High-temperature-resistant adhesive for bonding sensor and use method of high-temperature-resistant adhesive
Through the combination of high-density phosphate solution and composite filler, the problem of unstable existing high-temperature strain gauge adhesive in 1200℃ environment is solved, firm bonding of the sensor and reliability of high-temperature testing are achieved, and fast temperature testing is met Response to test requirements.
Patent Information
- Application Number
- CN202410395354.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-02
- Publication Date
- 2024-11-29
AI Technical Summary
The existing high-temperature strain gauge adhesives are unstable in an environment above 1200°C, which is prone to falling off, cracks or ablation, which cannot meet the needs of rapid temperature flush testing, and the high curing temperature affects the test accuracy and cycle.
The combination of phosphate solution and composite filler is used to prepare a high-density phosphate solution by reflux heating and evaporation heating. Polyphosphate components are added to form a three-dimensional network structure, and the bonding is enhanced with auxiliary fillers such as mullite fiber and alumina. Strength, room temperature curing and pressurized curing methods ensure firm bonding.
It realizes firm bonding of the sensor in an environment of 1200℃ without shedding, breakage, or cracks, improves the repeatability and efficiency of high-temperature tests, low curing temperature, avoids corrosion to the test substrate, and maintains mechanical properties.
Smart Images

Figure CN119039887A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a sensor bonding high temperature resistant adhesive and a use method thereof, and in particular to a 1200°C resistant inorganic phosphate special high temperature resistant adhesive and a use method thereof. Background Art
[0002] In a high-temperature service environment, the mechanical properties of materials and structures are significantly different from those in a normal temperature environment. High temperature degrades the mechanical properties of materials and produces significant thermal stress in the structure, significantly reducing the safety and reliability of the structure. Therefore, it is necessary to analyze the load-bearing reliability in a high-temperature environment. In ground thermal strength tests, the stress analysis of the structure usually uses strain measurement methods. When the strain test temperature exceeds 350°C, it is called a high-temperature strain test. In view of the characteristics of high-temperature strain measurement in ground tests, a high-temperature strain gauge / gauge contact strain measurement method is generally used to obtain local high-temperature strain data.
[0003] High temperature strain gauges are contact strain measurement sensors widely used in high temperature and heavy load fields such as aerospace, chemical industry, and energy. Their types and installation methods are also selected according to the bonding materials. For example, high temperature adhesive is often used to bond foil strain gauges on metal materials. When installing the strain gauge, a suitable adhesive must be selected for bonding and fixing at high temperature. Since the strain value measured by the strain gauge under high temperature conditions is not the true strain of the specimen, it contains the heat output of the strain gauge caused by temperature. The high temperature adhesive bonding method has a great influence on the measurement accuracy at high temperature. Therefore, stable and reliable bonding technology is the prerequisite for ensuring the accuracy of high temperature strain measurement.
[0004] During the test, in order to ensure rapid response, the strain gauge must be firmly bonded to the bonding substrate, and there must be no poor contact phenomena such as falling off, damage, cracks, and bulging. At present, the aerospace field uses imported high-temperature adhesives for sensors that are resistant to more than 1000℃. Foreign countries have imposed technical blockades on high-temperature adhesive materials for the bonding of such sensors that are resistant to rapid temperature shocks. Domestic research and development of such adhesives is still in its infancy, with poor high-temperature and rapid temperature shock resistance, easy cracking, bulging, and even falling off, poor ablation resistance, and a significant decrease in the performance of materials in the bonding area. At present, there is no high-performance adhesive material that meets the needs of rapid temperature shock applications. In the steady-state high-temperature test, some inorganic phosphate adhesives are used, and their maximum operating temperature is only 900℃. More than 3 step-type curing temperatures are required, and the maximum curing temperature is very high, usually not less than 400℃, which cannot meet the high-temperature test requirements above 1000℃. In addition, the sensor pasting curing process is complicated, affecting the test cycle. Excessive curing temperature will also cause the object being tested to undergo additional high-temperature treatment processes, affecting the actual performance of the material. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned defects and provide a high-temperature resistant adhesive for bonding sensors and a method for using the same, which solves the technical problems of existing adhesives being not resistant to high temperatures, having high curing temperatures, and causing serious corrosion to test substrates. The adhesive of the present invention cures quickly at room temperature, achieves curing strength after high-temperature baking, and is firmly bonded to the sample to be tested when subjected to a rapid temperature shock of 1200°C. It has a certain bonding strength both at room temperature and in high-temperature environments. The adhesive is suitable for pasting high-temperature resistant sensors during ultra-high temperature assessments.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] A sensor bonding high temperature resistant adhesive, comprising a phosphate solution and a composite filler, wherein the mass ratio of the phosphate solution to the composite filler is 100:85-120;
[0008] The density of phosphate solution is 1.60~1.80g / cm 3 ;
[0009] The density of the solution in the present invention is much greater than the density of the common phosphate solution (1.50-1.55 g / cm 3 ), a high-density phosphate solution is prepared by reflux heating and evaporation heating methods. The phosphate solution contains polyphosphate components, has a higher degree of polymerization, and forms a three-dimensional network structure with higher impact resistance.
