High-air-permeability and moisture-permeability protective film material with spongy communicated network structure and preparation method of protective film material
By adopting the synergistic effect of the sponge-like communication network structure and fluoropolymer in the preparation of microporous membranes, the problems of poor breathability and moisture permeability in the prior art are solved, and the high breathability, moisture permeability and liquid barrier properties are improved. , improves the wear comfort and work efficiency of protective clothing.
Patent Information
- Application Number
- CN202411284107.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The prior art ignores the breathability and moisture permeability of the material when preparing microporous membranes, resulting in the long-term wearing of protective clothing with poor breathability and moisture permeability, which will lead to moisture and heat accumulation, causing skin allergies, heat stroke and even fainting, and at the same time increase fatigue. Reduce work efficiency.
The preparation method of high breathable and moisture-permeable protective film material is adopted for the sponge-shaped communication network structure. By preparing hygroscopic inorganic salts, polymers and fluoropolymers into cast film liquid, the phase conversion is carried out in a solidification bath after scraping and coating. A spongy microporous membrane with high specific surface area and high porosity was formed. Combined with hydrophobic finishing agent and spraying treatment of nanoparticles, a microporous membrane with excellent breathable, moisture permeable and liquid barrier properties were prepared.
It has achieved significant improvements in the high breathability, moisture permeability and liquid barrier properties of the material, improved wear comfort and work efficiency, and met the practical application needs in the field of individual protection.
Smart Images

Figure CN119039657A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a highly breathable and moisture-permeable protective film material with a sponge-like interconnected network structure and a preparation method thereof, belonging to the technical field of micro-nano protective materials. Background Art
[0002] Breathable and moisture-permeable protective films have great potential in the field of personal protection and play a vital role in protecting life and health. With the improvement of quality of life and hygiene level, the demand for safe and comfortable protective fabrics continues to increase. In addition to good protective performance, medical protective materials must also have excellent breathability and moisture permeability to ensure the comfort of the wearer. In the past few decades, medical protective clothing has made great progress in protection, breathability, and thermal and moisture comfort. However, the key balance between protective ability and wearing comfort has been largely overlooked, which is closely related not only to the comfort of medical staff, but also to their work efficiency.
[0003] At present, medical protective clothing with excellent barrier properties can be produced by weaving, knitting and non-woven technologies. Woven fabric surface chemical finishing or additional barrier film is widely used in reusable medical clothing due to its simple production process and high cost-effectiveness. The non-solvent induced phase separation (NIPS) membrane preparation method is an efficient membrane preparation method invented in the 1960s. The asymmetric membrane structure prepared by this method has good selective permeability and easy to adjust the pore structure. It has become a common method for the research and commercial production of polymer coating membranes. The use of inorganic salts as pore-forming agents can accurately control the pore size and porosity of the material, and the chemical properties are stable and not easy to react adversely with other materials, ensuring the purity and performance of the porous material. In addition, inorganic salts are soluble in water and can be removed by simple water washing during post-treatment to avoid the influence of residual pore-forming agents on material properties.
[0004] Patent CN112918056B discloses a method for preparing a waterproof and breathable membrane, wherein the waterproof and breathable membrane comprises a medical non-woven fabric, a hydrophilic breathable membrane and an antibacterial waterproof membrane, wherein the antibacterial waterproof membrane and the medical non-woven fabric are respectively attached to the upper surface and the lower surface of the hydrophilic breathable membrane. In order to improve wearing comfort, a medical non-woven fabric is added to the inner side of the hydrophilic breathable membrane to avoid the occurrence of the adhesion phenomenon, but this has a certain impact on the breathability of the membrane, and the improvement of the breathability is not obvious enough.
[0005] Patent CN111019332B discloses a method for preparing a polyurethane waterproof and breathable membrane, wherein the waterproof and breathable membrane is mainly made of polyurethane resin, pore-forming agent, inorganic filler and organic solvent. The surface of the polyurethane waterproof and breathable membrane is formed by dry method, and has good breathability. However, the membrane prepared by this technology does not form a connected pore structure, is insufficient in air permeability, and has no ability to block other liquids (such as oil, synthetic blood and alcohol).
