Rust-to-rust anticorrosive paint and preparation method thereof
By using water-based epoxy resin and rust stabilizer to form a stable complex in the coating, the problem of insufficient adhesion of rust-preventive coatings is solved, achieving efficient corrosion prevention and low-cost rust prevention, suitable for complex equipment and rusted surfaces.
Patent Information
- Application Number
- CN202411315130.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-20
AI Technical Summary
Existing rust-preventive coatings do not bond well to metal surfaces, resulting in low adhesion and reduced corrosion resistance. Furthermore, traditional rust removal methods are labor-intensive and costly, making them difficult to apply to complex equipment.
Waterborne epoxy resin is used as the base material, and rust-transfer agents and rust-transfer stabilizers (such as zinc phosphate and oleic acid modified triazine covalent organic framework materials) are added. Stable complexes are formed through chemical reactions to improve the adhesion to the metal surface. Fillers such as graphene are added to enhance the density of the coating.
It improves the bonding stability between anti-corrosion coatings and steel structure surfaces, enhances anti-corrosion performance, reduces construction intensity and cost, and is suitable for both rusted and rust-free steel surfaces, shielding them from external corrosive media.
Smart Images

Figure CN119039857A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of chemical industry and material production equipment, and in particular to a rust-to-rust anti-corrosion coating and a preparation method thereof. Background Art
[0002] Metal corrosion is a phenomenon in which metals are destroyed by chemical or electrochemical effects of environmental media. Metal corrosion is prevalent in all industries and causes huge economic losses every year. Applying anti-corrosion coatings to metal surfaces is one of the main anti-corrosion measures for metals.
[0003] Traditional anti-rust paints cannot be applied directly on rusted metal surfaces. Rust must be thoroughly removed before painting. When the equipment is large, the structure is complex, and the construction conditions are harsh, it is difficult to use mechanized methods to remove rust. Manual grinding and rust removal are required, which is not only labor-intensive and inefficient, but also has high rust removal costs.
[0004] Rust-proof paint is a kind of paint that can be directly applied on a certain rusty metal surface. It stabilizes, passivates or converts the rust, turning the active rust into harmless substances, so as to achieve the dual purpose of both rust removal and protection, greatly improving the efficiency of anti-corrosion paint coating. However, in the prior art, the combination of rust-proof paint and metal surface is not sufficient, resulting in low adhesion of anti-corrosion paint, which in turn causes the paint to fall off and the anti-corrosion performance to decrease, increasing the frequency of paint re-brushing and equipment replacement, and also increasing enterprise costs. Summary of the invention
[0005] The present application provides a rust-to-rust anti-corrosion coating and a preparation method thereof, in order to solve the above-mentioned problems mentioned in the background technology.
[0006] On the one hand, the present application provides a rust-to-rust anti-corrosion coating, which is composed of the following components in parts by weight:
[0007] Water: 20-60 parts by weight;
[0008] Water-based epoxy resin: 25-40;
[0009] Surfactant: 10-12 parts by weight;
[0010] Filler: 5-12 parts by weight;
[0011] Rust removal agent: 0.3-0.6 parts by weight;
[0012] Curing agent: 10-15 parts by weight;
[0013] Pigment: 1-5 parts by weight;
[0014] Rust stabilizer: 0.2-0.4 parts by weight;
[0015] Defoamer: 0.5-0.7;
[0016] Thickener: 1-2.5 parts by weight;
[0017] The rust-proof stabilizer is zinc phosphate and oleic acid-modified triazine-based covalent organic framework material in a weight ratio of 1:0.3-0.7.
[0018] Optionally, the surfactant is coconut oil diethanolamide or dodecyl dimethyl betaine.
[0019] Optionally, the filler is one or more of graphene, molybdenum disulfide, mica, and boron nitride.
[0020] Optionally, the particle size of graphene, molybdenum disulfide, mica, and boron nitride is 10-100 nm.
[0021] Optionally, the rust-removing agent is one or more of hydrochloric acid, phytic acid, salicylic acid, tannic acid, ascorbic acid and oxalic acid.
[0022] Optionally, the pigment is one of titanium dioxide, lithopone, zinc oxide, antimony oxide, red iron oxide, hydrated yellow iron and black iron.
[0023] Optionally, the defoaming agent is one or more of BYK011, BYK012, and BYK024.
[0024] Optionally, the thickener is any one of polyacrylate, hydroxymethyl cellulose and agar.
[0025] On the other hand, the present application provides a method for preparing a rust-to-rust anti-corrosion coating, which is used to prepare the above-mentioned rust-to-rust anti-corrosion coating, and the preparation method comprises the following steps:
[0026] (1) Preparation of triazine-based covalent organic framework materials:
[0027] 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 1,3,5-tris(4-formylphenyl)benzene and mesitylene are added to the reactor in sequence, and then 1,4-dioxane and acetic acid are added, and ultrasonic dispersion is performed to form a mixed solution. The reactor is placed in an oil bath at a temperature of 110-140°C for reaction for 12-24 hours, and after the reaction is completed, it is cooled to room temperature to obtain a preliminary triazine-based covalent organic framework material, and the preliminary triazine-based covalent organic framework material is washed multiple times with tetrahydrofuran and acetone in sequence to obtain a triazine-based covalent organic framework material.
[0028] The molar ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to 1,3,5-tris(4-formylphenyl)benzene, mesitylene, 1,4-dioxane and acetic acid is 1:1-1.5:20-25:35-40:25-28.
[0029] (2) Preparation of oleic acid-modified triazine-based covalent organic framework material: The triazine-based covalent organic framework material and oleic acid are dispersed in anhydrous ethanol respectively, and ultrasonically treated for 10-35 minutes to form a triazine-based covalent organic framework material dispersion and an oleic acid dispersion. The triazine-based covalent organic framework material dispersion and the oleic acid dispersion are mixed and ultrasonically treated at a temperature of 30-45°C to obtain a modified triazine-based covalent organic framework material mixed solution. The solid is separated by centrifugation and washed with anhydrous ethanol at least 3 times to obtain an oleic acid-modified triazine-based covalent organic framework material.
[0030] (3) Add water-based epoxy resin, surfactant, rust removal agent, rust removal stabilizer and water into a container according to weight, and stir and mix at room temperature to form a dispersion.
[0031] (4) Add filler, curing agent, pigment, thickener and defoamer into the dispersion according to weight to obtain rust-to-rust anti-corrosion coating.
[0032] Optionally, the preparation step of the oleic acid-modified triazine-based covalent organic framework material also includes: the weight ratio of oleic acid to triazine-based covalent organic framework material is 1.5-3:1, the weight volume ratio of oleic acid to anhydrous ethanol in the oleic acid dispersion is 1g:10-20mL, and the weight volume ratio of triazine-based covalent organic framework material to anhydrous ethanol in the triazine-based covalent organic framework material dispersion is 1g:20-45mL.
