Preparation method and application of covalent organic framework material for converting imine into azo

By converting imine into azo-modified covalent organic frame material, the problems of poor conductivity and insufficient cycle stability in the prior art are solved, and high capacity and stable lithium-ion battery electrode material, Azo-trzn-COF material is realized The specific capacity of 2712mAh/g and good cycle stability were shown in the lithium-ion battery.

CN119039548APending Publication Date: 2024-11-29QUJING NORMAL UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411244659.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing covalent organic frame materials have poor conductivity and high molecular weight in lithium-ion batteries, making it difficult to obtain electrode materials with large capacity, high rate performance and high cycle stability.

Method used

By converting imine (C=N) to azo (N=N), modifying the covalent organic frame material, Azo-trzn-COF material is prepared and applied to the negative electrode material of lithium-ion batteries, improving its electronics Conductivity and electrochemical activity.

Benefits of technology

The specific capacity and cycle stability of the first discharge of lithium-ion batteries are significantly improved, and the Azo-trzn-COF material provides a specific capacity of 2712mAh/g and excellent cycle performance under the same conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039548A_ABST
    Figure CN119039548A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a covalent organic framework material for converting imine into azo and application of the covalent organic framework material. The preparation method comprises the following steps: firstly, dissolving 4 ', 4' '-((1, 3, 5-triazine-2, 4, 6-triyl) tri (oxy) tribenzaldehyde and 1, 4-diaminobenzene in 1, 4-dioxane, then adding m-trimethylbenzene, and uniformly stirring; then adding an acetic acid aqueous solution, and stirring; standing at room temperature, filtering and washing to obtain a product trzn-COF; the preparation method comprises the following steps: adding trzn-COF and DNB into dioxane, water and glacial acetic acid, and heating and standing in a reaction kettle; cooling to room temperature, filtering the mixture, and washing again; sequentially carrying out Soxhlet extraction on the obtained solid by using CHCl3 and tetrahydrofuran so as to prepare a covalent organic framework material Azo-trzn-COF; the invention also discloses application of the covalent organic framework material in preparation of an electrode material. The requirement for synthesis equipment is low, the synthesized covalent organic framework Azo-trzn-COF material is novel and stable in structure, and an electrode material prepared from the material is large in specific discharge capacity and good in stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a preparation method of a covalent organic framework material for converting imine into azo and application thereof. Background Art

[0002] With the reduction of traditional natural resources and the deterioration of the environment, the development of clean and renewable energy has become a top priority. Lithium-ion batteries are the most mature energy storage technology developed in the past decade, but to obtain larger storage capacity, higher energy density and longer cycle life, it is still necessary to find better electrode materials. Organic anode materials with N=N active sites have many attractive properties, such as high conductivity and abundant redox active sites. These materials provide new ideas for the development of advanced organic materials for sustainable, highly conductive and durable rechargeable batteries. Organic electrode materials have the advantages of light molecular weight, easy molecular structure design, fast electron / ion transfer speed, environmental sustainability and material flexibility. They are electrode materials with great development potential in lithium-ion battery systems. By converting imine (C=N) into azo (N=N), the strong π-π interaction between the two-dimensional COF layers significantly improves the electronic conductivity of COF and reduces the solubility of COF in the electrolyte. In addition, the introduction of N=N active sites significantly improves the electrochemical activity and capacity. Due to the improved conductivity, reduced dissolution of electrode materials, and enhanced electrochemical activity, LIBs assembled with Trzn-COF electrodes showed superior capacity output and superior cycling stability compared with those assembled with Trzn-COF electrodes.

[0003] Although there are many covalent organic frameworks reported so far, these materials have some disadvantages, such as few redox active sites, small specific capacitance, easy dissolution in electrolyte, resulting in poor cycle stability, etc. In order to overcome the above disadvantages, many researchers have recently discovered that covalent organic framework materials (COF) have novel structures and excellent stability. They are cleverly constructed by strong covalent bonds and organic building units. However, due to the poor conductivity and large molecular weight of covalent organic polymer materials, there are still many difficulties in obtaining covalent organic framework electrode materials with large capacity, high rate performance and high cycle stability. The present invention proposes a method for converting imine (C=N) into azo (N=N) to modify COF, and the covalent organic framework material is used as a negative electrode material for lithium-ion batteries, showing high specific capacity and cycle stability. At present, in the research on covalent organic framework electrode materials, the research that can be directly used for electrode materials is still very rare, so the research of this patent has good application prospects. Summary of the invention

[0004] In view of the problems mentioned in the background technology, the purpose of the present invention is to provide a lithium ion battery electrode material with high discharge specific capacity and stable cycle performance.