[0006] Patent CN107556715B discloses a waterproof and breathable membrane and its preparation method. The raw materials used are biomass materials, which are renewable resources, reducing the dependence on non-renewable petroleum resources, and polyester has good biodegradability. In order to meet the needs of environmental protection, the pore size of the waterproof and breathable membrane made by this method is small, which limits its application in outdoor protection.
[0007] Patent CN113430676B discloses a micro-nano fiber for medical protection and its preparation method. First, PP, polar polymer and additives are mixed in an extruder for melt mixing and plasticization, and granulation is performed to prepare PP alloy particles; then supercritical CO2 is used for dissolution and infiltration to obtain a PP alloy / supercritical fluid homogeneous system; finally, melt electrospinning is used to prepare a multi-level structure, low resistance, and high-efficiency PP composite micro-nano fiber membrane. This method replaces solution electrospinning with safe and green melt electrospinning, avoiding the use of toxic and harmful organic solvents in the spinning process.
[0008] However, the current phase separation method for preparing microporous membranes ignores the air permeability and moisture permeability of the material. Long-term wearing of protective clothing with poor air permeability and moisture permeability can lead to moisture and heat accumulation, causing skin allergies, heat stroke, and even syncope, while increasing fatigue and reducing work efficiency. Therefore, optimizing the bulk structure of the membrane material to improve the material's air permeability and moisture permeability, while improving the material's liquid barrier performance, is of great significance for practical applications in the field of personal protection. Summary of the invention
[0009] The purpose of the present invention is: to address the deficiencies in the prior art, the present invention provides a highly breathable and moisture permeable protective membrane material with a sponge-like interconnected network structure and a method for preparing the same, and specifically provides a phase inversion technology that is applicable to a wide range of polymer raw materials and can prepare a stable sponge-like interconnected network structure microporous membrane without a template. The microporous membrane prepared by this method has excellent breathable and moisture permeability and liquid barrier properties.
[0010] In order to achieve the above object, the present invention provides a method for preparing a sponge-like interconnected network structure highly breathable and moisture permeable protective film material, comprising the following steps:
[0011] Step 1: preparing a casting solution by preparing a hygroscopic inorganic salt, a polymer, a fluorine-containing polymer and a solvent;
[0012] Step 2: Scrape the casting solution onto the substrate to form a film to obtain an initial wet film;
[0013] Step 3: immersing the initial wet membrane obtained in step 2 into a coagulation bath for phase inversion to obtain a microporous membrane having a sponge-like interconnected network structure;
[0014] Step 4: Mix the hydrophobic finishing agent and nanoparticles to prepare a spraying liquid, spray it on the microporous membrane obtained in step 3, and dry it.
[0015] In the above preparation method, the selection of hygroscopic inorganic salts to mix with polymers is conducive to phase inversion pore formation. First, since the coagulation bath used in the phase inversion process is mainly composed of water, the solubility of inorganic salts makes it easier to form micron pores; secondly, although the hygroscopic inorganic salts will dissolve during the preparation process, their ionic form after being dissolved in water can promote the transformation and also change the properties of the material, thereby improving the moisture permeability. In addition, the size of the inorganic salt is adjustable during the conversion process, and those skilled in the art can adjust the corresponding size of micron or nanometer inorganic salts according to needs; the dissolution process of the inorganic salt in the solvent and water can be adjusted, and an excess of inorganic salt is more likely to form micron pores, while a small amount of inorganic salt is more likely to form nanopores.