[0033] The rust-to-rust anti-corrosion coating and preparation method thereof provided in the present application realize the preparation of the rust-to-rust anti-corrosion coating, improve the stability of the combination of the anti-corrosion coating and the surface of the steel structure, and thus greatly improve the anti-corrosion performance of the surface of the steel structure. Compared with the prior art, it has the following beneficial effects:
[0034] (1) By using water-based epoxy resin as the base resin and the main film-forming substance, a protective film can be formed on the surface of metal equipment after curing to achieve corrosion protection of the metal surface. By adding a rust-removing agent, a chemical reaction occurs with rust, and the formed stable complex firmly covers the steel surface to achieve the purpose of rust prevention. By adding a rust-removing stabilizer, a complex is further formed with the surface of the steel structure substrate, thereby improving the bonding force between the anti-corrosion coating and the steel structure surface. The rust-removing stabilizer is zinc phosphate and oleic acid-modified triazine-based covalent organic framework material. Zinc phosphate is tightly bound to metal ions, and the oleic acid-modified triazine-based covalent organic framework material reacts with metals to form metal complexes, thereby improving the bonding force with the steel structure surface, and at the same time synergistically with the rust-removing agent to promote the stability of the bonding between the rust-removing agent and the steel structure surface. This in turn improves the stability and corrosion resistance of the anti-corrosion coating. In addition, by grafting oleic acid onto a triazine-based covalent organic framework material, the presence of a carboxyl group can promote the stability of the binding between the rust stabilizer and the surface of the steel structure. The presence of long-chain alkanes in oleic acid is hydrophobic, which is beneficial to the anti-corrosion coating after film formation. It has a good shielding effect on external water and water vapor, greatly reducing the chemical and / or electrochemical corrosion caused by water infiltration into the anti-corrosion coating, improving the stable bonding between the steel structure surface and the anti-corrosion coating, and shielding the erosion of external corrosive media. The dual effects significantly improve the anti-corrosion performance of the anti-corrosion coating.
[0035] (2) The particle size of graphene, molybdenum disulfide, mica and boron nitride in the filler is 50-100nm, and it belongs to the lamellar structure, which can not only form a maze effect, increase the path for corrosive ions to penetrate the coating, and increase the barrier performance of the coating. It can also improve the mechanical strength of the coating applied to the metal surface, adjust the apparent density of the coating, make the filler and the water-based epoxy resin work together, improve the density of the coating after film formation, and have a positive role in isolating the corrosive medium.
[0036] (3) The operation method of the present application is simple, low-cost, universal, and easy to scale up for production.
[0037] (4) The present invention can not only be used for the rust removal, rust removal and rust prevention of rusted steel layers, but can also be used for rust-free steel surfaces to prevent rust. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, a brief introduction will be given below to the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0039] Figure 1A flow chart of the preparation process of a rust-to-rust anti-corrosion coating provided in one embodiment of the present application. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work also fall within the scope of protection of the present application.
[0041] On the one hand, the present application provides a rust-to-rust anti-corrosion coating, which is composed of the following components in parts by weight:
[0042] Water: 20-60 parts by weight;
[0043] Water-based epoxy resin: 25-40;
[0044] Surfactant: 10-12 parts by weight;
[0045] Filler: 5-12 parts by weight;
[0046] Rust removal agent: 0.3-0.6 parts by weight;
[0047] Curing agent: 10-15 parts by weight;
[0048] Pigment: 1-5 parts by weight;
[0049] Rust stabilizer: 0.2-0.4 parts by weight;
[0050] Defoamer: 0.5-0.7;
[0051] Thickener: 1-2.5 parts by weight;
[0052] The rust-proof stabilizer is zinc phosphate and oleic acid-modified triazine-based covalent organic framework material in a weight ratio of 1:0.3-0.7.
[0053] Specifically, in this application, water-based epoxy resin is used as the base resin and the main film-forming substance. After curing, a protective film can be formed on the surface of the metal equipment, isolating the metal surface from the atmosphere, thereby avoiding direct contact between oxygen, moisture in the air or solvents in contact with the metal surface of the metal equipment and the metal, thereby achieving corrosion protection on the metal surface. Wherein, the metal equipment is a metal or alloy such as steel, aluminum, etc. The addition of a surfactant can improve the dispersibility and dispersion stability of each component in the coating, and then when the coating is applied to the metal surface, the various components in the coating can be evenly dispersed on the metal surface, improving the uniformity of the coating, and then improving the anti-corrosion performance of the coating on the metal surface. Fillers can increase the hardness and wear resistance of the coating, and work together with water-based epoxy resin to improve the compactness of the film, thereby improving the anti-corrosion performance.
[0054] Rust removers can convert harmful rust into complexes or chelates with certain protective effects by chemically reacting with rust. This conversion not only converts the rust, but also forms a stable complex that firmly covers the steel surface, effectively blocking the contact between steel and air, achieving the purpose of rust prevention. Rust removers can fully infiltrate and penetrate the rust layer, and convert harmful corrosion products (such as Fe2O3 and other impurities) in the rust layer into stable harmless coatings (such as Fe3O4), which adhere to the steel surface, further improving the corrosion resistance of the coating. By using rust removers, the complex treatment process of grinding and rust removal on the steel structure surface before painting is avoided, which not only improves the efficiency of paint application, but also greatly reduces the construction intensity and coating processing costs.
[0055] The rust-removing stabilizer is used to further form a complex with the surface of the steel structure substrate after the coating is applied, and synergizes with the rust-removing agent to improve the bonding force between the anti-corrosion coating and the steel structure surface, while making the steel structure surface inactive and difficult to react with other substances, such as oxygen and water in the air. In this application, the rust-removing stabilizer is a zinc phosphate and oleic acid-modified triazine-based covalent organic framework material with a weight ratio of 1:0.3-0.7. Zinc phosphate can tightly bind to metal ions to form a difficult-to-dissolve precipitate, thereby effectively preventing the oxidation and corrosion of metal ions, significantly improving the anti-rust performance of the coating, improving the adhesion and coverage area of the coating to form a solid protective film, effectively resisting the erosion of humidity, oxygen and polluted environment on the coating, significantly improving the anti-corrosion performance of the coating and extending its service life. The oleic acid-modified triazine-based covalent organic framework material contains C=C, C=O, NH, and -CH that can react with metals, so that the oleic acid-modified triazine-based covalent organic framework material reacts with the surface of the steel structure substrate to generate a metal complex, thereby improving the binding with the steel structure surface, and synergizing with the rust-removing agent to promote the stability of the binding between the rust-removing agent and the steel structure surface, thereby improving the stability and corrosion resistance of the anticorrosive coating. In addition, by grafting oleic acid onto the triazine-based covalent organic framework material, on the one hand, the presence of oleic acid carboxyl groups can promote the binding stability of the rust-removing stabilizer and the steel structure surface, and on the other hand, oleic acid contains long-chain alkanes, and the presence of long-chain alkanes is hydrophobic, which is conducive to the anticorrosive coating after film coating, and has a good shielding effect on external water and water vapor, greatly reducing the chemical and / or electrochemical corrosion caused by water wetting the anticorrosive coating, while improving the stable binding between the steel structure surface and the anticorrosive coating, shielding the erosion of external corrosive media, and significantly improving the anticorrosive performance of the anticorrosive coating under the dual effects.