[0005] To achieve the above object, the present invention provides the following solutions: The present invention provides a method for preparing a covalent organic framework material by converting imine into azo, comprising the following steps: S1. Dissolve 4′,4′′-((1,3,5-triazine-2,4,6-triyl)tri(oxy)tribenzaldehyde and 1,4-diaminobenzene in 1,4-dioxane. After they are completely dissolved, add m-trimethylbenzene and stir evenly to obtain solution A. S2, adding acetic acid aqueous solution to the solution A obtained in S1, and then an orange-yellow precipitate appears, and the reaction mixture is stirred for another 5 minutes to obtain a mixture A; S3, the mixture A obtained in S2 was allowed to stand at room temperature for 3 days, filtered, and washed with 1,4-dioxane, methanol, acetone and tetrahydrofuran in sequence to obtain the product trzn-COF; S4, adding the trzn-COF and DNB obtained in S3 to dioxane, water, and glacial acetic acid, placing the mixture in a reaction kettle, heating it at high temperature, and standing it for 3 days to obtain a mixture B; S5, after cooling the mixture B obtained in S4 to room temperature, filtering the mixture B, and washing with NaOH aqueous solution, water, acetone, N, N-dimethylformamide, and tetrahydrofuran in sequence to obtain a solid A; S6. The solid A obtained in S5 is subjected to Soxhlet extraction with CHCl3 and tetrahydrofuran in sequence to prepare a covalent organic framework material Azo-trzn-COF.

[0006] Furthermore, in S1, the molar ratio of 4′,4″-((1,3,5-triazine-2,4,6-triyl)tri(oxy)tribenzaldehyde to 1,4-diaminobenzene is 1:2.

[0007] Furthermore, during the heating process of the reactor of S4, the temperature was heated from room temperature to 80°C at a heating rate of 2°C·min -1 ; Heating rate from 80℃ to 120℃ is 4℃·min -1 , after heating to 120℃, let it stand at constant temperature for 3 days.

[0008] Furthermore, the reaction time of Soxhlet extraction with CHCl3 in S6 is 6 h.

[0009] Furthermore, the reaction time of Soxhlet extraction with tetrahydrofuran in S6 is 6 h.

[0010] The present invention also provides a covalent organic framework material Azo-trzn-COF prepared by a preparation method of a covalent organic framework material which converts imine into azo.

[0011] The present invention also provides application of the covalent organic framework material in the preparation of electrode materials for lithium ion batteries.

[0012] The present invention also provides a method for preparing the electrode material of the lithium ion battery, comprising the following steps: S1, Azo-trzn-COF, PVDF, ks-6, and ECP were prepared into a mixture C in a mass ratio of 6:1:2:1; S2, adding NMP as a solvent to the mixture C, and preparing a lithium ion battery electrode slurry after stirring; S3. Coat the lithium-ion battery electrode slurry on a 12 μm copper foil with a coating thickness of 50 μm, and dry at 100° C. for 12 h to obtain a lithium-ion battery electrode material.

[0013] Beneficial effects of the present invention: The invention has low requirements on synthesis equipment, and the synthesized covalent organic framework Azo-trzn-COF material has a novel and stable structure, and the prepared covalent organic framework material Azo-trzn-COF can be used as a raw material for electrode materials of lithium ion batteries; at 0.01V-3V, at 800 mA g –1 Under the current density of , the assembled LIBs trzn-COF provided an initial discharge specific capacity of 1618 mAh / g. In comparison, Azo-trzn-COF provided an initial discharge specific capacity of 2712 mAh / g, which has a large discharge specific capacity and good stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0015] Figure 1 The schematic diagram of the synthesis of the covalent organic framework material Azo-trzn-COF of the present invention; Figure 2 A schematic diagram of the structure of the covalent organic framework material Azo-trzn-COF of the present invention; Figure 3 XRD patterns of trzn-COF and Azo-trzn-COF electrode materials; Figure 4 TEM images of trzn-COF and Azo-trzn-COF electrode materials Figure 5SEM and EDX element distribution diagrams of trzn-COF and Azo-trzn-COF electrode materials; Figure 6 Thermogravimetric analysis of trzn-COF and Azo-trzn-COF electrode materials; Figure 7 CV curves of trzn-COF and Azo-trzn-COF electrode materials; Figure 8 is the electrochemical impedance of trzn-COF and Azo-trzn-COF electrode materials; Fig. 9 Raman spectra of trzn-COF and Azo-trzn-COF electrode materials; DETAILED DESCRIPTION