[0016] In the above preparation method, a hygroscopic inorganic salt is added to the casting liquid. The hygroscopic inorganic salt usually has good solubility and can be dissolved and carried out during phase transformation in the aqueous coagulation bath to form a microporous membrane with a micro-nano porous structure. The self-assembly of the microporous membrane will obtain a sponge-like microporous membrane material with high specific surface area and high porosity. The additional capillary force generated by the structural characteristics of high specific surface area and high porosity is expected to increase its moisture absorption rate and greatly increase its contact area with the air, thereby enhancing the material's moisture permeability as well as the water diffusion rate and drying rate, thereby giving the material excellent air permeability and moisture permeability.
[0017] In addition, the introduction of fluorine-containing polymers in the above-mentioned preparation method changes the bulk properties of the casting liquid. The introduction of carbon-fluorine bonds with extremely high bond energy, combined with the "shielding protection effect" of fluorine atoms on carbon atoms, significantly improves the thermal stability, liquid repellency and chemical corrosion resistance of the polymer. In addition, fluorine atoms have extremely strong electronegativity and small atomic radius. The introduction of fluorine atoms into polymer molecules can achieve fine-tuning and modification of the molecular structure, block the sites where inorganic salts are easily soluble, and improve the dissolution pathway and speed of the molecules. At the same time, the hydrogen bonding between molecules can effectively delay the action time of inorganic salts in the phase transformation process, improve the molecular utilization and selectivity of the polymer solution in the phase transformation process, induce phase change and solidification of the solution, and promote its rapid self-assembly to form a sponge-like structure.
[0018] Preferably, the hygroscopic inorganic salt in step 1 is selected from at least one of an inorganic magnesium salt, an inorganic calcium salt, an inorganic sodium salt, an inorganic potassium salt, an inorganic copper salt and an inorganic ammonium salt;
[0019] The solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, chloroform, tetrahydrofuran, N-methylpyrrolidone, chloroform, methanol, ethanol, isopropanol, deionized water, acetone, dichloromethane, formic acid, acetic acid, dimethyl sulfoxide, ether, toluene, trichloroacetic acid and trifluoroacetic acid.
[0020] More preferably, the hygroscopic inorganic salt is selected from at least one of calcium chloride, magnesium chloride, potassium chloride, sodium sulfate, sodium chloride, copper sulfate, calcium oxide, ammonium sulfate, sodium hypochlorite and sodium hydroxide.
[0021] Preferably, the polymer in step 1 is selected from at least one of polyurethane, thermoplastic polyurethane, polyvinylidene fluoride, polyethylene, polyacrylonitrile, polystyrene, polycaprolactone, polyamide 6, polyamide 66, polyimide and polyethylene terephthalate;
[0022] The fluorine-containing polymer is at least one of fluorinated polyurethane (FPU), fluorinated polycarbonate (FPC), fluorinated acrylate (FAA) polymer, perfluoropolyether (PFPE), fluorinated polyester (FPET), fluorinated polyarylether (FPSF), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer (PFA), chlorotrifluoroethylene-ethylene copolymer (ECTFE), polychlorotrifluoroethylene (PCTFE), perfluorosulfonic acid (PFSA), fluorinated polyimide (FPI), perfluoro-2,2-dimethyl-1,3-dioxacyclopentene-tetrafluoroethylene (PDD-TFE) copolymer, chlorotrifluoroethylene-vinyl ether copolymer (FEVE), polyperfluoroethylene-propylene (FEP), polyvinyl fluoride (PVF) and tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (THV).
[0023] Preferably, in the casting solution obtained in step 1, the mass content of the polymer is 8-20%, the mass fraction ratio of the polymer to the hygroscopic inorganic salt is 9:1-5:5, and the mass content of the fluorine-containing polymer is 1-10%;
[0024] The viscosity of the casting liquid is 1 to 10 Pa·s. In the preparation method of the present invention, the viscosity of the prepared casting liquid is relatively low, which is more conducive to the conversion of the casting liquid phase into pores, which is different from the traditional non-solvent phase separation technology. The viscosity of the casting liquid is jointly adjusted by the molecular weight of the polymer and the type of inorganic salt. Adding CaCl2 to the casting liquid will reduce the viscosity of the solution, while adding LiCl will increase the viscosity of the casting liquid. Therefore, those skilled in the art can select polymers with suitable molecular weights and corresponding inorganic salt types according to the viscosity parameters.