[0056] Curing agent is used to accelerate the curing of the coating after coating is completed to form a coating, thereby playing an anti-corrosion role. Pigments are used to select pigments of appropriate colors to color the anti-corrosion coating according to equipment requirements. Defoamers are used to eliminate the foam generated when the anti-corrosion coating is stirred or coated, which is beneficial to the flatness of the anti-corrosion coating after coating, thereby improving the anti-corrosion performance. Thickeners are used to adjust the viscosity of anti-corrosion coatings to suit the surface of steel structure equipment in different environments.
[0057] Furthermore, the rust-removing stabilizer also includes 1,4-diaminoanthraquinone, and the weight ratio of 1,4-diaminoanthraquinone to zinc phosphate is 0.03-0.08:1. 1,4-diaminoanthraquinone contains anthraquinone groups, and the molecule contains multiple benzene rings, which are connected to each other through a conjugated system to form a π-bond conjugated system. At the same time, anthraquinone is also connected to an amino group. The rust-removing agent activates the surface of the steel structure and the rust, and the nitrogen atom in the amino group can coordinate with the external electrons generated on the surface of the steel structure, so that 1,4-diaminoanthraquinone has a strong adhesion to the surface of the steel structure. At the same time, the π-bond conjugated system of the anthraquinone group has good stability, which can promote the stability between the rust-removing stabilizer and the surface of the steel structure. At the same time, it synergizes with zinc phosphate and oleic acid-modified triazine-based covalent organic framework materials to improve the stability of the adhesion between the anti-corrosion coating and the surface of the steel structure.
[0058] Furthermore, the rust-to-rust anti-corrosion coating provided by the present application also includes 1-3 parts by weight of a dispersant and 1-2 parts by weight of an anti-settling agent. The dispersant can improve the dispersibility of each component in the coating and help improve the uniformity of the coating. The anti-settling agent can prevent the sedimentation of each component in the coating and improve the anti-sagging performance of the coating. Among them, the dispersant is purchased from BYK190 of BYK Chemical Co., Ltd. of Germany, and the anti-settling agent is purchased from BYK-410 of BYK Chemical Co., Ltd. of Germany.
[0059] Through the above scheme, the present application improves the stability of the combination of the anti-corrosion coating and the surface of the steel structure, improves the adhesion between the anti-corrosion coating and the surface of the steel structure, and thus greatly improves the anti-corrosion performance of the surface of the steel structure. By using water-based epoxy resin as the base resin and the main film-forming substance, a protective film can be formed on the surface of the metal equipment after curing, thereby achieving corrosion protection of the metal surface. By adding a rust-removing agent, a chemical reaction occurs with rust, and harmful rust is converted into a complex or chelate with a protective effect, and the formed stable complex is firmly covered on the surface of the steel, blocking the contact between the steel and the air, thereby achieving the purpose of rust prevention. By adding a rust-removing stabilizer, a complex is further formed with the surface of the steel structure substrate, and synergistically acts with the rust-removing agent to improve the bonding force between the anti-corrosion coating and the surface of the steel structure. The rust-removing stabilizer is a triazine-based covalent organic framework material modified by zinc phosphate and oleic acid. Zinc phosphate can be tightly combined with metal ions to form a difficult-to-dissolve precipitate. The oleic acid-modified triazine-based covalent organic framework material reacts with the metal to generate a metal complex, thereby improving the combination with the steel structure surface. At the same time, it synergizes with the rust-removing agent to promote the stability of the combination between the rust-removing agent and the steel structure surface. Thus, the stability and corrosion resistance of the anticorrosive coating are improved. In addition, by grafting oleic acid onto the triazine-based covalent organic framework material, on the one hand, the presence of the oleic acid carboxyl group can promote the stability of the combination between the rust-removing stabilizer and the steel structure surface. On the other hand, oleic acid contains long-chain alkanes, and the presence of long-chain alkanes is hydrophobic, which is conducive to the anticorrosive coating to have a good shielding effect on external water and water vapor after film coating, greatly reducing the chemical and / or electrochemical corrosion caused by water wetting the anticorrosive coating, improving the stable combination between the steel structure surface and the anticorrosive coating, and shielding the erosion of external corrosive media. Under the dual effect, the anticorrosive performance of the anticorrosive coating is significantly improved, and the production cost is reduced.
[0060] Optionally, the surfactant is coconut oil diethanolamide or dodecyl dimethyl betaine.
[0061] Specifically, coconut oil diethanolamide or dodecyl dimethyl betaine can reduce the surface energy of each component in the coating, improve the dispersibility of the coating, and then promote the uniformity of the coating during coating, which is beneficial for each component to fully play its role and ensure the anti-corrosion performance of the anti-corrosion coating.
[0062] Optionally, the filler is one or more of graphene, molybdenum disulfide, mica, and boron nitride.
[0063] Specifically, graphene, molybdenum disulfide, mica, and boron nitride all have a lamellar structure, which can not only form a maze effect, increase the path for corrosive ions to penetrate the coating, and increase the barrier performance of the coating, but also improve the mechanical strength of the coating applied to the metal surface, adjust the apparent density of the coating, and make the filler and water-based epoxy resin work together to improve the density of the coating after film formation, which has a positive role in isolating corrosive media.
[0064] Optionally, the particle size of graphene, molybdenum disulfide, mica, and boron nitride is 10-100 nm.
[0065] Specifically, smaller particle sizes can more conveniently fill the rust on the surface of the steel structure, and synergize with the water-based epoxy resin to form a denser protective film on the surface of the steel structure, so as to increase the path for corrosive ions to penetrate the coating, increase the barrier properties of the coating, and isolate it from external corrosive media.
[0066] Optionally, the rust-removing agent is one or more of hydrochloric acid, phytic acid, salicylic acid, tannic acid, ascorbic acid and oxalic acid.