[0016] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention. The terms "include", "including", "have", "contain" and the like used herein are open terms, which means including but not limited to. Example 1

[0017] like Figures 1 to 5 As shown, the prior art in this embodiment has the following problems: the inventors found that due to the poor conductivity and large molecular weight of covalent organic polymer materials, there are still many difficulties in obtaining covalent organic framework electrode materials with large capacity, high rate performance and high cycle stability; Therefore, the inventors provide a method for preparing a covalent organic framework material by converting imine into azo, comprising the following steps: S1. Dissolve 4′,4′′-((1,3,5-triazine-2,4,6-triyl)tri(oxy)tribenzaldehyde and 1,4-diaminobenzene in 1,4-dioxane. After they are completely dissolved, add m-trimethylbenzene and stir evenly to obtain solution A. The molar ratio of 4′,4″-((1,3,5-triazine-2,4,6-triyl)tri(oxy)tribenzaldehyde to 1,4-diaminobenzene in S1 is 1:2.

[0018] S2, adding acetic acid aqueous solution to the solution A obtained in S1, and then an orange-yellow precipitate appears, and the reaction mixture is stirred for another 5 minutes to obtain a mixture A; S3, the mixture A obtained in S2 was allowed to stand at room temperature for 3 days, filtered, and washed with 1,4-dioxane, methanol, acetone and tetrahydrofuran in sequence to obtain the product trzn-COF; S4, adding the trzn-COF and DNB obtained in S3 to dioxane, water, and glacial acetic acid, placing the mixture in a reaction kettle, heating it at high temperature, and standing it for 3 days to obtain a mixture B; During the heating process of the reactor of S4, the temperature was heated from room temperature to 80°C at a heating rate of 2°C·min -1 ; Heating rate from 80℃ to 120℃ is 4℃·min -1 , after heating to 120℃, let it stand at constant temperature for 3 days.

[0019] S5, after cooling the mixture B obtained in S4 to room temperature, filtering the mixture B, and washing with NaOH aqueous solution, water, acetone, N, N-dimethylformamide, and tetrahydrofuran in sequence to obtain a solid A; S6. The solid A obtained in S5 is subjected to Soxhlet extraction with CHCl3 and tetrahydrofuran in sequence to prepare a covalent organic framework material Azo-trzn-COF.

[0020] Among them, the reaction time of Soxhlet extraction with CHCl3 in S6 is 6 h.

[0021] The reaction time of Soxhlet extraction with tetrahydrofuran in S6 is 6 h.

[0022] The present invention also provides a covalent organic framework material Azo-trzn-COF prepared by a preparation method of a covalent organic framework material which converts imine into azo.

[0023] The present invention also provides application of the covalent organic framework material in the preparation of electrode materials for lithium ion batteries.

[0024] The present invention also provides a method for preparing the electrode material of the lithium ion battery, comprising the following steps: S1, Azo-trzn-COF, PVDF, ks-6, and ECP were prepared into a mixture C in a mass ratio of 6:1:2:1; S2, adding NMP as a solvent to the mixture C, and preparing a lithium ion battery electrode slurry after stirring; S3. Coat the lithium-ion battery electrode slurry on a 12 μm copper foil with a coating thickness of 50 μm, and dry at 100° C. for 12 h to obtain a lithium-ion battery electrode material. Example 2