[0025] The reason why the present invention controls the "viscosity range of the casting liquid to be 1 to 10 Pa·s" is that: the bulk property (viscosity) of the casting liquid is a necessary condition for the formation of the pore structure; if the casting liquid has a high viscosity, compared with a low-viscosity solution, the high-viscosity casting liquid has a high solvent content and high intermolecular friction, so it is more difficult to diffuse the solvent and the non-solvent in the same non-solvent coagulation bath, that is, the solution is easy to solidify, which is not conducive to the self-assembly molding of the pore structure and is not easy to produce a sponge-like network structure.
[0026] Preferably, the method for preparing the casting solution in step 1 comprises:
[0027] A hygroscopic inorganic salt is added to a solvent, and the mixture is continuously stirred at room temperature. Then, a polymer and a fluorine-containing polymer are added in sequence, and the mixture is continuously stirred at room temperature to obtain a uniform initial casting solution.
[0028] More preferably, the continuous stirring time is 2 to 20 hours, and the continued stirring time is 10 to 20 hours.
[0029] Preferably, the substrate in step 2 is selected from at least one of woven fabrics, knitted fabrics, non-woven fabrics and electrospun fiber membranes.
[0030] Preferably, the thickness of the film formed by scraping in step 2 is 100 to 2500 μm.
[0031] Preferably, the temperature of the coagulation bath in step 3 is 20-60° C., and the phase inversion time is 0.5-2 h.
[0032] Preferably, the coagulation bath is at least one of water, a mixture of water and ethanol, and a mixture of water and DMF.
[0033] The reason why the present invention controls the film-laying process parameters of the casting liquid "film-laying thickness 100-2500 μm, coagulation bath temperature 20-60° C., phase transformation time 0.5-2 h" is because: it determines whether a sponge-like structure can be formed. If the film-laying thickness is too high, it will be difficult for the casting liquid to form connected channels during the transformation process within the same transformation time; the coagulation bath temperature affects the sponge-like shape; if the coagulation bath temperature is too low, it will be unfavorable for rapid molding during the transformation process; if the coagulation bath temperature is too high, the polymer properties will be unstable, thereby increasing the instability of the phase transformation and affecting the formation of the pore structure; the change in the phase transformation time affects the pore-forming effect; if the time is too short, the transformation time will be insufficient, the inorganic salt will not be sufficiently dissolved, the pore-forming effect will be poor, and ultimately the material will have poor air permeability; if the transformation time is too long, it will lead to waste of resources.
[0034] Preferably, the hydrophobic finishing agent in step 4 is a liquid, selected from at least one of fluorine-containing compounds (such as perfluoropolyether compounds PFPE), silicone resins (such as polydimethylsiloxane), fluorosilicone polymers (such as fluorosilicone acrylate copolymers), fluorocarbon polymers (such as polyperfluoropropylene) and Teflon.
[0035] The nanoparticles are selected from at least one of hydrophobic nano-silicon dioxide, metal oxides (such as at least one of zinc oxide, titanium dioxide, copper oxide and iron oxide) and metal nanoparticles (such as silver nanoparticles and / or gold nanoparticles).
[0036] Preferably, the mass content of the nanoparticles in the spraying liquid in step 4 is 1-15%.
[0037] The present invention also provides a highly breathable and moisture-permeable protective film material having a sponge-like interconnected network structure prepared by the above-mentioned preparation method.
[0038] The protective film material prepared by the present invention has vertically connected pores and a horizontally dense micro-nanopore structure with an average pore size of 1 to 15 μm. The microporous film has a large specific surface area and porosity, with a specific surface area of more than 10 m 2 / g, porosity>70%.