[0067] Specifically, the surface of steel structures easily absorbs corrosive media such as oxygen and moisture in the air and rusts. The main components of the products are compounds of trivalent iron and divalent iron, which are loose and unstable. The rust-removing agent is an inorganic hydrochloric acid or organic acid or a mixture of the two. It passivates or transforms the active harmful iron compounds in the rust layer into harmless and stable coatings. At the same time, it chelates with the rust to form a complex film with strong adhesion to the surface of the steel structure, so that the film is firmly adsorbed on the surface of the steel structure, achieving the purpose of rust-removing and corrosion prevention.
[0068] Wherein, the mass percentage of hydrochloric acid is 5-10%.
[0069] Optionally, the pigment is one of titanium dioxide, lithopone, zinc oxide, antimony oxide, red iron oxide, hydrated yellow iron and black iron.
[0070] Specifically, pigments are used to color anti-corrosion coatings and are added as needed in actual working conditions.
[0071] Optionally, the defoaming agent is one or more of BYK011, BYK012, and BYK024, all of which are purchased from BYK Chemical Co., Ltd. of Germany.
[0072] Optionally, the thickener is any one of polyacrylate, hydroxymethyl cellulose and agar.
[0073] On the other hand, Figure 1 As shown, the present application provides a method for preparing a rust-to-rust anti-corrosion coating, which is used to prepare the above-mentioned rust-to-rust anti-corrosion coating, and the preparation method comprises the following steps:
[0074] (1) Preparation of triazine-based covalent organic framework materials:
[0075] Add 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 1,3,5-tris(4-formylphenyl)benzene and mesitylene to a reactor in sequence, then add 1,4-dioxane and acetic acid, and perform ultrasonic dispersion to form a mixed solution; then place the reactor in an oil bath at a temperature of 110-140° C. to react for 12-24 hours, and cool to room temperature after the reaction to obtain a preliminary triazine-based covalent organic framework material, and wash the preliminary triazine-based covalent organic framework material with tetrahydrofuran and acetone in sequence for multiple times to obtain a triazine-based covalent organic framework material;
[0076] The molar ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to 1,3,5-tris(4-formylphenyl)benzene, mesitylene, 1,4-dioxane and acetic acid is 1:1-1.5:20-25:35-40:25-28;
[0077] (2) Preparation of oleic acid-modified triazine-based covalent organic framework material: Disperse the triazine-based covalent organic framework material and oleic acid in anhydrous ethanol respectively, and perform ultrasonic treatment for 10-35 minutes to form a triazine-based covalent organic framework material dispersion and an oleic acid dispersion. Mix the triazine-based covalent organic framework material dispersion and the oleic acid dispersion, and perform ultrasonic treatment at a temperature of 30-45° C. to obtain a modified triazine-based covalent organic framework material mixed solution. Centrifuge to obtain a solid, and wash it with anhydrous ethanol at least 3 times to obtain an oleic acid-modified triazine-based covalent organic framework material.
[0078] (3) adding water-based epoxy resin, surfactant, rust removal agent, rust removal stabilizer and water into a container according to weight, stirring and mixing at room temperature to form a dispersion;
[0079] (4) Add filler, curing agent, pigment, thickener and defoamer into the dispersion according to weight to obtain rust-to-rust anti-corrosion coating.
[0080] Specifically, at room temperature, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 1,3,5-tris(4-formylphenyl)benzene are dispersed in mesitylene, 1,4-dioxane and acetic acid to form a mixed solution, which is then transferred to an oil bath at a temperature of 110-140°C for reaction for 12-24 hours, so that the amino groups on 2,4,6-tris(4-aminophenyl)-1,3,5-triazine react with 1,3,5-tris(4-formylphenyl)benzene to generate a triazine-based covalent organic framework material containing C=C, C=O, NH, -CH, which can react with the metal on the surface of the steel structure to generate a metal complex and improve the bonding stability with the surface of the steel structure. Among them, room temperature refers to a temperature of 20-35°C. By ultrasonic treatment at 30-45°C, oleic acid is grafted onto a triazine-based covalent organic framework material, one end of the carboxyl group of the oleic acid is connected to the triazine-based covalent organic framework material, and the other end is a long-chain alkyl group, thereby improving the hydrophobicity of the anticorrosive coating. During the modification process, the triazine-based covalent organic framework material and oleic acid are dispersed in anhydrous ethanol and ultrasonically dispersed respectively, so that the dispersion is more uniform, thereby improving the modification degree of the triazine-based covalent organic framework material, and the oleic acid has a high degree of reaction with the triazine-based covalent organic framework material, thereby improving the anticorrosive performance of the anticorrosive coating.
[0081] Optionally, the step of preparing the oleic acid-modified triazine-based covalent organic framework material further comprises: washing the modified triazine-based covalent organic framework material mixed solution, and then vacuum drying to obtain the oleic acid-modified triazine-based covalent organic framework material.
[0082] Specifically, drying makes the oleic acid modified triazine-based covalent organic framework material more pure, facilitates the mixing of the oleic acid modified triazine-based covalent organic framework material with various components, and facilitates the metering when adding. During vacuum drying, the material is dried in a vacuum drying oven at 120-140° C. for 10-14 hours, and the vacuum degree is 0.01 Pa to 10 Pa.
[0083] Optionally, the weight ratio of oleic acid to triazine-based covalent organic framework material is 1.5-3:1, the weight volume ratio of oleic acid to anhydrous ethanol in the oleic acid dispersion is 1g:10-20mL, and the weight volume ratio of triazine-based covalent organic framework material to anhydrous ethanol in the triazine-based covalent organic framework material dispersion is 1g:20-45mL.
[0084] Specifically, the amount of oleic acid is greater than that of triazine-based covalent organic framework materials, which helps oleic acid to be more fully grafted onto triazine-based covalent organic framework materials. Increasing the amount of oleic acid can synergize with the rust-removing agent to promote the combination of the modified triazine-based covalent organic framework materials with the surface of the steel structure, improve the adhesion of the anti-corrosion coating, and at the same time, oleic acid can improve the hydrophobicity of the anti-corrosion coating, thereby improving the anti-corrosion performance. Controlling the amount of anhydrous ethanol can not only improve the uniformity of the oleic acid dispersion and the triazine-based covalent organic framework material dispersion, but also improve the degree of reaction during oleic acid modification.
[0085] Among them, the weight volume ratios of oleic acid, triazine-based covalent organic framework material and anhydrous ethanol in the oleic acid dispersion and the triazine-based covalent organic framework material dispersion respectively only represent the proportional relationship and are not limited to the above-mentioned specific values. In actual working conditions, the ratio can be enlarged or reduced according to the amount of reactants.