[0010] The composite filler comprises an auxiliary filler and a curing agent, wherein the auxiliary filler comprises mullite fiber and silicon dioxide, and further comprises one or more of aluminum oxide, titanium dioxide or chromium trioxide.
[0011] Furthermore, the phosphate solution is one or more of an aluminum phosphate solution or a chromium aluminum phosphate solution.
[0012] Further, the curing agent is fused magnesium oxide;
[0013] The mass ratio of the curing agent to the auxiliary filler is 0.1 to 0.2.
[0014] Furthermore, the mass ratio of the phosphate solution to the composite filler is 100:86-100.
[0015] Further, the synthesis method of the aluminum phosphate solution comprises:
[0016] Phosphoric acid with a concentration of ≥85%, aluminum hydroxide and water are mixed and refluxed at 90-120°C for 0.5-2h to obtain an aluminum dihydrogen phosphate solution; the mass ratio of phosphoric acid, aluminum hydroxide and water is 100:20-33.3:48-80;
[0017] The aluminum dihydrogen phosphate solution is evaporated at a temperature of 50 to 120° C. for 0.5 to 4 hours, and the density of the solution is adjusted to a desired density to obtain an aluminum phosphate solution having a desired density;
[0018] The synthesis method of aluminum chromium phosphate solution comprises:
[0019] Phosphoric acid with a concentration of ≥85%, aluminum hydroxide, chromium oxide and water are mixed and refluxed at 90-120° C. for 0.5-2 hours to obtain a chromium aluminum phosphate solution; the mass ratio of phosphoric acid, aluminum hydroxide, chromium oxide and water is 100:20-33.3:10-20:48-80.
[0020] The aluminum chromium phosphate solution is evaporated at a temperature of 50 to 120° C. for 0.5 to 4 hours, and the density of the solution is adjusted to a desired density to obtain an aluminum chromium phosphate solution with a desired density.
[0021] Furthermore, the particle size of the composite filler is 0.5-10 μm.
[0022] Furthermore, the preparation method of the composite filler includes:
[0023] The curing agent and the auxiliary filler are mixed and ball-milled in a ball mill for 4 to 8 hours to obtain a powder; the rotation speed of the ball mill is 100 to 250 rpm;
[0024] The powder is sieved and dried in an oven for 1 to 5 hours at a drying temperature of 100 to 200°C;
[0025] The composite filler is obtained by natural drying and cooling.
[0026] The method for using the above-mentioned high temperature resistant adhesive for bonding a sensor comprises:
[0027] Under room temperature, the phosphate solution and the composite filler are mixed and stirred to obtain an adhesive;
[0028] Apply adhesive on the surface of the substrate to be bonded, and bond the sensor to the surface of the substrate to be bonded;
[0029] The sensor surface is covered with breathable fluorine-free varnished cloth, and a pressurizing mechanism acts on the breathable fluorine-free varnished cloth to perform pressurized curing;
[0030] Remove the breathable fluorocarbon paint cloth and the bonding is completed.
