydrogen and ethyl difluorochloroacetate gas are introduced at a molar ratio of 30:1, and the reaction is carried out for 4 hours. The product is collected to obtain ethyl difluoroacetate, a pesticide intermediate.

[0045] Comparative Examples 1-8 Compared with Example 3, the difference is that the catalyst is prepared by Comparative Preparation Examples 1-8.

[0046] Test Example 2 The reactions in Examples 1-3 of the present invention and Comparative Examples 1-8 were evaluated, and the results are shown in Table 2.

[0047] Table 2 Group Conversion rate of ethyl difluorochloroacetate (%) Purity of ethyl difluoroacetate (%) Example 1 99.6 97.8 Example 2 99.1 98.2 Example 3 99.8 98.9 Comparative Example 1 88.7 93.2 Comparative Example 2 91.5 91.1 Comparative Example 3 92.8 93.6 Comparative Example 4 90.7 92.8 Comparative Example 5 80.5 88.5 Comparative Example 6 78.2 86.9 Comparative Example 7 89.9 94.1 Comparative Example 8 84.5 90.5 It can be seen from the above table that the methods in Examples 1-3 of the present invention can obtain high-yield and high-purity pesticide intermediate ethyl difluoroacetate products.

[0048] Test Example 3 After the catalysts in Examples 1-3 of the present invention and Comparative Examples 1-8 were continuously catalyzed for 200 hours, reaction evaluation was performed. The results are shown in Table 3.

[0049] Table 3 Group Conversion rate of ethyl difluorochloroacetate (%) Purity of ethyl difluoroacetate (%) Example 1 97.8 96.5 Example 2 97.3 96.9 Example 3 98.2 97.4 Comparative Example 1 86.4 90.5 Comparative Example 2 85.2 88.9 Comparative Example 3 83.9 86.7 Comparative Example 4 82.5 87.4 Comparative Example 5 72.1 84.3 Comparative Example 6 68.9 82.7 Comparative Example 7 75.6 85.7 Comparative Example 8 78.2 83.3 It can be seen from the above table that the catalysts in Examples 1-3 of the present invention still maintain a relatively high catalytic activity after continuously performing the catalytic reaction for 200 hours.

[0050] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a pesticide intermediate ethyl difluoroacetate, characterized in that: The catalyst is placed in a fixed bed, the air is replaced by an inert gas, the temperature is raised, hydrogen and ethyl difluorochloroacetate gas are introduced, the product is collected while the reaction proceeds, and ethyl difluoroacetate, an intermediate of the pesticide, is obtained.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the hydrogen to ethyl chlorodifluoroacetate gas is 25-35:

1.

3. The preparation method according to claim 1, characterized in that: The temperature is raised to 180-190°C.

4. The preparation method according to claim 1, characterized in that: The preparation method of the catalyst is as follows: S1. Preparation of wrinkled nanospheres: Dissolve microcrystalline cellulose, starch and carboxymethyl chitosan in water to form a uniform solution, spray dry and carbonize to obtain wrinkled nanospheres; S2. Preparation of carrier: adding wrinkled nanospheres to ethanol, adding aluminum isopropoxide, tetraethyl orthosilicate and tetrabutyl titanate, stirring and mixing, adding ammonia water to adjust the pH value of the solution, stirring the reaction, centrifuging, washing, drying, and calcining to obtain a carrier; S3. Ni / Cu loading: adding the carrier to water, adding nickel salt and copper salt, stirring for adsorption, evaporating the solvent, washing, and drying to obtain a Ni / Cu loaded catalyst; S4. Regulation of Ca / Mg ions: Add the Ni / Cu loaded catalyst into water, add calcium salt and magnesium salt, heat and stir to react, filter, wash, and dry to obtain a modified Ni / Cu loaded catalyst; S5. La doping: dissolve lanthanum salt in water, add modified Ni / Cu loaded catalyst, impregnate, filter, wash and dry to obtain the catalyst.

5. The preparation method according to claim 4, characterized in that: In step S1, the mass ratio of microcrystalline cellulose, starch and carboxymethyl chitosan is 1-2:7-10:4-6, the carbonization temperature is 750-850° C., and the time is 1-3 h.

6. The preparation method according to claim 4, characterized in that: In step S2, the mass ratio of the wrinkled nanospheres, aluminum isopropoxide, tetraethyl orthosilicate and tetrabutyl titanate is 10:1-2:3-4:1-2, the pH value of the adjusted solution is 9-10, the stirring reaction time is 3-5 hours, the calcination temperature is 300-400°C, and the time is 2-3 hours.

7. The preparation method according to claim 4, characterized in that: The mass ratio of the carrier, nickel salt and copper salt in step S3 is 5:1-2:0.4-0.9, the stirring adsorption time is 0.5-1h, the nickel salt is at least one of nickel chloride, nickel nitrate and nickel sulfate, and the copper salt is at least one of copper chloride, copper sulfate and copper nitrate.

8. The preparation method according to claim 4, characterized in that: The mass ratio of the Ni / Cu loaded catalyst, calcium salt and magnesium salt in step S4 is 100:1-2:0.7-1.2, the temperature of the heating and stirring reaction is 40-50°C, the time is 1-2h, the calcium salt is calcium chloride or calcium nitrate, and the magnesium salt is magnesium chloride, magnesium sulfate or magnesium nitrate.

9. The preparation method according to claim 4, characterized in that: In step S5, the mass ratio of the lanthanum salt to the modified Ni / Cu loaded catalyst is 0.5-1:100, the impregnation time is 3-5h, and the lanthanum salt is lanthanum chloride.

10. The preparation method according to claim 4, characterized in that: The preparation method of the catalyst is specifically as follows: S1. Preparation of wrinkled nanospheres: 1-2 parts by weight of microcrystalline cellulose, 7-10 parts by weight of starch and 4-6 parts by weight of carboxymethyl chitosan are dissolved in water to form a uniform solution, spray dried, and carbonized at 750-850° C. for 1-3 h to obtain wrinkled nanospheres; S2. Preparation of a carrier: 10 parts by weight of wrinkled nanospheres were added to ethanol, 1-2 parts by weight of aluminum isopropoxide, 3-4 parts by weight of ethyl orthosilicate and 1-2 parts by weight of tetrabutyl titanate were added, and the mixture was stirred and mixed uniformly, and ammonia was added dropwise to adjust the pH value of the solution to 9-10, and the reaction was stirred for 3-5 hours, centrifuged, washed, dried, and calcined at 300-400°C for 2-3 hours to obtain a carrier; S3 Ni / Cu loading: 5 parts by weight of the carrier was added to water, 1-2 parts by weight of nickel salt and 0.4-0.9 parts by weight of copper salt were added, and the adsorption was stirred for 0.5-1h, the solvent was evaporated, washed, and dried to obtain a Ni / Cu loaded catalyst; S4. Regulation of Ca / Mg ions: 10 parts by weight of a Ni / Cu-loaded catalyst is added to water, 0.1-0.2 parts by weight of a calcium salt and 0.07-0.12 parts by weight of a magnesium salt are added, heated to 40-50° C., stirred for reaction for 1-2 hours, filtered, washed, and dried to obtain a modified Ni / Cu-loaded catalyst; S5. La doping: 0.05-0.1 parts by weight of lanthanum salt is dissolved in water, 10 parts by weight of modified Ni / Cu loaded catalyst is added, and the mixture is immersed for 3-5 hours, filtered, washed, and dried to obtain a catalyst.