[0086] The rust-to-rust anti-corrosion coating provided by the present application is applied by brushing, roller coating or spraying, and the coating thickness is determined according to the actual working conditions. When multiple layers of coating are required, the next layer of coating is applied after the previous layer is dried.
[0087] The present invention is further described in detail below in conjunction with the examples. However, it should be understood that the examples are for illustrative purposes only and are not intended to limit the scope of the present invention.
[0088] Embodiment 1:
[0089] A rust-to-rust anti-corrosion coating and a preparation method thereof, the preparation method comprising the following steps:
[0090] (1) Preparation of triazine-based covalent organic framework materials:
[0091] At room temperature, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 1,3,5-tris(4-formylphenyl)benzene and mesitylene are added to a reaction kettle in sequence, and then 1,4-dioxane and acetic acid are added, and ultrasonic dispersion is performed to form a mixed solution; the reaction kettle is then placed in an oil bath at a temperature of 110° C. to react for 12-24 hours, and after the reaction is completed, the reaction kettle is cooled to room temperature to obtain a preliminary product of a triazine-based covalent organic framework material, and the preliminary product of the triazine-based covalent organic framework material is washed multiple times with tetrahydrofuran and acetone in sequence to obtain a triazine-based covalent organic framework material;
[0092] The molar ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to 1,3,5-tris(4-formylphenyl)benzene, mesitylene, 1,4-dioxane and acetic acid is 1:1:20:35:25;
[0093] (2) Preparation of oleic acid-modified triazine-based covalent organic framework material: The triazine-based covalent organic framework material and oleic acid are dispersed in anhydrous ethanol respectively, and ultrasonic treatment is performed for 10-35 minutes to form a triazine-based covalent organic framework material dispersion and an oleic acid dispersion. The triazine-based covalent organic framework material dispersion and the oleic acid dispersion are mixed and ultrasonic treatment is performed at a temperature of 30°C to obtain a modified triazine-based covalent organic framework material mixed liquid. The solid is separated by centrifugation and washed with anhydrous ethanol for at least 3 times, and dried in a vacuum drying oven at a vacuum degree of 0.01Pa and a temperature of 110°C for 14 hours. The oleic acid-modified triazine-based covalent organic framework material is obtained.
[0094] The weight ratio of oleic acid to triazine-based covalent organic framework material is 1.5:1, the weight volume ratio of oleic acid to anhydrous ethanol in the oleic acid dispersion is 1g:10mL, and the weight volume ratio of the triazine-based covalent organic framework material to anhydrous ethanol in the triazine-based covalent organic framework material dispersion is 1g:20mL.
[0095] (3) adding water-based epoxy resin, surfactant, rust removal agent, rust removal stabilizer and water into a container according to weight, stirring and mixing at room temperature to form a dispersion;
[0096] The surfactant is coconut oil diethanolamide, the derusting agent is 5% hydrochloric acid by weight, and the derusting stabilizer is zinc phosphate and oleic acid modified triazine covalent organic framework material in a weight ratio of 1:0.3. The ingredients include 20 parts by weight of water, 25 parts of waterborne epoxy resin, 10 parts by weight of surfactant, 0.3 parts by weight of derusting agent, and 0.2 parts by weight of derusting stabilizer.
[0097] (4) Add filler, curing agent, pigment, thickener, defoamer, dispersant and anti-settling agent to the dispersion according to weight to obtain rust-to-rust anti-corrosion coating.
[0098] Among them, 5 parts by weight of filler, 10 parts by weight of curing agent, 1 part by weight of pigment, 0.5 parts by weight of defoamer, 1 part by weight of thickener, 1 part by weight of dispersant and 1 part by weight of anti-settling agent.
[0099] The filler is graphene with a particle size of 50nm, the curing agent is m-phenylenediamine, the pigment is titanium dioxide, the thickener is polyacrylate, the defoamer is BYK011, the dispersant is BYK190, and the anti-settling agent is BYK-410.
[0100] Embodiment 2:
[0101] A rust-to-rust anti-corrosion coating and a preparation method thereof, the preparation method comprising the following steps:
[0102] The difference from Example 1 is that:
[0103] (1) Preparation of triazine-based covalent organic framework materials:
[0104] At room temperature, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 1,3,5-tris(4-formylphenyl)benzene and mesitylene are added to a reactor in sequence, and then 1,4-dioxane and acetic acid are added, and ultrasonic dispersion is performed to form a mixed solution; the reactor is then placed in an oil bath at a temperature of 120° C. to react for 14 hours, and after the reaction is completed, the reaction is cooled to room temperature to obtain a preliminary product of a triazine-based covalent organic framework material, and the preliminary product of the triazine-based covalent organic framework material is washed multiple times with tetrahydrofuran and acetone in sequence to obtain a triazine-based covalent organic framework material;
[0105] The molar ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to 1,3,5-tris(4-formylphenyl)benzene, mesitylene, 1,4-dioxane and acetic acid is 1:1.2:21:31:26;
[0106] (2) Preparation of oleic acid-modified triazine-based covalent organic framework material: The triazine-based covalent organic framework material and oleic acid were dispersed in anhydrous ethanol respectively, and ultrasonic treatment was performed for 12 minutes to form a triazine-based covalent organic framework material dispersion and an oleic acid dispersion. The triazine-based covalent organic framework material dispersion and the oleic acid dispersion were mixed and ultrasonic treatment was performed at a temperature of 34°C to obtain a modified triazine-based covalent organic framework material mixed solution. The solid was centrifuged and washed with anhydrous ethanol for at least 3 times, and dried in a vacuum drying oven at a vacuum degree of 1.5 Pa and a temperature of 125°C for 13 hours. The oleic acid-modified triazine-based covalent organic framework material was obtained.
[0107] The weight ratio of oleic acid to triazine-based covalent organic framework material is 1.8:1, the weight volume ratio of oleic acid to anhydrous ethanol in the oleic acid dispersion is 1g:12mL, and the weight volume ratio of the triazine-based covalent organic framework material to anhydrous ethanol in the triazine-based covalent organic framework material dispersion is 1g:28mL.
[0108] (3) adding water-based epoxy resin, surfactant, rust removal agent, rust removal stabilizer and water into a container according to weight, stirring and mixing at room temperature to form a dispersion;
[0109] The rust-removing stabilizer is a zinc phosphate and oleic acid-modified triazine-based covalent organic framework material in a weight ratio of 1:0.4. The rust-removing agent is a mixed solution obtained by mixing 8% hydrochloric acid and phytic acid in a weight ratio of 1:2, wherein 30 parts by weight of water, 30 parts of waterborne epoxy resin, 11 parts by weight of surfactant, 0.4 parts by weight of rust-removing agent, and 0.3 parts by weight of rust-removing stabilizer.