[0031] Further, at room temperature, the phosphate solution and the composite filler are repeatedly ground and mixed in a mortar.
[0032] When using a mortar for mixing, the agglomerated powder can be ground apart to facilitate the infiltration of the solution, and repeated grinding can ensure the mixing and dispersion of the ultrafine powder.
[0033] The thickness of the adhesive applied on the surface of the substrate to be bonded is 0.05 to 0.3 mm.
[0034] In the present invention, the density difference between the solution and the powder is relatively large. Due to the surface tension, it is difficult to mix very fine powder with the solution evenly by ordinary stirring. The ultrafine powder is prone to agglomeration into powder clumps. In addition, the amount of glue used to coat the sensor once is very small (<10g), making it even more difficult to ensure the uniformity of the mixing. Therefore, the present invention uses a mortar for repeated grinding to effectively improve the uniformity of the mixture.
[0035] Further, the pressurized curing method includes:
[0036] After pressurized curing at room temperature for 30 minutes to 1 hour, pressurized curing is performed at 80°C ± 5°C for 1 to 3 hours or pressurized curing is performed at room temperature for 1 to 2 days. During the curing process, the pressure is maintained at 0.01 to 0.05 atmospheres. During the curing process, the adhesive shrinks and needs to be continuously pressurized. The pressure must be greater than the contact pressure, but too much pressure can easily squeeze out the glue liquid completely, resulting in glue shortage. The present invention applies 0.01 to 0.05 atmospheres during the curing process, which can effectively improve the bonding quality.
[0037] Furthermore, the sensor is a sensor that can withstand rapid temperature shock at 1200°C; the rapid temperature shock at 1200°C is a rapid temperature rise process of 100-150°C / s from room temperature to 1200°C.
[0038] Compared with the prior art, the present invention has at least one of the following beneficial effects:
[0039] (1) The present invention creatively proposes a sensor bonding high temperature resistant adhesive that can withstand rapid temperature shocks of 1200°C. It undergoes a rapid temperature rise process of 100-150°C / s from room temperature to 1200°C, and is firmly bonded to the bonding substrate without any poor contact phenomena such as falling off, breakage, cracks, and bulging. The effect rate of high temperature testing is fast, and the repeatability of multiple high temperature tests is good.
[0040] (2) The adhesive of the present invention has a relatively long working period of 15 to 30 minutes at room temperature, and can be quickly dried on the surface after being coated on the surface of the substrate. The adhesive can be cured at room temperature for 0.5 to 1 hour and then at 80±5°C for 2 hours, or at room temperature for 1 day. The curing temperature and curing process are simple.
[0041] (3) The thermal weight loss of the present invention from room temperature to 1200°C in air is ≤5%, and the compressive shear strength at room temperature is 0.5-3MPa, and the compressive shear strength at 1200°C is 0.2-1MPa. After the test, the high-temperature adhesive is easy to remove from the surface without damaging the test substrate. The adhesive does not corrode the test sample and does not affect its mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1(a) state after bonding; (b) state before high temperature test; (c) state after high temperature test of Example 1 of the present invention;
[0043] Figure 2 The test results of the high temperature temperature measurement test repeated twice in Example 1 of the present invention;
[0044] Figure 3 (a) state after bonding; (b) state before high temperature test; (c) state after high temperature test of Example 2 of the present invention;
[0045] Figure 4 The test results of the high temperature temperature measurement test repeated twice in Example 2 of the present invention;
[0046] Figure 5 (a) state after bonding; (b) state before high temperature test; (c) state after high temperature test of Example 4 of the present invention;
[0047] Figure 6 The test results of the high temperature temperature measurement test repeated twice in Example 4 of the present invention;
[0048] Figure 7 (a) The state after bonding of Comparative Example 1 of the present invention; (b) The state after high temperature test;
[0049] Figure 8 (a) The state after bonding of Comparative Example 2 of the present invention; (b) The state after high temperature test;
[0050] Fig. 9 (a) The state after bonding of Comparative Example 3 of the present invention; (b) The state after high temperature test. DETAILED DESCRIPTION
[0051] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.