[0039] The reason why the protective film material prepared by the present invention has excellent air permeability, moisture permeability and reverse liquid penetration barrier performance is that: the protective film material prepared by the present invention has a sponge-like connected network structure in the vertical direction, forms a pore size gradient with the substrate in the thickness direction, and has an additional differential capillary effect, which enables moisture to be quickly and directional transmitted in the thickness direction. Therefore, the coordinated regulation of the connected channels and the gradient pore structure in the present invention significantly improves the air permeability and moisture permeability of the material; at the same time, the micro-nano pore structure in the horizontal direction and the addition of fluorine-containing polymers, due to the dense small pore structure and capillary resistance, the water transfer is hindered, thereby realizing the material's barrier to liquids.
[0040] The present invention also provides the use of the above-mentioned sponge-like interconnected network structure highly breathable and moisture-permeable protective film material in the preparation of medical protective equipment.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] (1) Different from the traditional non-solvent phase separation method for preparing microporous membranes, in the preparation method of the present invention, the addition of hygroscopic inorganic salts makes the casting solution highly soluble, and the solubility of the inorganic salts makes it easier to form a polymer-poor phase. The solubility and the competition between the solvent and the non-solvent diffusion induce the self-assembly of the sponge-like interconnected network structure, thereby realizing the controllable preparation of highly breathable and moisture-permeable membrane materials;
[0043] (2) Different from the traditional non-solvent phase separation method for preparing microporous membranes, in the preparation method of the present invention, the addition of fluorine-containing polymers increases the carbon-fluorine bond content of the casting solution, increases the electronegativity of the wet membrane during the phase transformation process, utilizes the aggregation of fluorine atoms to form, blocks the easily soluble sites of inorganic salts, improves the dissolution path and speed of molecules, and achieves liquid repellency and chemical corrosion resistance of the membrane material;
[0044] (3) The membrane materials prepared by the existing non-solvent phase conversion technology ignore the air permeability and moisture permeability of the materials, resulting in poor wearing comfort and low work efficiency during use. The present invention introduces micron-sized inorganic salts and fluorine-containing polymers to synergistically prepare a micro-nano interconnected network structure, which maintains the protective performance while taking into account the high air permeability and high moisture permeability of the material to meet the actual application needs in the field of personal protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a surface electron microscope image of a protective film with a sponge-like interconnected network pore structure with high air and moisture permeability.
[0046] Figure 2 This is a cross-sectional electron microscope image of a protective film with a sponge-like interconnected network pore structure that has high air and moisture permeability.
[0047] Figure 3 The contact angles of water, synthetic blood, oil and ethanol aqueous solution within 300s of the sponge-like interconnected network pore structure protective film.
[0048] Figure 4 The air permeability and moisture permeability of the sponge-like interconnected network pore structure protective film are compared with those of commercial protective products. DETAILED DESCRIPTION
[0049] In order to make the present invention more clearly understood, preferred embodiments are described in detail below with reference to the accompanying drawings.
[0050] Unless otherwise specified, the materials, reagents, etc. used in the following examples are conventional commercially available products.
[0051] Example 1
[0052] A method for preparing a highly breathable and moisture permeable protective film material having a sponge-like interconnected network structure, the specific steps of which are as follows:
[0053] Step 1: Dissolve the pore-forming agent CaCl2 in N,N-dimethylformamide, stir at room temperature for 6 hours until completely dissolved, and then add polyurethane (PU, M W 50,000 to 100,000) and different mass fractions of fluorinated polyurethane (FPU, Shanghai Taifu, product number: QF99-4) were stirred under constant magnetic stirring at room temperature for 10 hours to obtain a uniform PU / FPU / CaCl2 casting solution.
[0054] Step 2: Pour the casting liquid obtained in step 1 onto the woven fabric substrate, and use a coating applicator to scrape the casting liquid onto the substrate. The solution volume of the casting liquid is controlled to be 9 mL, and the thickness of the coating applicator is selected to be 250 μm to obtain a PU / FPU / CaCl2 wet film.
