High-temperature energy-saving infrared heat radiation coating and preparation method thereof

By optimizing the formulation and preparation process of high-temperature energy-saving infrared thermal radiation coatings, the problems of poor heat resistance and production complexity of existing coatings in high-temperature environments are solved, and high infrared emissivity and thermal shock stability are achieved. It is suitable for high-temperature industrial equipment , improves equipment efficiency and energy efficiency.

CN119039811APending Publication Date: 2024-11-29ZHENGZHOU ZHENFA NEW MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411364035.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-28
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing high-temperature infrared thermal radiation coatings have poor heat resistance in high-temperature environments, are prone to cracking or peeling, and have complex production processes, which limit their application and economic benefits in high-temperature and frequent temperature changes.

Method used

Using high-temperature energy-saving infrared thermal radiation coating formula, including wollastonite fiber, ceramic fiber, aluminum silicate cotton, sepiol velvet, iron oxide, silica sol, bentonite powder, dispersant and defoaming agent, through drying screening, surface The steps of processing, adding liquid components and powder components, and adding additives are prepared to improve the infrared emissivity and thermal shock stability of the coating.

Benefits of technology

It significantly improves the infrared emissivity and thermal shock stability of the coating, prevents the coating from cracking due to concentrated thermal stress, extends its service life, is suitable for high-temperature industrial equipment, and improves the operating efficiency and energy efficiency of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of thermal radiation coatings, in particular to a high-temperature energy-saving infrared thermal radiation coating and a preparation method thereof.The high-temperature energy-saving infrared thermal radiation coating is prepared from, by mass, 35-45 parts of wollastonite fiber, 5-15 parts of ceramic fiber, 5-10 parts of aluminum silicate wool, 5-10 parts of sepiolite fabric, 5-15 parts of ferric oxide and 12-18 parts of silica sol. 5-10 parts of a thickening agent, 0.7-3 parts of a dispersing agent and 0.5-2 parts of a defoaming agent; according to the high-temperature energy-saving infrared heat radiation coating, the formula and the preparation process of the coating are improved, the prepared coating has extremely high infrared emissivity, meanwhile, the thermal shock resistance and the heat resistance are greatly improved, and the thermal shock resistance and the heat resistance are greatly improved in actual use compared with infrared heat radiation coatings in the prior art; according to the present invention, the coating material can be effectively prevented from cracking or peeling due to thermal stress concentration during the actual application, and can be prevented from cracking due to excessive thermal stress during the rapid heating and cooling process, such that the high stability and the long service life can be provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of thermal radiation coatings, and in particular relates to a high-temperature energy-saving infrared thermal radiation coating and a preparation method thereof. Background Art

[0002] With the rapid development of my country's economy, people's demand for energy is increasing. Due to my country's large population and lower per capita energy consumption than developed countries, energy shortage has become one of the important factors restricting economic development. The main energy-consuming equipment in my country's high-energy-consuming industrial system is industrial kilns, which account for about 25% to 40% of the total energy consumption. In industrial kilns, when the internal temperature reaches 1000℃, heat transfer is mainly achieved through thermal radiation, and thermal radiation heat transfer can account for more than 90% of the total heat transfer. However, when the working temperature of general kiln refractory materials reaches above 1000℃, the emissivity will drop significantly to below 0.4, affecting the thermal efficiency of industrial kilns and causing energy waste.

[0003] Infrared thermal radiation coating is a high-efficiency energy-saving material used in industrial kilns. It can be sprayed on the heating surface of the furnace body of various kilns to form a dense coating with a thickness of 0.2~0.4mm. With its large infrared radiation rate, it strengthens the thermal radiation intensity in the furnace, allowing the fuel to burn fully, reducing heat loss and greatly improving the thermal efficiency of the furnace. my country started late in the research of infrared thermal radiation coatings. At present, the more mature infrared thermal radiation coatings are mostly used in medium and low temperatures below 1200℃. There is still a lack of application of infrared thermal radiation coatings for high-temperature industrial kilns working above 1200℃.