[0052] The word “exemplary” is used exclusively herein to mean “serving as an example, example, or illustration.” Any embodiment described herein as “exemplary” is not necessarily to be construed as preferred or advantageous over other embodiments.
[0053] The present invention provides a special high-temperature resistant inorganic phosphate adhesive resistant to 1200°C, which has excellent high-temperature resistance and rapid temperature shock performance, ablation resistance, low curing temperature, and no corrosion to the substrate, thereby having the advantages of high-temperature resistance and high bonding reliability. It is mainly used in the pasting of contact strain measurement sensors in high-temperature and heavy-load fields such as aerospace, chemical industry, and energy that require high-temperature resistance and high reliability.
[0054] The sensor bonding high temperature resistant adhesive capable of resisting rapid temperature shock at 1200°C of the present invention comprises a phosphate solution and a composite filler, wherein the composite filler comprises a curing agent and an auxiliary filler; the mass fraction ratio of the phosphate solution to the composite filler is 100:(85-120); the phosphate solution is at least one of an aluminum phosphate solution and a chromium aluminum phosphate solution; the curing agent is magnesium oxide; one of the auxiliary fillers is mullite fiber and silicon dioxide, and the other auxiliary fillers comprise at least one of aluminum oxide, titanium dioxide or chromium trioxide.
[0055] In a specific embodiment, the mass fraction ratio of the phosphate solution to the composite filler is 100:86.
[0056] In a specific embodiment, the mass fraction ratio of the phosphate solution to the composite filler is 100:100.
[0057] In a specific embodiment, the synthesis method of aluminum phosphate solution is to react phosphoric acid (CAS: 7664-38-2), aluminum hydroxide (CAS: 21645-51-2) and water, reflux at 90-120°C for 0.5-2h, and then evaporate the solution at 50-120°C for 0.5-4h to adjust the required phosphate solution density to 1.60-1.80g / cm 3 ; Phosphoric acid concentration ≥ 85%, its mass fraction is 100, the mass fraction of aluminum hydroxide is 20-33.3, and the mass fraction of water is 48-80. The synthesis method of aluminum chromium phosphate solution is to react phosphoric acid (CAS: 7664-38-2), aluminum hydroxide (CAS: 21645-51-2), chromium oxide (133-82-0) and water, reflux reaction at 90-120°C for 0.5-2h, and then evaporate the solution at 50-120°C for 0.5-4h to adjust the required phosphate solution density to 1.60-1.80g / cm 3 ; Phosphoric acid concentration ≥ 85%, its mass fraction is 100, the mass fraction of aluminum hydroxide is 20 to 33.3, the mass fraction of chromium oxide is 10 to 20, and the mass fraction of water is 48 to 80.
[0058] The present invention adopts the above synthesis method, and the aluminum hydroxide in the obtained solution has a lower limit than that of the general synthesis method.
[0059] In a specific embodiment, the phosphate solution is synthesized by a method having a density ranging from 1.60 to 1.80 g / cm 3 .
[0060] The density of the solution in the present invention is much greater than the density of the common phosphate solution (1.50-1.55 g / cm 3), a high-density phosphate solution is prepared by reflux heating and evaporation heating methods. The phosphate solution contains polyphosphate components, has a higher degree of polymerization, and forms a three-dimensional network structure with higher impact resistance.
[0061] In a specific implementation manner, the mass ratio of the curing agent to the auxiliary filler is 0.1 to 0.2.
[0062] In a specific embodiment, the magnesium oxide is fused magnesium oxide.
[0063] In a specific embodiment, the particle size of the composite filler is in the range of 0.5 to 10 μm, wherein the particle size of the mullite fiber refers to the fiber diameter.
[0064] In a specific embodiment, the preparation method of the composite filler is to mix the curing agent and the auxiliary filler, and ball mill them in a ball mill for 4-8 hours, and the speed of the ball mill is 100-250rpm; then the powder is sieved, and dried in an oven for 1-5 hours, and the drying temperature is 100-200°C; and naturally dried and cooled to obtain the composite filler.
