Method for inhibiting thermal degradation of polylactic acid
Modified polylactic acid is prepared by combining L-lactide and thiodecafluoroctyl trihydroxysilane, which solves the problem of thermal degradation and preparation process of polylactic acid, and achieves thermal stability and fluidity at high temperatures promote.
Patent Information
- Application Number
- CN202411310092.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-29
AI Technical Summary
Polylactic acid has a fast thermal degradation rate at high temperatures, a complex preparation process and poor dispersion of additives, which limits its application in the field of heat resistance.
Modified polylactic acid is prepared by reaction and twin screw extrusion after vacuum drying, and siloxane and fluorine elements are introduced by the combination of L-lactide and thirty-degree fluoride catalyst. , enhance molecular structural stability and fluidity.
The melt temperature and fluidity of polylactic acid are improved, the thermal stability and fluidity of its high temperature are enhanced, thermal degradation is avoided, and the preparation process is simplified.
Smart Images

Figure BDA0005050388280000051 
Figure BDA0005050388280000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a method for inhibiting thermal degradation of polylactic acid. Background Art
[0002] Polylactic acid is a new type of biodegradable material, made from starch raw materials from renewable plant resources. Starch raw materials are saccharified to obtain glucose, which is then fermented with glucose and certain strains of bacteria to produce high-purity lactic acid, which is then synthesized into polylactic acid of a certain molecular weight through chemical synthesis. It has good biodegradability and can be completely degraded by microorganisms in nature after use, eventually generating carbon dioxide and water, without polluting the environment. It is a recognized environmentally friendly material.
[0003] Polylactic acid is sensitive to heat and has poor thermal stability, which greatly limits the application of polylactic acid in fields with high heat resistance requirements. Polylactic acid requires good melt fluidity during the spinning process, but for heat-sensitive polylactic acid, although increasing the spinning temperature can improve fluidity, it is also very easy to cause thermal degradation. Thermal oxygen stabilizers are usually used to modify the heat resistance of polylactic acid. However, the intermolecular force between thermal oxygen stabilizers and polylactic acid is weak, resulting in poor dispersibility in polylactic acid copolymer resins.
[0004] Copolymerization modification of polylactic acid can make it have a variety of excellent properties. The Chinese patent application with publication number CN117430792A discloses a polylactic acid-poly-ε-caprolactone block copolymer and its preparation method and application. By mixing lactide, initiator, and catalyst, removing the monomer after step-by-step polymerization, the obtained copolymer has higher toughness and thermodynamic stability, but its preparation process is cumbersome and not suitable for continuous production in industry. The Chinese patent application with publication number CN117659654A discloses a polylactic acid composition and its application in melt-blown spinning. By adding iodate and siloxane to polylactic acid, the molten fluid temperature of the polylactic acid composition is effectively increased to improve the fluidity of polylactic acid. However, after the temperature rises to 220°C, the degradation rate of polylactic acid is greatly accelerated. Therefore, providing a polylactic acid with a simple preparation process and melt having both fluidity and heat resistance is a technical problem that needs to be solved at present. Summary of the invention
[0005] In order to solve the technical problems mentioned in the background technology that the preparation process of polylactic acid copolymer is complicated, the auxiliary agent is unevenly dispersed in the polylactic acid copolymer resin, and the thermal degradation rate of polylactic acid is fast at high temperature, the present invention provides a method for inhibiting the thermal degradation of polylactic acid.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for inhibiting thermal degradation of polylactic acid comprises the following steps:
[0008] Step 1: prepare the following raw materials by weight: 100 parts of L-lactide, 1-2 parts of terminal hydroxyl fluorinated silane, 0.1-0.5 parts of tin-containing catalyst, and 0.1-0.5 parts of thermal oxidation stabilizer;
[0009] The second step is to add the above raw materials into the reactor according to weight, react at a temperature of 150-190°C and a pressure of 1-3MPa for 2-6h, then transfer to a vacuum drying oven with a vacuum degree of -0.1MPa and vacuum dry at 80°C for 10h, remove the monomer, and granulate through twin-screw extrusion to obtain modified polylactic acid.
[0010] Furthermore, the terminal hydroxyl fluorine-containing silane is tridecafluorooctyltrihydroxysilane.
[0011] Further, tridecafluorooctyl trihydroxysilane is prepared by the following steps:
[0012] Add tridecafluorooctyltrimethoxysilane and a rotor to a three-necked flask, raise the temperature to 100°C, add deionized water dropwise, and react at a constant temperature for 2 hours. After the reaction is completed, perform reduced pressure distillation at 2.67 KPa and 80°C for 3 hours to remove low-boiling substances to obtain tridecafluorooctyltrihydroxysilane.
[0013] Furthermore, the tin salt catalyst includes any one of stannous octoate and stannous chloride, or a complex of the two.
[0014] Furthermore, the thermal oxidation stabilizer includes one or more of antioxidant 1010, antioxidant 1076, and antioxidant 2246.