[0004] The existing high-temperature infrared thermal radiation coating has poor high-temperature resistance in actual use. The coating may crack or peel due to concentrated thermal stress in a high-temperature environment, and the coating may crack due to excessive thermal stress during rapid temperature rise and fall. This limits the application of the coating in high-temperature and frequent temperature change environments; at the same time, the raw material production process of high-temperature infrared thermal radiation coating is complicated, which makes the economic benefits of infrared thermal radiation coating relatively poor, limiting its promotion in large-scale industrial applications. Therefore, how to overcome the above-mentioned technical problems and defects has become a key issue that needs to be solved. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects described in the background technology, so as to realize a high-temperature energy-saving infrared thermal radiation coating to solve the problems of high impurity content (especially CaO content), low load softening temperature, low refractoriness and poor thermal shock resistance of tin bath top cover bricks in the prior art.

[0006] In order to achieve the above-mentioned object of the invention, the technical solution of the present invention is: A high-temperature energy-saving infrared thermal radiation coating, comprising the following components in parts by mass: 35-45 parts of wollastonite fiber, 5-15 parts of ceramic fiber, 5-10 parts of aluminum silicate wool, 5-10 parts of sepiolite wool, 5-15 parts of iron oxide, 12-18 parts of silica sol, 5-10 parts of thickener, 0.7-3 parts of dispersant, and 0.5-2 parts of defoamer.

[0007] In the above-mentioned high-temperature energy-saving infrared heat radiation coating, the thickener is bentonite powder, the dispersant is sodium tripolyphosphate, and the defoamer is polyether-modified silicone oil.

[0008] In the above-mentioned high-temperature energy-saving infrared thermal radiation coating, preferably, the high-temperature energy-saving infrared thermal radiation coating includes the following components in parts by mass: 40 parts of wollastonite fiber, 15 parts of ceramic fiber, 5 parts of aluminum silicate wool, 5 parts of sepiolite wool, 10 parts of iron oxide, 15 parts of silica sol, 8 parts of bentonite powder, 1 part of sodium tripolyphosphate, and 1 part of polyether modified silicone oil.

[0009] In the above-mentioned high-temperature energy-saving infrared thermal radiation coating, preferably, the high-temperature energy-saving infrared thermal radiation coating includes the following components in parts by mass: 45 parts of wollastonite fiber, 10 parts of ceramic fiber, 10 parts of aluminum silicate wool, 5 parts of sepiolite wool, 5 parts of iron oxide, 15 parts of silica sol, 8 parts of bentonite powder, 1 part of sodium tripolyphosphate, and 1 part of polyether modified silicone oil.

[0010] In the above-mentioned high-temperature energy-saving infrared thermal radiation coating, preferably, the high-temperature energy-saving infrared thermal radiation coating includes the following components in parts by mass: 35 parts of wollastonite fiber, 5 parts of ceramic fiber, 10 parts of aluminum silicate wool, 10 parts of sepiolite wool, 15 parts of iron oxide, 15 parts of silica sol, 8 parts of bentonite powder, 1 part of sodium tripolyphosphate, and 1 part of polyether modified silicone oil.

[0011] The present invention also discloses a method for preparing the above-mentioned high-temperature energy-saving infrared heat radiation coating, and the preparation method comprises: Step 1: Drying and screening; Place the powder raw materials such as wollastonite fiber, ceramic fiber, aluminum silicate wool, and sepiolite wool in a drying oven and dry them at 80-100°C for 2-4 hours to remove moisture from the raw materials. After drying, use a 180-250 mesh screen to screen the dried raw materials to ensure uniform particle size.

[0012] Step 2: Surface treatment: Stir the iron oxide at 70-80°C, add a surfactant solution, and continue stirring for 1.5-2h. The surfactant is a silane coupling agent, and the amount added is 2%-3% of the mass of the iron oxide.