[0065] At room temperature, the phosphate solution and the composite filler are mixed in proportion and stirred evenly. After 0.5 to 1 hour at room temperature, the mixture is kept at 80°C ± 5°C for 2 hours to complete curing, thereby obtaining the sensor bonding high temperature resistant adhesive capable of withstanding rapid temperature shock of 1200°C.
[0066] The method for using the high temperature resistant adhesive for bonding sensors resistant to 1200°C rapid temperature shock includes:
[0067] At room temperature, mix the above phosphate solution and composite filler in a mortar according to the proportion, stir evenly, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, the thickness of which is controlled at 0.05-0.3 mm, and apply breathable fluorine-free paint cloth. After pressurizing and curing at room temperature for 30 minutes to 1 hour, heat and cure at 80°C for 2 hours. During the curing process, maintain a pressure of 0.01-0.05 atmospheres. After heating, the breathable fluorine-free paint cloth can be removed for subsequent tests.
[0068] Existing adhesives often fall off or crack when they experience a rapid temperature rise process of 100-150℃ / s from room temperature to 1200℃, and some of them burn through, with delayed test response, prone to overheating, and poor test repeatability. The sensor bonding high temperature resistant adhesive that can withstand 1200℃ rapid temperature shock provided by the present invention undergoes a rapid temperature rise process of 100-150℃ / s from room temperature to 1200℃, and is firmly bonded to the bonding substrate without falling off, breakage, cracks, bulging, and other poor contact phenomena. The effect rate of high temperature testing is fast, and the repeatability of multiple high temperature tests is good.
[0069] Existing adhesives usually need to be left at room temperature for a long time and undergo more than three step-by-step temperature increases, with the highest curing temperature being nearly 400°C. The sensor bonding high-temperature resistant adhesive that can withstand 1200°C rapid temperature shocks provided by the present invention has a long operating period of 15 to 30 minutes at room temperature, and can be quickly dried on the surface when applied to the substrate surface. The adhesive can be cured by curing at room temperature for 1 hour and then at 80°C for 2 hours, or curing at room temperature for 1 day. The curing temperature and curing process are simple.
[0070] Existing adhesives often cause serious corrosion to test substrates such as composite materials, significantly reducing the mechanical properties of the materials. The thermal weight loss of the adhesive of the present invention from room temperature to 1200°C in air is ≤5%, and the compressive shear strength at room temperature is 0.5-3MPa, and the compressive shear strength at 1200°C is 0.2-1MPa. During high-temperature testing, the modulus of the adhesive is low and it is relatively soft to the test sample. After the test, the high-temperature adhesive is easy to remove from the surface without damaging the test substrate. The adhesive does not corrode the test sample and does not affect its mechanical properties. The bonding strength of the adhesive is low. When the surface is wiped with a wet cloth dipped in water, the bonding strength will be lower after the adhesive absorbs water, making it easier to remove.
[0071] Example:
[0072] The sensor bonding high temperature resistant adhesive of the present invention which can withstand rapid temperature shock of 1200°C comprises a phosphate solution and a composite filler;
[0073] The composite filler includes a curing agent and an auxiliary filler;
[0074] The mass ratio of the phosphate solution to the composite filler is 100:(85-120); within the above two groups of distribution ratios, the prepared adhesive has a suitable viscosity before curing at room temperature, has strong construction operability, and ensures strong bonding strength.
[0075] The phosphate solution is at least one of an aluminum phosphate solution and a chromium aluminum phosphate solution; the density range is 1.60 to 1.80 g / cm 3 The above-mentioned phosphate solution has suitable reactivity and storage stability. The phosphate solution within this density range has a low water content while ensuring a low viscosity, thereby avoiding excessive water solvent in the adhesive, which affects the density of the adhesive layer after curing.
[0076] The density of the solution in the present invention is much greater than the density of the common phosphate solution (1.50-1.55 g / cm 3 ), a high-density phosphate solution is prepared by reflux heating and evaporation heating methods. The phosphate solution contains polyphosphate components, has a higher degree of polymerization, and forms a three-dimensional network structure with higher impact resistance.