[0110] (4) Add filler, curing agent, pigment, thickener, defoamer, dispersant and anti-settling agent to the dispersion according to weight to obtain rust-to-rust anti-corrosion coating.
[0111] Among them, there are 7 parts by weight of filler, 11.5 parts by weight of curing agent, 2 parts by weight of pigment, 0.6 parts by weight of defoamer, 1.5 parts by weight of thickener, 2 parts by weight of dispersant and 1.5 parts by weight of anti-settling agent.
[0112] The filler is graphene and mica in a weight ratio of 2:1.
[0113] Embodiment 3:
[0114] A rust-to-rust anti-corrosion coating and a preparation method thereof, the preparation method comprising the following steps:
[0115] The difference from Example 1 is that:
[0116] (1) Preparation of triazine-based covalent organic framework materials:
[0117] At room temperature, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 1,3,5-tris(4-formylphenyl)benzene and mesitylene are added to a reaction kettle in sequence, and then 1,4-dioxane and acetic acid are added, and ultrasonic dispersion is performed to form a mixed solution; the reaction kettle is then placed in an oil bath at a temperature of 130° C. to react for 12 hours, and after the reaction is completed, the reaction is cooled to room temperature to obtain a preliminary product of a triazine-based covalent organic framework material, and the preliminary product of the triazine-based covalent organic framework material is washed multiple times with tetrahydrofuran and acetone in sequence to obtain a triazine-based covalent organic framework material;
[0118] The molar ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to 1,3,5-tris(4-formylphenyl)benzene, mesitylene, 1,4-dioxane and acetic acid is 1:1.3:23:33:27;
[0119] (2) Preparation of oleic acid modified triazine-based covalent organic framework material: The triazine-based covalent organic framework material and oleic acid are dispersed in anhydrous ethanol respectively, and ultrasonic treatment is performed for 10-35 minutes to form a triazine-based covalent organic framework material dispersion and an oleic acid dispersion. The triazine-based covalent organic framework material dispersion and the oleic acid dispersion are mixed and ultrasonic treatment is performed at a temperature of 38°C to obtain a modified triazine-based covalent organic framework material mixed solution. The solid is separated by centrifugation and washed with anhydrous ethanol for at least 3 times, and dried in a vacuum drying oven at a vacuum degree of 2Pa and a temperature of 130°C for 10 hours. The oleic acid modified triazine-based covalent organic framework material is obtained.
[0120] The weight ratio of oleic acid to triazine-based covalent organic framework material is 2.1:1, the weight volume ratio of oleic acid to anhydrous ethanol in the oleic acid dispersion is 1g:14mL, and the weight volume ratio of the triazine-based covalent organic framework material to anhydrous ethanol in the triazine-based covalent organic framework material dispersion is 1g:36mL.
[0121] (3) adding water-based epoxy resin, surfactant, rust removal agent, rust removal stabilizer and water into a container according to weight, stirring and mixing at room temperature to form a dispersion;
[0122] The rust-removing stabilizer is a zinc phosphate and oleic acid-modified triazine-based covalent organic framework material in a weight ratio of 1:0.5. The rust-removing agent is a mixed solution obtained by mixing 10% hydrochloric acid and phytic acid in a weight ratio of 1:3, wherein the mixture includes 45 parts by weight of water, 35 parts of waterborne epoxy resin, 12 parts by weight of surfactant, 0.5 parts by weight of rust-removing agent, and 0.4 parts by weight of rust-removing stabilizer.
[0123] (4) Add filler, curing agent, pigment, thickener, defoamer, dispersant and anti-settling agent to the dispersion according to weight to obtain rust-to-rust anti-corrosion coating.
[0124] Among them, the filler is 9.5 parts by weight, the curing agent is 13 parts by weight, the pigment is 3.5 parts by weight, the defoamer is 0.7, the thickener is 2 parts by weight, the dispersant is 3 parts by weight and the anti-settling agent is 2 parts by weight. The filler is molybdenum disulfide and boron nitride in a weight ratio of 2:1.
[0125] Embodiment 4:
[0126] A rust-to-rust anti-corrosion coating and a preparation method thereof, the preparation method comprising the following steps:
[0127] The difference from Example 3 is that:
[0128] (1) Preparation of triazine-based covalent organic framework materials:
[0129] At room temperature, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 1,3,5-tris(4-formylphenyl)benzene and mesitylene are added to a reactor in sequence, and then 1,4-dioxane and acetic acid are added, and ultrasonic dispersion is performed to form a mixed solution; the reactor is then placed in an oil bath at a temperature of 140° C. to react for 12 hours, and after the reaction is completed, the reaction is cooled to room temperature to obtain a preliminary triazine-based covalent organic framework material, and the preliminary triazine-based covalent organic framework material is washed multiple times with tetrahydrofuran and acetone in sequence to obtain a triazine-based covalent organic framework material;
[0130] The molar ratio of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to 1,3,5-tris(4-formylphenyl)benzene, mesitylene, 1,4-dioxane and acetic acid is 1:1.5:25:40:28;
[0131] (2) Preparation of oleic acid modified triazine-based covalent organic framework material: The triazine-based covalent organic framework material and oleic acid are dispersed in anhydrous ethanol respectively, and ultrasonic treatment is performed for 10-35 minutes to form a triazine-based covalent organic framework material dispersion and an oleic acid dispersion. The triazine-based covalent organic framework material dispersion and the oleic acid dispersion are mixed and ultrasonic treatment is performed at a temperature of 45°C to obtain a modified triazine-based covalent organic framework material mixed liquid. The solid is separated by centrifugation and washed with anhydrous ethanol for at least 3 times, and dried in a vacuum drying oven at a vacuum degree of 5Pa and a temperature of 140°C for 10 hours. The oleic acid modified triazine-based covalent organic framework material is obtained.
[0132] The weight ratio of oleic acid to triazine-based covalent organic framework material is 3:1, the weight volume ratio of oleic acid to anhydrous ethanol in the oleic acid dispersion is 1g:20mL, and the weight volume ratio of the triazine-based covalent organic framework material to anhydrous ethanol in the triazine-based covalent organic framework material dispersion is 1g:45mL.
[0133] (3) adding water-based epoxy resin, surfactant, rust removal agent, rust removal stabilizer and water into a container according to weight, stirring and mixing at room temperature to form a dispersion;
[0134] The rust-removing stabilizer is a zinc phosphate and oleic acid-modified triazine-based covalent organic framework material in a weight ratio of 1:0.7. The rust-removing agent is a mixed solution obtained by mixing 5% hydrochloric acid and salicylic acid in a weight ratio of 1:2, wherein the mixture includes 60 parts by weight of water, 40 parts of waterborne epoxy resin, 12 parts by weight of surfactant, 0.6 parts by weight of rust-removing agent, and 0.4 parts by weight of rust-removing stabilizer.