[0013] Step 3: Add liquid ingredients; add silica sol, bentonite powder and water into a stirring kettle, set the initial stirring speed to 150-200 rpm, and continue stirring for 8-10 minutes until the mixture is evenly mixed.

[0014] Step 4: Add powder components; gradually add pretreated wollastonite fiber, ceramic fiber, aluminum silicate wool, sepiolite wool and iron oxide in small amounts several times, with each addition amount being 10%-20% of the total powder amount. Each time the added powder is fully mixed with the liquid, add the powder again.

[0015] During the addition process, gradually increase the stirring speed from 150-200rpm to 400-600rpm within 5-10min, and continue stirring for 40-60min to ensure that the powder and liquid components are fully mixed.

[0016] Step 5: Adding additives; add dispersant and defoamer to the mixture obtained in step 4, and continue stirring at a stirring speed of 600-800 rpm for 20-30 minutes to obtain the coating.

[0017] Compared with the prior art, the high temperature energy-saving infrared heat radiation coating of the present invention has at least the following beneficial effects: The high-temperature energy-saving infrared thermal radiation coating of the present invention is improved through the coating formula and preparation process. The obtained coating has extremely high infrared emissivity, and at the same time greatly improves thermal shock stability and heat resistance. In actual use, it has greatly improved compared with the infrared thermal radiation coating in the prior art. It can effectively prevent the coating from cracking or peeling due to concentrated thermal stress during actual use, and prevent the coating from cracking due to excessive thermal stress during rapid heating and cooling. It has strong stability and a long service life.

[0018] The high-temperature energy-saving infrared thermal radiation coating with the above weight percentage components is prepared by the above steps, which has many advantages in high strength, high temperature resistance, heat insulation, infrared radiation, chemical stability, good thixotropy, strong crack resistance and environmental protection in high temperature environment. It is particularly suitable for various industrial equipment and pipelines that need to work under high temperature conditions and require high efficiency and energy saving. It can not only improve the operating efficiency of the equipment, but also extend the service life of the equipment and reduce energy consumption, which meets the requirements of modern industry for high efficiency, environmental protection and economy. DETAILED DESCRIPTION

[0019] The high temperature energy-saving infrared heat radiation coating of the present invention is described in more detail below through specific implementation methods. Example 1

[0020] This embodiment discloses a high-temperature energy-saving infrared heat radiation coating, which is used to solve the problems of high impurity content (especially CaO content), low load softening temperature, low refractoriness and poor thermal shock resistance of tin bath roof bricks in the prior art. In this embodiment, the high-temperature energy-saving infrared heat radiation coating comprises the following components in parts by mass: 35-45 parts of wollastonite fiber, 5-15 parts of ceramic fiber, 5-10 parts of aluminum silicate wool, 5-10 parts of sepiolite wool, 5-15 parts of iron oxide, 12-18 parts of silica sol, 5-10 parts of thickener, 0.7-3 parts of dispersant, and 0.5-2 parts of defoamer.

[0021] In this embodiment, the addition of wollastonite fiber, ceramic fiber and aluminum silicate wool can improve the high temperature resistance and mechanical strength of the coating, so that the coating can maintain its physical and chemical properties in a high temperature environment. At the same time, iron oxide, as a highly efficient infrared radiation material, can absorb and re-radiate heat, thereby enhancing the energy-saving effect of the coating. The use of silica sol as a binder enhances the adhesion of the coating, allowing it to firmly adhere to the substrate.

[0022] The thickener described in this embodiment is bentonite powder, the dispersant is sodium tripolyphosphate, and the defoaming agent is polyether modified silicone oil.

[0023] Specifically, the high-temperature energy-saving infrared thermal radiation coating includes the following components in parts by mass. In this embodiment, 45 parts of wollastonite fiber, 10 parts of ceramic fiber, 10 parts of aluminum silicate wool, 5 parts of sepiolite wool, 5 parts of iron oxide, 15 parts of silica sol, 8 parts of bentonite powder, 1 part of sodium tripolyphosphate, and 1 part of polyether modified silicone oil.