[0077] The curing agent is magnesium oxide; the magnesium oxide is fused magnesium oxide. The curing agent has excellent high temperature resistance, and the cured product cured by the phosphate solution has excellent high temperature resistance. The fused magnesium oxide has undergone high temperature hot melt treatment, so its reaction activity is much lower than that of magnesium oxide without surface treatment, so that the prepared adhesive has a longer operating period and a suitable room temperature curing reaction rate.
[0078] One of the auxiliary fillers is mullite fiber. The auxiliary filler is fibrous and can form a three-dimensional network structure in the adhesive to improve the body strength of the adhesive layer, relieve thermal stress, and avoid the spread of cracks. In addition, it has high temperature resistance of more than 1400°C, excellent thermal shock resistance, chemical stability, and good oxidation resistance at high temperatures. One of the auxiliary fillers is silicon dioxide. The auxiliary filler is spherical and can form a densely packed structure in the adhesive to improve the body strength of the adhesive layer. At the same time, it has good thermal conductivity, can quickly conduct temperature, reduce the lag of test feedback, and improve the sensitivity of the test. In addition, it has high temperature resistance of more than 1400°C, excellent thermal shock resistance, chemical stability, and good oxidation resistance at high temperatures. Other auxiliary fillers include at least one of alumina, titanium dioxide, or chromium trioxide. The auxiliary filler is spherical, which can further improve thermal conductivity and further improve the sensitivity of the test. The above-mentioned auxiliary filler has high temperature resistance of more than 1800°C, high strength at room temperature and high temperature, good thermal shock resistance, stable chemical properties, good oxidation resistance at high temperature, and improves the residual rate of high-temperature solidified materials. The above-mentioned auxiliary filler can also react with part of the incompletely reacted phosphate solution to form a cross-linked network, thereby improving the strength of the solidified material of the system.
[0079] In a specific embodiment, the mass fraction ratio of the phosphate solution to the composite filler is 100: 86. Under this composition ratio, the construction operation performance is excellent and the room temperature bonding strength is high.
[0080] In a specific embodiment, the mass fraction ratio of the phosphate solution to the composite filler is 100: 100. Under this composition ratio, while ensuring good construction operability, it has a higher high-temperature bonding strength compared to the mass fraction ratio of 100:86.
[0081] The mass ratio range of the curing agent and the auxiliary filler is 0.1 to 0.2. Within this mass ratio range of the curing agent and the auxiliary filler, the reaction rate at room temperature is suitable, the bonding strength is high, and the adhesive has a long operating period at room temperature. The content of the curing agent is appropriate to avoid excessive cross-linking of the adhesive, and the chemical reaction bonding strength at high temperature is moderate, while retaining a high residual rate of high-temperature cured products.
[0082] The particle size range of the curing agent is 0.5-10 μm. This particle size range has a suitable specific surface area, a moderate reaction contact surface, and a moderate reaction activity. The adhesive has a long operating period at room temperature and a high bonding strength at room temperature.
[0083] The particle size range of other auxiliary fillers is 0.5-10 μm, which is close to the particle size range of the curing agent. At the same time, the particle sizes of the curing agent and other auxiliary fillers are well matched, which reduces the void ratio between different particle sizes and improves the reaction activity.
[0084] The preparation method of the composite filler is as follows: mixing the curing agent and the auxiliary filler, ball milling in a ball mill for 4-8 hours, the rotation speed of the ball mill is 100-250rpm; drying in an oven for 1-5 hours, the drying temperature is 100-200℃; and naturally drying and cooling to obtain the composite filler.
[0085] At room temperature, the phosphate solution and the composite filler are mixed in proportion and stirred evenly. After 0.5 to 1 hour at room temperature, the mixture is kept at 80°C ± 5°C for 2 hours to complete curing, thereby obtaining the sensor bonding high temperature resistant adhesive capable of withstanding rapid temperature shock of 1200°C.
[0086] More specifically, the method for using the high temperature resistant adhesive for bonding sensors resistant to 1200°C rapid temperature shock includes the following steps:
[0087] At room temperature, the phosphate solution and the composite filler are mixed in a mortar according to a certain proportion. The agglomerated ultrafine composite filler is ground and dispersed in a manner similar to wet grinding, and then soaked and mixed evenly with the phosphate solution. Repeated grinding can ensure the mixing and dispersion of the ultrafine powder.