[0015] Furthermore, the amount ratio of the added amount of deionized water to the added amount of tridecafluorooctyltrimethoxysilane is 2:1.
[0016] Furthermore, the temperature for removing the monomer is 150-180° C., the vacuum pressure is 50-180 Pa, and the time is 1-2 hours.
[0017] Beneficial effects of the present invention:
[0018] In order to increase the melt temperature of polylactic acid and thus improve the melt fluidity. The present invention uses L-lactide and tridecafluorooctyl trihydroxysilane as base materials, tin salt as a catalyst, and a thermal oxygen stabilizer as an auxiliary agent to improve the heat resistance of a polylactic acid melt. Tridecafluorooctyl trihydroxysilane is the base material after hydrolysis modification treatment of the present invention, and the terminal hydroxyl group contained in the tridecafluorooctyl trihydroxysilane can undergo a condensation reaction with the carboxyl group after depolymerization of L-lactide, thereby achieving the purpose of introducing siloxane and fluorine elements into the polylactic acid at the same time. The silicon-oxygen bond (SiO) has an extremely high bond energy, which makes the entire molecular structure very stable. This stability makes siloxane difficult to decompose or deteriorate at high temperatures, thereby showing excellent heat resistance. The introduction of fluorine atoms enhances the interaction between polymer chains, hinders the movement of chain segments, and further improves the thermal stability of the material. In addition, the special structure of SiO makes the internal friction between molecules smaller, showing higher fluidity. As the temperature increases, the thermal motion of the siloxane molecules intensifies, and the interaction force between the molecules weakens, thereby resulting in reduced viscosity and enhanced fluidity. In summary, the polylactic acid prepared by the present invention is not easy to be thermally degraded at high temperatures while maintaining high fluidity. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1
[0021] A method for inhibiting thermal degradation of polylactic acid comprises the following steps:
[0022] Step 1: prepare the following raw materials by weight: 100 parts of L-lactide, 1 part of tridecafluorooctyl trihydroxysilane, 0.1 parts of stannous chloride, and 0.1 parts of antioxidant 1010;
[0023] In the second step, the above raw materials are added into the reactor according to weight parts, reacted at a temperature of 150°C and a pressure of 1MPa for 6 hours, then transferred to a vacuum drying oven with a vacuum degree of -0.1MPa and vacuum drying at 80°C for 10 hours, and the monomers are removed at 150°C and a vacuum pressure of 50Pa for 2 hours, and then extruded and granulated at 190°C by a twin-screw to obtain modified polylactic acid. The melt index and thermal degradation rate are tested and the results are listed in Table 1 below.
[0024] Tridecafluorooctyl trihydroxysilane is prepared by the following steps:
[0025] Add tridecafluorooctyltrimethoxysilane and a rotor to a three-necked flask, heat the oil bath to a reaction material temperature of 100°C, add deionized water in an amount twice that of tridecafluorooctyltrimethoxysilane dropwise, and react at a constant temperature for 2 hours. After the reaction is completed, perform reduced pressure distillation at 2.67 KPa and 80°C for 3 hours to remove low-boiling substances to obtain tridecafluorooctyltrihydroxysilane.
[0026] Example 2
[0027] A method for inhibiting thermal degradation of polylactic acid comprises the following steps:
[0028] Step 1: prepare the following raw materials by weight: 100 parts of L-lactide, 1.5 parts of tridecafluorooctyl trihydroxysilane, 0.3 parts of stannous octoate, and 0.3 parts of antioxidant 1076;
[0029] In the second step, the above raw materials are added into the reactor according to weight parts, reacted at a temperature of 170°C and a pressure of 2MPa for 4 hours, then transferred to a vacuum drying oven with a vacuum degree of -0.1MPa and vacuum drying at 80°C for 10 hours, and the monomers are removed at 165°C and a vacuum pressure of 115Pa for 1.5 hours, and then extruded and granulated at 190°C by a twin-screw to obtain modified polylactic acid. The melt index and thermal degradation rate are tested and the results are listed in Table 1 below.
[0030] The preparation process of tridecafluorooctyltrihydroxysilane is the same as that in Example 1.
[0031] Example 3
[0032] A method for inhibiting thermal degradation of polylactic acid comprises the following steps:
[0033] Step 1: prepare the following raw materials by weight: 100 parts of L-lactide, 2 parts of tridecafluorooctyl trihydroxysilane, 0.5 parts of stannous chloride, and 0.5 parts of antioxidant 2246;
[0034] In the second step, the above raw materials are added into the reactor according to weight parts, reacted at a temperature of 190°C and a pressure of 3MPa for 2h, then transferred to a vacuum drying oven with a vacuum degree of -0.1MPa and vacuum drying at 80°C for 10h, and the monomers are removed at 180°C and a vacuum pressure of 180Pa for 1h, and then extruded and granulated at 190°C by a twin-screw to obtain modified polylactic acid. The melt index and thermal degradation rate are tested and the results are listed in Table 1 below.
[0035] The preparation process of tridecafluorooctyltrihydroxysilane is the same as that in Example 1.