[0024] By adding a high proportion of wollastonite fiber and aluminum silicate wool content, the obtained coating performs better in thermal insulation and mechanical strength. Adding a high content of aluminum silicate wool makes the obtained coating have better thermal insulation effect, which is suitable for high-temperature equipment with high strength and good thermal insulation performance, such as industrial furnace linings, high-temperature pipelines, etc.

[0025] This embodiment also discloses a method for preparing the high-temperature energy-saving infrared heat radiation coating of the above weight percentage components, comprising the following steps: Step 1: Drying and screening; Place the powder raw materials such as wollastonite fiber, ceramic fiber, aluminum silicate wool, and sepiolite wool in a drying oven and dry them at 80-100°C for 2-4 hours to remove moisture from the raw materials. After drying, use a 180-250 mesh screen to screen the dried raw materials to ensure uniform particle size.

[0026] Step 2: Surface treatment: Stir the iron oxide at 70-80°C, add a surfactant solution, and continue stirring for 1.5-2h. The surfactant is a silane coupling agent, and the amount added is 2%-3% of the mass of the iron oxide.

[0027] Step 3: Add liquid ingredients; add silica sol, bentonite powder and water into a stirring kettle, set the initial stirring speed to 150-200 rpm, and continue stirring for 8-10 minutes until the mixture is evenly mixed.

[0028] Step 4: Add powder components; gradually add pretreated wollastonite fiber, ceramic fiber, aluminum silicate wool, sepiolite wool and iron oxide in small amounts several times, with each addition amount being 10%-20% of the total powder amount. Each time the added powder is fully mixed with the liquid, add the powder again.

[0029] During the addition process, gradually increase the stirring speed from 150-200rpm to 400-600rpm within 5-10min, and continue stirring for 40-60min to ensure that the powder and liquid components are fully mixed.

[0030] Step 5: Adding additives; add dispersant and defoamer to the mixture obtained in step 4, and continue stirring at a stirring speed of 600-800 rpm for 20-30 minutes to obtain the coating.

[0031] The high-temperature energy-saving infrared thermal radiation coating with the above weight percentage components is prepared by the above steps, which achieves the advantages of high strength, high temperature resistance, heat insulation, infrared radiation, chemical stability, good thixotropy, strong crack resistance and environmental protection in high temperature environment. It is particularly suitable for various industrial equipment and pipelines that need to work under high temperature conditions and require high efficiency and energy saving, such as industrial furnace linings, high-temperature pipelines, heating furnaces, heat treatment equipment, etc. that require rapid heating. The high-temperature energy-saving infrared thermal radiation coating with the above weight percentage components is prepared by the above steps, which can not only improve the operating efficiency of the equipment, but also extend the service life of the equipment and reduce energy consumption, which meets the requirements of modern industry for high efficiency, environmental protection and economy. Example 2

[0032] The same points as the above embodiment will not be repeated here, but the difference is that: In this embodiment, the high-temperature energy-saving infrared thermal radiation coating is measured in mass percentage. The high-temperature energy-saving infrared thermal radiation coating includes the following components, measured in mass parts: 35 parts of wollastonite fiber, 5 parts of ceramic fiber, 10 parts of aluminum silicate wool, 10 parts of sepiolite wool, 15 parts of iron oxide, 15 parts of silica sol, 8 parts of bentonite powder, 1 part of sodium tripolyphosphate, and 1 part of polyether modified silicone oil.

[0033] Compared with Example 1, in this example, the content of wollastonite fiber and ceramic fiber is reduced, and the content of sepiolite wool and iron oxide is increased. The high content of iron oxide can effectively improve the infrared radiation ability of the coating, accelerate the heat dissipation of the surface of the object, reduce heat accumulation, and improve thermal efficiency, thereby contributing to energy conservation and emission reduction. At the same time, the high content of sepiolite wool helps to improve the thixotropy and stability of the coating, while the polyether-modified silicone oil improves the fluidity and construction properties of the coating, making it smoother and more uniform when spraying or brushing, facilitating construction, and improving construction efficiency and quality.