[0025] Based on the above embodiments, the inventors conducted the following experiments: 4′,4′′-((1,3,5-triazine-2,4,6-triyl)tri(oxy)tribenzaldehyde (800 mg) and 1,4-diaminobenzene (384 mg) were dissolved in 1,4-dioxane (40.0 mL). After complete dissolution, m-trimethylbenzene (40.0 mL) was added and stirred evenly. Then, about 4.0 mL of acetic acid aqueous solution (3 M) was added. An orange-yellow precipitate began to appear immediately. Subsequently, the reaction mixture was stirred for another 5 minutes. It was allowed to stand at room temperature for 3 days. After filtration, the product was washed with 1,4-dioxane, methanol, acetone and tetrahydrofuran in sequence. Trzn-COF (500 mg) and DNB (690 mg) were added to dioxane (40 ml), water (10 ml), glacial acetic acid (2.5 ml), and allowed to stand at 120 ° C for 3 days. After cooling to room temperature, the mixture was filtered and washed with NaOH aqueous solution (1 M), water, acetone, N, The solid was washed with N-dimethylformamide and tetrahydrofuran in turn. The solid was extracted with CHCl3 and tetrahydrofuran for 12 h, respectively, to obtain Azo-trzn-COF as a red powder.

[0026] Azo-trzn-COF, PVDF, ks-6, and ECP were prepared into a mixture in a mass ratio of 6:1:2:1, NMP was added as a solvent, and the mixture was stirred to prepare a lithium-ion battery electrode slurry. The lithium-ion battery electrode slurry was coated on a 12μm copper foil with a coating thickness of 50μm, and dried at 100°C for 12h to obtain a lithium-ion battery electrode. The negative electrode of the lithium-ion battery was cut into a circular electrode with a diameter of 12mm, and the lithium-ion battery counter electrode used a metal lithium sheet with a diameter of 15mm. The electrolyte was: 1mol / L LiTFSI containing 2% LiNO3 was dissolved in a solvent of dimethyl ether (DME) and 1,3-dioxolane (DOL) (molar ratio DME:DOL=1:1 Vol%), and assembled into a 2032 button cell in a glove box filled with argon.

[0027] The structures of the synthesized trzn-COF and Azo-trzn-COF materials were characterized. Figure 2 and Figure 3 It can be seen that the structure of the Azo-trzn-COF obtained in this embodiment is similar to that of the theoretical simulation, indicating that the target product is obtained. TEM results show that the Azo-trzn-COF material has a grid-like interior and a sheet-like interlayer. The Azo-trzn-COF material synthesized by SEM morphology analysis and EDX energy spectrum analysis has a layered microporous structure, which is tightly bound inside and contains C, N, and O elements.

[0028] The thermal stability of trzn-COF and Azo-trzn-COF was studied by thermogravimetric analysis (TGA), and obvious weight loss was observed after 313°C, indicating that they have high thermal stability. Figure 6 It is shown that at room temperature, the Azo-trzn-COF electrode was subjected to cyclic voltammetry (CV) measurements in the voltage range of 0.01-3.0V (scan rate of 0.1mv / s). During the negative scan of the first cycle, the CV curve showed a cathode peak, corresponding to a multi-step Li intercalation process, followed by the electrochemical reduction of Azo-trzn-COF. During the positive scan, the anodic peak corresponds to the reversible oxidation of the active groups in Azo-trzn-COF. In the following cycles, the CV curves almost overlap, indicating the highly reversible reaction and excellent cycle stability of Azo-trzn-COF based on lithium-ion batteries. Figure 7 It shows that electrochemical impedance spectroscopy (EIS) tests were carried out on trzn-COF and Azo-trzn-COF. Each impedance spectrum consists of a semicircle in the high-frequency region and a slash in the low-frequency range, which respectively obtain the electron transfer resistance (RET) and Warburg impedance. The semicircle of the Azo-trzn-COF electrode and the uncycled trzn-COF in the high-medium frequency region decreases, and the charge transfer impedance decreases. The slash in the low-frequency region is caused by the warbug impedance of the ions on the electrode. By comparison, it is found that the angle of the low-frequency curve of the Azo-trzn-COF electrode is smaller, which is caused by the increasing diffusion impedance when the ions in the electrolyte diffuse to the surface of the Azo-trzn-COF electrode. Fig. 9 The Raman spectra of trzn-COF and Azo-trzn-COF were compared and it was found that the imine (1628 cm −1 ) disappears, the azo bond (1441 cm −1 ) appears, indicating that the imine is converted into an azo compound. Comparison of the spectra of trzn-COF converted to Azo-trzn-COF revealed that the imine bond (1628 cm −1 ) disappears, the azo bond (1441 cm −1 ) exists, indicating that key conversion has been achieved.