[0135] (4) Add filler, curing agent, pigment, thickener, defoamer, dispersant and anti-settling agent to the dispersion according to weight to obtain rust-to-rust anti-corrosion coating.
[0136] Among them, there are 12 parts by weight of filler, 15 parts by weight of curing agent, 5 parts by weight of pigment, 0.7 parts by weight of defoamer, 1-2.5 parts by weight of thickener, 3 parts by weight of dispersant and 2 parts by weight of anti-settling agent.
[0137] Embodiment 5:
[0138] A rust-to-rust anti-corrosion coating and a preparation method thereof, the preparation method comprising the following steps:
[0139] The difference from Example 3 is that:
[0140] (3) adding water-based epoxy resin, surfactant, rust removal agent, rust removal stabilizer and water into a container according to weight, stirring and mixing at room temperature to form a dispersion;
[0141] The rust-reducing stabilizer is zinc phosphate, oleic acid-modified triazine-based covalent organic framework material and 1,4-diaminoanthraquinone in a weight ratio of 1:0.3:0.03.
[0142] Embodiment 6:
[0143] A rust-to-rust anti-corrosion coating and a preparation method thereof, the preparation method comprising the following steps:
[0144] The difference from Example 3 is that:
[0145] (3) adding water-based epoxy resin, surfactant, rust removal agent, rust removal stabilizer and water into a container according to weight, stirring and mixing at room temperature to form a dispersion;
[0146] The rust-reducing stabilizer is zinc phosphate, oleic acid-modified triazine-based covalent organic framework material and 1,4-diaminoanthraquinone in a weight ratio of 1:0.5:0.05.
[0147] Embodiment 7:
[0148] A rust-to-rust anti-corrosion coating and a preparation method thereof, the preparation method comprising the following steps:
[0149] The difference from Example 3 is that:
[0150] (3) adding water-based epoxy resin, surfactant, rust removal agent, rust removal stabilizer and water into a container according to weight, stirring and mixing at room temperature to form a dispersion;
[0151] The rust-reducing stabilizer is zinc phosphate, oleic acid-modified triazine-based covalent organic framework material and 1,4-diaminoanthraquinone in a weight ratio of 1:0.7:0.08.
[0152] Comparative Example 1
[0153] The difference from Example 3 is that:
[0154] (3) The rust stabilizer is zinc phosphate and oleic acid modified triazine-based covalent organic framework material in a weight ratio of 1:0.2.
[0155] Comparative Example 2
[0156] The difference from Example 3 is that:
[0157] (3) The rust stabilizer is zinc phosphate and oleic acid modified triazine-based covalent organic framework material in a weight ratio of 1:0.8.
[0158] Comparative Example 3
[0159] The difference from Example 3 is that:
[0160] (3) The rust stabilizer is zinc phosphate.
[0161] Comparative Example 4
[0162] The difference from Example 3 is that:
[0163] (3) The rust stabilizer is an oleic acid-modified triazine-based covalent organic framework material.
[0164] Comparative Example 5
[0165] The difference from Example 3 is that:
[0166] (3) The rust stabilizer is 1,4-diaminoanthraquinone.
[0167] Comparative Example 6
[0168] The difference from Example 3 is that:
[0169] The preparation of the modified triazine-based covalent organic framework material in step (2) is not performed, and the rust stabilizer is a triazine-based covalent organic framework material.
[0170] Comparative Example 7
[0171] The difference from Example 3 is that:
[0172] (3) No rust stabilizer is added to the rust-to-rust anti-corrosion coating.
[0173] Experimental example
[0174] The anticorrosive coatings prepared by Examples 1 to 7 and Comparative Examples 1 to 7 were applied to the surface of the steel structure by brushing to form a coating, and the dry film thickness of the coating was 50-55 um. The hardness, water resistance, impact resistance and adhesion of the coating were tested. At the same time, the salt spray resistance of the coating was tested. Each experiment was conducted at least 3 times in parallel, and the average value was taken. The results are shown in Table 1.
[0175] The test standards in the experimental examples are as follows:
[0176] Paint and varnish pencil method for determination of film hardness GB / T 6739-2022
[0177] Determination of water resistance of paint film《GB / T 1733-1993》
[0178] Determination of impact resistance of paint films《GB / T 1732-2020》
[0179] Determination of neutral salt spray resistance of paints and varnishes《GB / T 1771-2007》
[0180] Table 1
[0181] hardness Water resistance / h Impact strength / J / m Adhesion / Grade Salt spray resistance / h Example 1 1H 300 145 Level 2 785 Example 2 2H 320 145 Level 2 793 Example 3 3H 350 155 Level 1 798 Example 4 3H 346 145 Level 1 786 Example 5 3H 345 150 Level 1 893 Example 6 3H 330 150 Level 1 985 Example 7 3H 330 145 Level 1 987 Comparative Example 1 1H 260 135 Level 3 653 Comparative Example 2 2H 240 130 Level 3 624 Comparative Example 3 2H 140 140 Level 4 575 Comparative Example 4 2H 290 130 Level 3 592 Comparative Example 5 1H 200 110 Level 3 581 Comparative Example 6 2H 180 110 Level 4 457 Comparative Example 7 F 130 100 Level 4 416
[0182] It can be seen from Table 1 that the performance of the anticorrosive coatings prepared in Examples 1 to 7 is significantly improved compared to that in Comparative Examples 1 to 7. Among them, the hardness of the coatings in Examples 3 to 7 is the highest. Compared with Comparative Example 1, the hardness and salt spray resistance time of the coatings in Examples 3 to 7 are significantly improved. Since the rust-removing stabilizer in Comparative Example 1 does not use oleic acid-modified triazine-based covalent organic skeleton materials, it is shown that the density of the protective film generated on the surface of the steel structure by the rust-removing stabilizer alone is worse than that of the coating with oleic acid-modified triazine-based covalent organic skeleton materials added. It shows that the oleic acid-modified triazine-based covalent organic skeleton material can react with the surface of the steel structure matrix to generate a metal complex, improve the bonding with the steel structure surface, and synergize with the rust-removing stabilizer to promote the stability of the bonding between the rust-removing stabilizer and the steel structure surface.