[0088] Since the viscosity of phosphate solution is slightly large (>0.2Pa·s) and there is a significant density difference between the solution and the filler, due to the effect of surface tension, it is difficult to mix the ultrafine composite filler with the solution evenly using ordinary stirring methods, and the problem of ultrafine powder agglomeration is prone to occur. In addition, the amount of glue prepared at one time when coating the sensor is very small (<10g), and simple mixing of small doses is difficult to ensure mixing uniformity.
[0089] Apply a small amount of adhesive to the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, and control the thickness to be 0.05-0.3mm. Stick a breathable fluorine-four paint cloth on the outside of the adhesive, pressurize and cure at room temperature for 30min-1h, and heat and cure at 80℃ for 2h. Maintain a pressure of 0.01-0.05 atmospheres during the curing process. After heating, the breathable fluorine-four paint cloth can be removed for subsequent tests. The function of the breathable fluorine-four paint cloth is to isolate the adhesive and the pressurizing mechanism.
[0090] Example 1
[0091] A sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock at 1200°C, the specific implementation steps are as follows:
[0092] The materials were weighed according to the formula shown in Table 1, refluxed at 100 °C for 2 h, and then evaporated at 80 °C for 2 h to obtain a density of 1.65 g / cm 3 The materials are weighed according to the formula shown in Table 2, and ball-milled in a ball mill for 6 hours at a speed of 250 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 110°C; and naturally dried and cooled to obtain a composite filler.
[0093] The phosphate solution and the composite filler were mixed in a mass fraction ratio of 100:86 and stirred evenly to obtain a sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock of 1200°C and has an operating period of about 25 minutes.
[0094] The adhesive was cured at room temperature for 0.5 hours and then kept at 80°C for 2 hours. The maximum thermal weight loss in air from room temperature to 1200°C was 3.9%. A certain amount of the adhesive was used to bond graphite (standard bonding sample). After curing at room temperature for 0.5 hours and then at 80°C for 2 hours, the compressive shear strength at room temperature was 2.9MPa and the compressive shear strength at 1200°C was 0.4MPa.
[0095] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, and control the thickness to be 0.1mm. Paste it with breathable fluorine-free paint cloth, pressurize it at room temperature for 30 minutes, and heat it at 80℃ for 2 hours. Figure 1 and Figure 2 After heating, the breathable fluorine-free paint cloth can be removed and a rapid heating test of 140°C / s can be carried out. When the temperature is raised to 1200°C, the sensor has excellent bonding effect, without bulging, cracks, falling off, etc. The thermal response is rapid, but after two repeated tests, the corresponding temperature of the second time is slightly higher than the first time.
[0096] Table 1 Example 1 Phosphate solution ratio
[0097] raw material Dosage (weight) Phosphoric acid 100 Aluminum hydroxide 33 water 48
[0098] Table 2 Composite filler ratio of Example 1
[0099] raw material Dosage (weight) D50 particle size (μm) Fused Magnesium Oxide 10 5 Mullite fiber 5 9 Silicon dioxide 87 6.5 Titanium Dioxide 5 3 Chromium trioxide 3 3
[0100] Example 2
[0101] A sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock at 1200°C, the specific implementation steps are as follows:
[0102] The materials were weighed according to the formula shown in Table 3, refluxed at 100°C for 1.5 h, and then evaporated at 60°C for 1.5 h to obtain a density of 1.62 g / cm3 The materials are weighed according to the formula shown in Table 4, and ball-milled in a ball mill for 4 hours at a speed of 150 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 120°C; and naturally dried and cooled to obtain a composite filler.
[0103] The phosphate solution and the composite filler are mixed in a mass fraction ratio of 100:100 and stirred evenly to obtain a sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock of 1200°C and has an operating period of about 15 minutes.