[0036] Comparative Example 1
[0037] The tridecafluorooctyl trihydroxysilane in Example 1 was removed, and the remaining raw materials and preparation process were the same as in Example 1 to obtain polylactic acid. The melt index and thermal degradation rate of polylactic acid were tested and the results are listed in Table 1 below.
[0038] Comparative Example 2
[0039] The antioxidant 1076 in Example 2 was removed, and the remaining raw materials and preparation process were the same as in Example 2 to obtain polylactic acid. The melt index and thermal degradation rate of polylactic acid were tested and the results are listed in Table 1 below.
[0040] Comparative Example 3
[0041] The tridecafluorooctyl trihydroxysilane in Example 1 was replaced by terminal hydroxymethyl silane, and the remaining raw materials and preparation process were the same as Example 1 to obtain polylactic acid. The melt index and thermal degradation rate of the polylactic acid were tested and the results are listed in Table 1 below.
[0042] Hydroxyl-terminated methyl silane is prepared by the following steps:
[0043] Add dimethoxymethylsilane and rotor to a three-necked flask equipped with a condenser, thermometer and nitrogen protection device, heat the oil bath to a reaction material temperature of 100°C, add deionized water in an amount twice that of dimethoxymethylsilane dropwise, and react at a constant temperature for 2 hours. After the reaction is completed, perform reduced pressure distillation at 2.67 KPa and 80°C for 3 hours to remove low-boiling substances to obtain terminal hydroxymethylsilane.
[0044] The polylactic acid obtained in Examples 1 to 3 and Comparative Examples 1 to 3 was subjected to melt index and thermal degradation rate performance tests. The melt index was measured at 190° C. and 220° C., 2.16 kg, respectively, according to ASTM D1238. The thermal degradation rate was measured by TGA at 200° C. and 220° C., respectively, under a nitrogen atmosphere. The results are shown in Table 1:
[0045] Table 1
[0046]
[0047]
[0048] It can be seen from Table 1 that when dimethoxymethylsilane is introduced into the raw material, the melt index (MI) of polylactic acid is improved and the degradation rate of polylactic acid at a high temperature of 220°C is inhibited. If tridecafluorooctyl trihydroxysilane is selected as the raw material, the performance will be further improved. If the raw material does not contain a thermal oxygen stabilizer, the melt index decreases and the degradation rate accelerates, indicating that the one-pot polymerization effectively solves the problem of uniform dispersion of the additives in the polylactic acid copolymer resin.
[0049] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for inhibiting thermal degradation of polylactic acid, characterized in that: The following steps are involved: 100 parts of L-lactide, 1-2 parts of terminal hydroxyl fluorinated silane, 0.1-0.5 parts of tin salt catalyst and 0.1-0.5 parts of thermal oxidation stabilizer are added into a reaction kettle by weight, and reacted at a temperature of 150-190°C and a pressure of 1-3MPa for 2-6h, and then transferred to a vacuum drying oven with a vacuum degree of -0.1MPa and vacuum dried at 80°C for 10h, and then the monomer is removed, and extrusion granulation is performed to obtain modified polylactic acid.
2. The method for inhibiting thermal degradation of polylactic acid according to claim 1, characterized in that: The terminal hydroxyl fluorinated silane is tridecafluorooctyl trihydroxysilane.
3. The method for inhibiting thermal degradation of polylactic acid according to claim 2, characterized in that: Tridecafluorooctyl trihydroxysilane is prepared by the following steps: Add tridecafluorooctyltrimethoxysilane and a rotor to a three-necked flask, raise the temperature to 100°C, add deionized water dropwise, and react at a constant temperature for 2 hours. After the reaction is completed, perform reduced pressure distillation at 2.67 KPa and 80°C for 3 hours to remove low-boiling substances to obtain tridecafluorooctyltrihydroxysilane.
4. The method for inhibiting thermal degradation of polylactic acid according to claim 1, characterized in that: The tin salt catalyst includes any one of stannous octoate and stannous chloride or a complex of the two.
5. The method for inhibiting thermal degradation of polylactic acid according to claim 1, characterized in that: The thermal oxidation stabilizer includes any one or more of antioxidant 1010 , antioxidant 1076 , and antioxidant 2246 .
6. The method for inhibiting thermal degradation of polylactic acid according to claim 3, characterized in that: The molar ratio of the amount of deionized water added to the amount of tridecafluorooctyltrimethoxysilane added is 2:
1.
7. The method for inhibiting thermal degradation of polylactic acid according to claim 1, characterized in that: The temperature for removing the monomer is 150-180°C, the vacuum pressure is 50-180Pa, and the time is 1-2h.
8. The method for inhibiting thermal degradation of polylactic acid according to claim 1, characterized in that: The twin-screw granulation temperature is 190°C.
Citation Information
Patent Citations
Polylactic acid-poly (epsilon-caprolactone) block copolymer as well as preparation method and application thereof
CN117430792A
Polylactic acid composition and application thereof in melt-blown spinning
CN117659654A