[0183] It can be seen from the water resistance test that the anticorrosive coatings prepared in Examples 1 to 7 have good water resistance compared to Comparative Examples 1 to 7. Comparing Comparative Example 4 with Comparative Example 6, it can be seen that the reason why the coating of the present application has good water resistance is not only that the oleic acid-modified triazine-based covalent organic skeleton material contains C=C, C=O, NH, -CH that can react with metals, so that the oleic acid-modified triazine-based covalent organic skeleton material reacts with the surface of the steel structure substrate to form a metal complex, but also because oleic acid is grafted onto the triazine-based covalent organic skeleton material to form a metal complex. On the organic skeleton material, on the one hand, the presence of oleic acid carboxyl can promote the bonding stability between the rust stabilizer and the steel structure surface; on the other hand, oleic acid contains long-chain alkanes, and the presence of long-chain alkanes is hydrophobic, which is beneficial to the anti-corrosion coating after film formation. It has a good shielding effect on external water and water vapor, greatly reducing the chemical and / or electrochemical corrosion caused by water infiltration into the anti-corrosion coating, improving the stable bonding between the steel structure surface and the anti-corrosion coating, and shielding the erosion of external corrosive media. The dual effect significantly improves the anti-corrosion performance of the anti-corrosion coating.
[0184] Observation of the impact resistance also shows that the rust stabilizer reacts with the surface of the steel structure substrate and works synergistically with the rust stabilizer to improve the bonding force between the anti-corrosion coating and the steel structure surface, while making the steel structure surface inactive and difficult to react with other substances, such as oxygen and water in the air. At the same time, the rust stabilizer composed of zinc phosphate, oleic acid-modified triazine-based covalent organic framework material and 1,4-diaminoanthraquinone significantly improves the adhesion of the anti-corrosion coating to the steel structure surface, improves the stability of the protective film on the steel structure surface, and thus improves the anti-corrosion effect of the anti-corrosion coating on the steel structure surface.
[0185] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, ordinary technicians in the field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A rust-to-rust anti-corrosion coating, characterized in that: The rust-to-rust anti-corrosion coating is composed of the following components in parts by weight: Water: 20-60 parts by weight; Water-based epoxy resin: 25-40; Surfactant: 10-12 parts by weight; Filler: 5-12 parts by weight; Rust removal agent: 0.3-0.6 parts by weight; Curing agent: 10-15 parts by weight; Pigment: 1-5 parts by weight; Rust stabilizer: 0.2-0.4 parts by weight; Defoamer: 0.5-0.7; Thickener: 1-2.5 parts by weight; The rust stabilizer is zinc phosphate and oleic acid modified triazine-based covalent organic framework material in a weight ratio of 1:0.3-0.
7.
2. The rust-to-rust anti-corrosion coating according to claim 1, characterized in that: The surfactant is coconut oil diethanolamide or dodecyl dimethyl betaine.
3. The rust-to-rust anti-corrosion coating according to claim 1, characterized in that: The filler is one or more of graphene, molybdenum disulfide, mica and boron nitride.
4. The rust-to-rust anti-corrosion coating according to claim 3, characterized in that: The particle sizes of the graphene, the molybdenum disulfide, the mica and the boron nitride are 10-100 nm.
5. The rust-to-rust anti-corrosion coating according to any one of claims 1 to 4, characterized in that: The rust-removing agent is one or more of hydrochloric acid, phytic acid, salicylic acid, tannic acid, ascorbic acid and oxalic acid.
6. The rust-to-rust anti-corrosion coating according to claim 1, characterized in that: The pigment is one of titanium dioxide, lithopone, zinc oxide, antimony oxide, red iron oxide, hydrated yellow iron and black iron.
7. The rust-to-rust anti-corrosion coating according to claim 1, characterized in that: The defoaming agent is one or more of BYK011, BYK012 and BYK024.
8. The rust-to-rust anti-corrosion coating according to claim 1, characterized in that: The thickener is any one of polyacrylate, hydroxymethyl cellulose and agar.
9. A method for preparing a rust-to-rust anti-corrosion coating, used for preparing the rust-to-rust anti-corrosion coating according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: (1) Preparation of triazine-based covalent organic framework materials: Add 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 1,3,5-tris(4-formylphenyl)benzene and mesitylene to a reaction kettle in sequence, then add 1,4-dioxane and acetic acid, and perform ultrasonic dispersion to form a mixed solution; place the reaction kettle in an oil bath at a temperature of 110-140° C. to react for 12-24 hours, and cool to room temperature after the reaction to obtain a preliminary triazine-based covalent organic framework material, and wash the preliminary triazine-based covalent organic framework material with tetrahydrofuran and acetone in sequence for multiple times to obtain a triazine-based covalent organic framework material; The molar ratio of the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to 1,3,5-tris(4-formylphenyl)benzene, the mesitylene, the 1,4-dioxane and the acetic acid is 1:1-1.5:20-25:35-40:25-28; (2) Preparation of oleic acid-modified triazine-based covalent organic framework material: The triazine-based covalent organic framework material and oleic acid are dispersed in anhydrous ethanol respectively, and ultrasonic treatment is performed for 10-35 minutes to form a triazine-based covalent organic framework material dispersion and an oleic acid dispersion. The triazine-based covalent organic framework material dispersion and the oleic acid dispersion are mixed and ultrasonic treatment is performed at a temperature of 30-45° C. to obtain a modified triazine-based covalent organic framework material mixed solution. The solid is separated by centrifugation and washed with anhydrous ethanol at least 3 times to obtain the oleic acid-modified triazine-based covalent organic framework material. (3) adding the waterborne epoxy resin, the surfactant, the rust removal agent, the rust removal stabilizer and the water into a container according to weight, and stirring and mixing at room temperature to form a dispersion; (4) Adding the filler, the curing agent, the pigment, the thickener and the defoaming agent to the dispersion according to weight to obtain the rust-to-rust anti-corrosion coating.
10. The method for preparing the rust-to-rust anti-corrosion coating according to claim 9, characterized in that: The preparation step of the oleic acid-modified triazine-based covalent organic framework material also includes: the weight ratio of the oleic acid to the triazine-based covalent organic framework material is 1.5-3:1, the weight volume ratio of the oleic acid to the anhydrous ethanol in the oleic acid dispersion is 1g:10-20mL, and the weight volume ratio of the triazine-based covalent organic framework material to the anhydrous ethanol in the triazine-based covalent organic framework material dispersion is 1g:20-45mL.
Citation Information
Patent Citations
Waterborne rust conversion primer coating with rust and preparation method thereof
CN107987591A
Environment-friendly water-based gas-phase long-acting antirust solution composition, preparation method and use method
CN108034949A
Preparation method of porous covalent organic framework material with triazine structure
CN112898515A
Waterborne epoxy on-rust anticorrosive coating as well as preparation method and application of waterborne epoxy on-rust anticorrosive coating
CN113999592A
Method for producing iron rust-reducing water-based rustproofing coating
JP2011168757A