[0029] and at 0.01V-3V, at 800 mA g –1 Under the current density of , the assembled LIBs trzn-COF provided an initial discharge specific capacity of 1618 mAh / g. In comparison, the electrode material with Azo-trzn-COF as raw material provided an initial discharge specific capacity of 2712 mAh / g. It has a large discharge specific capacity and good stability.

[0030] It can be seen from the above embodiments that the present invention has low requirements for synthesis equipment, the synthesized covalent organic framework Azo-trzn-COF material has a novel and stable structure, and the prepared covalent organic framework material Azo-trzn-COF can be used as a raw material for electrode materials of lithium-ion batteries; under the same conditions, its discharge specific capacity is large and its stability is good.

[0031] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a covalent organic framework material by converting imine into azo, characterized in that: The following steps are involved: S1. Dissolve 4′,4′′-((1,3,5-triazine-2,4,6-triyl)tri(oxy)tribenzaldehyde and 1,4-diaminobenzene in 1,4-dioxane. After they are completely dissolved, add m-trimethylbenzene and stir evenly to obtain solution A. S2, adding acetic acid aqueous solution to the solution A obtained in S1, and then an orange-yellow precipitate appears, and the reaction mixture is stirred for another 5 minutes to obtain a mixture A; S3, the mixture A obtained in S2 was allowed to stand at room temperature for 3 days, filtered, and washed with 1,4-dioxane, methanol, acetone and tetrahydrofuran in sequence to obtain the product trzn-COF; S4, adding the trzn-COF and DNB obtained in S3 to dioxane, water, and glacial acetic acid, placing the mixture in a reaction kettle, heating it at high temperature, and standing it for 3 days to obtain a mixture B; S5, after cooling the mixture B obtained in S4 to room temperature, filtering the mixture B, and washing with NaOH aqueous solution, water, acetone, N, N-dimethylformamide, and tetrahydrofuran in sequence to obtain solid A; S6. The solid A obtained in S5 is subjected to Soxhlet extraction with CHCl3 and tetrahydrofuran in sequence to prepare a covalent organic framework material Azo-trzn-COF.

2. The method for preparing a covalent organic framework material for converting imine into azo according to claim 1, characterized in that: The molar ratio of 4′,4″-((1,3,5-triazine-2,4,6-triyl)tri(oxy)tribenzaldehyde to 1,4-diaminobenzene in S1 is 1:

2.

3. The method for preparing a covalent organic framework material for converting imine into azo according to claim 1, characterized in that: During the heating process of the reactor of S4, the temperature was heated from room temperature to 80°C at a heating rate of 2°C·min -1 ; Heating from 80℃ to 120℃ at a heating rate of 4℃·min -1 , after heating to 120℃, let it stand at constant temperature for 3 days.

4. The method for preparing a covalent organic framework material for converting imine into azo according to claim 1, characterized in that: The reaction time of Soxhlet extraction with CHCl3 in S6 is 6 h.

5. The method for preparing a covalent organic framework material for converting imine into azo according to claim 1, characterized in that: The reaction time of Soxhlet extraction with tetrahydrofuran in S6 is 6 h.

6. The covalent organic framework material according to any one of claims 1 to 5, characterized in that: The covalent organic framework material Azo-trzn-COF is prepared by the method for preparing the covalent organic framework material by converting imine into azo.

7. Use of the covalent organic framework material according to claim 6 in the preparation of electrode materials for lithium-ion batteries.

8. The method for preparing an electrode material for a lithium ion battery according to claim 7, characterized in that: The following steps are involved: S1, Azo-trzn-COF, PVDF, ks-6, and ECP were prepared into a mixture C in a mass ratio of 6:1:2:1; S2, adding NMP as a solvent to the mixture C, and preparing a lithium ion battery electrode slurry after stirring; S3. Coating the lithium-ion battery electrode slurry on a 12 μm copper foil with a coating thickness of 50 μm, and drying at 100° C. for 12 h to obtain a lithium-ion battery electrode material.

Citation Information

Cited By

  • Nitrogen heterocyclic covalent organic framework material as well as preparation method and application thereof

    CN119931038A

  • Azo polymer fiber electrode and fiber battery application

    CN120015830A

  • An azo polymer fiber electrode and its application in fiber batteries

    CN120015830B