[0055] Step 3: The wet film of step 2 is immediately immersed in a water coagulation bath for 3 hours for phase inversion, and a porous PU / FPU framework is deposited. Subsequently, it is washed with ultrapure water and dried at 60°C to finally obtain a microporous membrane with a micro-nano network pore structure.
[0056] Step 4: The microporous membrane prepared in step 3 was then sprayed using a 1 mm caliber gravity-fed spray gun with an operating pressure of 4 Bar, a spray distance of 20 cm, and a spray gun flow rate of 30 mL min -1 A highly permeable protective microporous membrane PU / FPU@TRG was obtained. The spraying liquid components are fluorine-based water- and oil-repellent finishing agent (three-proof finishing agent TRG, Shanghai Xinwu Textile Technology Co., Ltd.) and hydrophobic nano-silica (CAS No.: 68611-44-9, Shanghai McLean Biochemical Technology Co., Ltd.), and the amount of silica added is 5wt%.
[0057] Thus, the sponge-like interconnected network structure highly breathable and moisture permeable protective film material is obtained, with a tensile breaking strength of 65.56 MPa, a water pressure resistance of 12.86 kPa, a water contact angle of 131°, a synthetic blood contact angle of 126°, an oil contact angle of 104°, and an ethanol-water contact angle of 85°. Figure 3 The sponge-like interconnected micro-nanoscale network pore channels in the microporous membrane are conducive to the rapid transmission of gas and moisture molecules. Compared with commercial protective clothing, it has excellent gas and moisture permeability, with an air permeability of 14.24 mm s -1 , moisture permeability is 7.92kg m -2 d -1 ,like Figure 4 shown.
[0058] Example 2
[0059] Step 1: Same as step 1 in Example 1, except that the pore-forming agent is MgCl2.
[0060] Step 2: Same as step 2 in Example 1.
[0061] Step 3: Same as step 3 in Example 1.
[0062] Step 4: Same as step 4 in Example 1.
[0063] The obtained sponge-like interconnected network structure highly breathable and moisture permeable protective membrane material has a tensile strength of 62.42Mpa, a water pressure resistance of 12.12kPa, a water contact angle of 130°, a synthetic blood contact angle of 124°, an oil contact angle of 102°, and an ethanol-water contact angle of 81°. The sponge-like interconnected micro-nanoscale network pore channels in the microporous membrane are conducive to the rapid transmission of gas and moisture molecules, and the air permeability is 14.69mm s -1 , moisture permeability is 7.64kg m -2 d -1 .
[0064] Example 3
[0065] Step 1: Same as step 1 in Example 1, except that the pore-forming agent is KCl.
[0066] Step 2: Same as step 2 in Example 1.
[0067] Step 3: Same as step 3 in Example 1.
[0068] Step 4: Same as step 4 in Example 1.
[0069] The obtained sponge-like interconnected network structure highly breathable and moisture permeable protective membrane material has a tensile strength of 64.01 MPa, a water pressure resistance of 12.06 kPa, a water contact angle of 133°, a synthetic blood contact angle of 128°, an oil contact angle of 105°, and an ethanol-water contact angle of 89°. The sponge-like interconnected micro-nanoscale network pore channels in the microporous membrane are conducive to the rapid transmission of gas and moisture molecules, and the air permeability is 14.54 mm s -1 , moisture permeability is 7.82kg m -2 d -1 .
[0070] Example 4
[0071] Step 1: Same as step 1 in Example 1, except that the pore-forming agent is KCl.
[0072] Step 2: Same as step 2 in Example 1.
[0073] Step 3: Same as step 3 in Example 1.
[0074] Step 4: Same as step 4 in Example 1.