[0034] The high-temperature energy-saving infrared heat radiation coating prepared by the above weight percentage components has a slightly lower heat insulation than that of Example 1, but has a higher heat radiation efficiency and is suitable for occasions requiring rapid heating, such as industrial furnaces, paint booths, etc. Example 3

[0035] The same points as the above embodiment will not be repeated here, but the difference is that: In this embodiment, the high-temperature energy-saving infrared thermal radiation coating includes the following components in parts by mass: 40 parts of wollastonite fiber, 12 parts of ceramic fiber, 8 parts of aluminum silicate wool, 5 parts of sepiolite wool, 10 parts of iron oxide, 15 parts of silica sol, 8 parts of bentonite powder, 1 part of sodium tripolyphosphate, and 1 part of polyether modified silicone oil.

[0036] Compared with Example 1 and Example 2, in this embodiment, the content of wollastonite fiber, ceramic fiber and iron oxide is balanced on the basis of ensuring the overall strength. At the same time, it can effectively dissipate heat without affecting other performance indicators due to excessive iron oxide. The coating made of the above-mentioned mass percentage components has reached a good balance in terms of coating strength, thermal insulation performance, infrared radiation performance, fire resistance, etc., and the performance in all aspects is relatively balanced.

[0037] The coating made of the above mass percentage components has a relatively balanced ratio of each component, which is conducive to the overall optimization of material performance and has good comprehensive performance. Through reasonable component ratio, it has achieved a good balance in mechanical strength, thermal insulation performance, infrared radiation performance and chemical stability, and is suitable for application scenarios that require comprehensive performance. It can not only meet the thermal insulation and mechanical strength requirements of medium-temperature industrial equipment, but also play its comprehensive performance advantages in occasions such as building insulation layers. It is suitable for medium-temperature industrial equipment that needs to balance mechanical strength and thermal insulation performance, such as medium-temperature heating furnaces, heat exchangers, etc.

[0038] In summary, the following Table 1 is obtained: Element Example 1 Example 2 Example 3 Wollastonite fiber (parts) 45 35 38 Ceramic fiber (parts) 10 5 12 Aluminum silicate wool (parts) 10 10 8 Sepiolite (part) 5 10 8 Iron oxide (parts) 5 15 12 Silica sol (parts) 15 15 13 Bentonite powder (parts) 8 8 7 Tripolyphosphate (parts) 1 1 1 Polyether modified silicone oil (parts) 1 1 1 According to the performance test of the high-temperature energy-saving infrared heat radiation coatings prepared by the multiple groups of embodiments in Table 1 above, the following Table 2 is obtained after the test: From Table 1 and Table 2 above, we can conclude that: The high-temperature energy-saving infrared thermal radiation coating made by the components of Examples 1, 2, and 3 can effectively improve the infrared emissivity compared to the prior art, while greatly improving the thermal shock stability and heat resistance. It can be seen that the component contents of Examples 1, 2, and 3 are more reasonable, and Example 3 is the best example.

[0039] In addition, it should be noted that the preparation ingredients of Examples 1, 2, and 3 of this specification are not unique and unchanging data. This specification only lists the most representative mass percentage data of raw materials for preparing bricks with better performance and suitable for three different scenarios.

[0040] Unless otherwise defined, technical or scientific terms used herein shall have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs.

[0041] The exemplary implementation modes of the present invention are described in detail above with reference to the preferred embodiments. The protection scope of the present invention is not limited thereto. It can be understood by those skilled in the art that, without departing from the concept of the present invention, various modifications and variations can be made to the above-mentioned specific embodiments, and various combinations of the various technical features proposed in the present invention can be made without exceeding the protection scope of the present invention.