[0075] The obtained sponge-like interconnected network structure highly breathable and moisture permeable protective membrane material has a tensile strength of 62.56 MPa, a water pressure resistance of 11.67 kPa, a water contact angle of 132°, a synthetic blood contact angle of 128°, an oil contact angle of 103°, and an ethanol-water contact angle of 85°. The sponge-like interconnected micro-nanoscale network pore channels in the microporous membrane are conducive to the rapid transmission of gas and moisture molecules, and the air permeability is 14.96 mm s -1 , moisture permeability is 7.76kg m -2 d -1 .
[0076] Example 5
[0077] Step 1: The same as step 1 in Example 1, except that the fluorine-containing polymer is polyvinylidene fluoride.
[0078] Step 2: Same as step 2 in Example 1.
[0079] Step 3: Same as step 3 in Example 1.
[0080] Step 4: Same as step 4 in Example 1.
[0081] The obtained sponge-like interconnected network structure highly breathable and moisture permeable protective membrane material has a tensile strength of 60.21Mpa, a water pressure resistance of 13.96kPa, a water contact angle of 140°, a synthetic blood contact angle of 132°, an oil contact angle of 114°, and an ethanol-water contact angle of 94°. The sponge-like interconnected micro-nanoscale network pore channels in the microporous membrane are conducive to the rapid transmission of gas and moisture molecules, and the air permeability is 15.266mm s -1 , moisture permeability is 8.21kg m -2 d -1 .
[0082] Example 6
[0083] Step 1: The same as step 1 in Example 1, except that the fluorine-containing polymer is fluorine-containing polycarbonate.
[0084] Step 2: Same as step 2 in Example 1.
[0085] Step 3: Same as step 3 in Example 1.
[0086] Step 4: Same as step 4 in Example 1.
[0087] The obtained sponge-like interconnected network structure highly breathable and moisture permeable protective membrane material has a tensile strength of 58.46Mpa, a water pressure resistance of 13.41kPa, a water contact angle of 138°, a synthetic blood contact angle of 128°, an oil contact angle of 110°, and an ethanol-water contact angle of 98°. The sponge-like interconnected micro-nanoscale network pore channels in the microporous membrane are conducive to the rapid transmission of gas and moisture molecules, and the air permeability is 14.62mm s -1 , moisture permeability is 9.67kg m -2 d -1 .
[0088] Example 7
[0089] Step 1: The same as step 1 in Example 1, except that the fluorine-containing polymer is a fluorine-containing acrylic resin.
[0090] Step 2: Same as step 2 in Example 1.
[0091] Step 3: Same as step 3 in Example 1.
[0092] Step 4: Same as step 4 in Example 1.
[0093] The obtained sponge-like interconnected network structure highly breathable and moisture permeable protective membrane material has a tensile strength of 56.62Mpa, a water pressure resistance of 12.74kPa, a water contact angle of 137°, a synthetic blood contact angle of 125°, an oil contact angle of 109°, and an ethanol-water contact angle of 95°. The sponge-like interconnected micro-nanoscale network pore channels in the microporous membrane are conducive to the rapid transmission of gas and moisture molecules, and the air permeability is 14.52mm s -1 , moisture permeability is 8.66kg m -2 d -1 .
[0094] The above description is only a preferred embodiment of the present invention and is not any formal or substantial limitation of the present invention. It should be pointed out that a person skilled in the art can make several improvements and supplements without departing from the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a highly breathable and moisture permeable protective film material having a sponge-like interconnected network structure, characterized in that: The following steps are involved: Step 1: preparing a casting solution by preparing a hygroscopic inorganic salt, a polymer, a fluorine-containing polymer and a solvent; Step 2: Scrape the casting solution onto the substrate to form a film to obtain an initial wet film; Step 3: immersing the initial wet membrane obtained in step 2 into a coagulation bath for phase inversion to obtain a microporous membrane having a sponge-like interconnected network structure; Step 4: Mix the hydrophobic finishing agent and nanoparticles to prepare a spraying liquid, spray it on the microporous membrane obtained in step 3, and dry it.