Claims

1. A high temperature energy-saving infrared thermal radiation coating, Features: The high-temperature energy-saving infrared thermal radiation coating includes the following components in parts by mass: 35-45 parts of wollastonite fiber, 5-15 parts of ceramic fiber, 5-10 parts of aluminum silicate wool, 5-10 parts of sepiolite wool, 5-15 parts of iron oxide, 12-18 parts of silica sol, 5-10 parts of thickener, 0.7-3 parts of dispersant, and 0.5-2 parts of defoamer.

2. The high temperature energy-saving infrared heat radiation coating according to claim 1, Features: The thickener is bentonite powder, the dispersant is sodium tripolyphosphate, and the defoamer is polyether modified silicone oil.

3. The high temperature energy-saving infrared heat radiation coating according to claim 2, Features: The high-temperature energy-saving infrared thermal radiation coating includes the following components, measured by mass: 45 parts of wollastonite fiber, 10 parts of ceramic fiber, 10 parts of aluminum silicate wool, 5 parts of sepiolite wool, 5 parts of iron oxide, 15 parts of silica sol, 8 parts of bentonite powder, 1 part of sodium tripolyphosphate, and 1 part of polyether modified silicone oil.

4. The high temperature energy-saving infrared heat radiation coating according to claim 2, Features: The high-temperature energy-saving infrared thermal radiation coating includes the following components, measured by mass: 35 parts of wollastonite fiber, 5 parts of ceramic fiber, 10 parts of aluminum silicate wool, 10 parts of sepiolite wool, 15 parts of iron oxide, 15 parts of silica sol, 8 parts of bentonite powder, 1 part of sodium tripolyphosphate, and 1 part of polyether modified silicone oil.

5. The high temperature energy-saving infrared heat radiation coating according to claim 2, Features: The high-temperature energy-saving infrared thermal radiation coating includes the following components, measured by mass: 38 parts of wollastonite fiber, 12 parts of ceramic fiber, 8 parts of aluminum silicate wool, 8 parts of sepiolite wool, 12 parts of iron oxide, 13 parts of silica sol, 7 parts of bentonite powder, 1 part of sodium tripolyphosphate, and 1 part of polyether modified silicone oil.

6. A method for preparing a high-temperature energy-saving infrared thermal radiation coating, Features: Step 1: Drying and screening; Place the powder raw materials such as wollastonite fiber, ceramic fiber, aluminum silicate wool, and sepiolite wool in a drying oven and dry them at 80-100°C for 2-4 hours to remove moisture from the raw materials. After drying, use a 180-250 mesh screen to screen the dried raw materials to ensure uniform particle size. Step 2: Surface treatment: Stir the iron oxide at 70-80°C, add a surfactant solution, and continue stirring for 1.5-2h. The surfactant is a silane coupling agent, and the amount added is 2%-3% of the mass of the iron oxide. Step 3: Add liquid ingredients; add silica sol, bentonite powder and water into a stirring kettle, set the initial stirring speed to 150-200 rpm, and continue stirring for 8-10 minutes until the mixture is evenly mixed; Step 4: Add powder components; gradually add pretreated wollastonite fiber, ceramic fiber, aluminum silicate wool, sepiolite wool and iron oxide in small amounts for multiple times, with the amount added each time being 10%-20% of the total powder amount, and add powder again after the powder is fully mixed with the liquid each time; During the addition process, gradually increase the stirring speed from 150-200rpm to 400-600rpm within 5-10min, and continue stirring for 40-60min to ensure that the powder and liquid components are fully mixed; Step 5: Adding additives; add dispersant and defoamer to the mixture obtained in step 4, and continue stirring at a stirring speed of 600-800 rpm for 20-30 minutes to obtain the coating.

Citation Information

Patent Citations

  • High-temperature-resistant, infrared radiation preventing and energy-saving coating

    CN106928832A

  • Preparation method of inorganic insulated waterproof coating for outer wall of building

    CN108102473A