2. The preparation method according to claim 1, characterized in that The hygroscopic inorganic salt in step 1 is selected from at least one of an inorganic magnesium salt, an inorganic calcium salt, an inorganic sodium salt, an inorganic potassium salt, an inorganic copper salt and an inorganic ammonium salt; The solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, chloroform, tetrahydrofuran, N-methylpyrrolidone, chloroform, methanol, ethanol, isopropanol, deionized water, acetone, dichloromethane, formic acid, acetic acid, dimethyl sulfoxide, ether, toluene, trichloroacetic acid and trifluoroacetic acid.
3. The preparation method according to claim 1, characterized in that: The polymer in step 1 is selected from at least one of polyurethane, thermoplastic polyurethane, polyvinylidene fluoride, polyethylene, polyacrylonitrile, polystyrene, polycaprolactone, polyamide 6, polyamide 66, polyimide and polyethylene terephthalate; The fluorine-containing polymer is selected from at least one of fluorinated polyurethane (FPU), fluorinated polycarbonate (FPC), fluorinated acrylate (FAA) polymer resin, perfluoropolyether (PFPE), fluorinated polyester (FPET), fluorinated polyarylether (FPSF), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer (PFA), trifluorochloroethylene-ethylene copolymer (ECTFE), polytrifluorochloroethylene (PCTFE), perfluorosulfonic acid (PFSA), fluorinated polyimide (FPI), perfluoro-2,2-dimethyl-1,3-dioxacyclopentene-tetrafluoroethylene (PDD-TFE) copolymer, trifluorochloroethylene-vinyl ether copolymer (FEVE), polyperfluoroethylene propylene (FEP), polyvinyl fluoride (PVF) and tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (THV).
4. The preparation method according to claim 1, characterized in that: In the casting solution obtained in step 1, the mass content of the polymer is 8-20%, the mass fraction ratio of the polymer to the hygroscopic inorganic salt is 9:1-5:5, and the mass content of the fluorine-containing polymer is 1-10%; The viscosity of the casting solution is 1-10 Pa·s.
5. The preparation method according to claim 1, characterized in that: The substrate in step 2 is selected from at least one of woven fabrics, knitted fabrics, non-woven fabrics and electrospun fiber membranes. And / or, the thickness of the film formed by scraping in step 2 is 100 to 2500 μm.
6. The preparation method according to claim 1, characterized in that: In step 3, the temperature of the coagulation bath is 20 to 60° C., and the phase inversion time is 0.5 to 2 hours; The coagulation bath is at least one of water, a mixture of water and ethanol, and a mixture of water and DMF.
7. The preparation method according to claim 1, characterized in that: The hydrophobic finishing agent in step 4 is selected from at least one of fluorine-containing compounds, silicone resins, fluorosilicone polymers, fluorocarbon polymers and Teflon; The nanoparticles are selected from at least one of hydrophobic nano-silicon dioxide, metal oxides, and metal nanoparticles.
8. The preparation method according to claim 1, characterized in that: The mass content of the nanoparticles in the spraying liquid of step 4 is 1-15%.
9. A sponge-like interconnected network structure highly breathable and moisture permeable protective membrane material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the highly breathable and moisture permeable protective film material with a sponge-like interconnected network structure as claimed in claim 9 in the preparation of medical protective equipment.
Citation Information
Patent Citations
Manufacture method of polyvinyl chloride panel ultrafiltration membrane
CN102743980A
Method for preparing super-hydrophobic micro-porous membrane by synergistic regulation and control phase separation of inorganic salt aqueous solution
CN107519767A
Hydrophobic membrane with micro-nano-structure surface functional layer and preparation method thereof
CN107970789A
Nano self cleaning silk broadcloth and products
CN1563555A
Oil, water and sweat repellent microporous membrane materials
US5260360A
Cited By
Preparation method of high-frequency flexible copper-clad plate
CN121038113A
Pressure compensation element (PCE) comprising a c2-, c3- or c4-fluoropolymer- or -copolymer-coated membrane