[0104] The adhesive was cured at room temperature for 0.5 hours and then kept at 80℃ for 2 hours. The maximum thermal weight loss in air from room temperature to 1200℃ was 3.5%. A certain amount of the adhesive was used to bond graphite, and after curing at room temperature for 0.5 hours and then at 80℃ for 2 hours, the compressive shear strength at room temperature was 2.1MPa and the compressive shear strength at 1200℃ was 0.8MPa.
[0105] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, and control the thickness to be 0.15mm. Paste the breathable fluorine-free paint cloth, pressurize and cure at room temperature for 30 minutes, and then heat and cure at 80℃ for 2 hours. Figure 3 and Figure 4 After heating, the breathable fluorine-free paint cloth can be removed and a rapid heating test of 140°C / s can be carried out. When the temperature is raised to 1200°C, the sensor has excellent bonding effect, without bulging, cracks, falling off, etc. The thermal response is rapid. After two repeated tests, the test repeatability is good.
[0106] Table 3 Example 2 Phosphate solution ratio
[0107] raw material Dosage (weight) Phosphoric acid 100 Aluminum hydroxide 25 water 50
[0108] Table 4 Composite filler ratio of Example 2
[0109] raw material Dosage (weight) D50 particle size (μm) Fused Magnesium Oxide 14 1.5 Mullite fiber 7 7 Silicon dioxide 75 5 Titanium Dioxide 13 5 Alumina 5 5
[0110] Example 3
[0111] A sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock at 1200°C, the specific implementation steps are as follows:
[0112] The materials were weighed according to the formula shown in Table 5, refluxed at 100°C for 1 h, and then evaporated at 50°C for 0.5 h to obtain a density of 1.60 g / cm 3The materials are weighed according to the formula shown in Table 6, and ball-milled in a ball mill for 8 hours at a speed of 250 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 120°C; and naturally dried and cooled to obtain a composite filler.
[0113] The phosphate solution and the composite filler were mixed in a mass fraction ratio of 100:86 and stirred evenly to obtain a sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock of 1200°C and has an operating period of about 30 minutes.
[0114] The adhesive was cured at room temperature for 0.5 hours and then kept at 80°C for 2 hours. The maximum thermal weight loss in air from room temperature to 1200°C was 4.6%. A certain amount of the adhesive was used to bond graphite, and after curing at room temperature for 0.5 hours and then at 80°C for 2 hours, the compressive shear strength at room temperature was 2.7MPa and the compressive shear strength at 1200°C was 0.2MPa.
[0115] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, the thickness is controlled at 0.05mm, and stick on the breathable fluorine-four paint cloth. After pressurizing and curing at room temperature for 30 minutes, heat and cure at 80℃ for 2 hours. After heating, the breathable fluorine-four paint cloth can be removed, and a rapid heating test of 100℃ / s is carried out. When the temperature is raised to 1200℃, the sensor has excellent bonding effect, no bulging, cracks, falling off, etc., and the thermal response is rapid. After two repeated tests, the repeatability of the test is good.
[0116] Table 5 Example 3 Phosphate solution ratio
[0117] raw material Dosage (weight) Phosphoric acid 100 Aluminum hydroxide 22 water 80
[0118] Table 6 Composite filler ratio of Example 3
[0119]
[0120]
[0121] Example 4
[0122] A sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock at 1200°C, the specific implementation steps are as follows:
[0123] The materials were weighed according to the formula shown in Table 7, refluxed at 100°C for 1 h, and then evaporated at 50°C for 0.5 h to obtain a density of 1.60 g / cm 3The materials are weighed according to the formula shown in Table 8, and ball-milled in a ball mill for 6 hours at a speed of 200 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 120°C; and naturally dried and cooled to obtain a composite filler.
[0124] The phosphate solution and the composite filler are mixed in a mass fraction ratio of 100:120 and stirred evenly to obtain a sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock of 1200°C and has an operating period of about 15 minutes.
[0125] The adhesive was cured at room temperature for 0.5 hours and then kept at 80°C for 2 hours. The maximum thermal weight loss in air from room temperature to 1200°C was 4.0%. A certain amount of the adhesive was used to bond graphite, and after curing at room temperature for 0.5 hours and then at 80°C for 2 hours, the compressive shear strength at room temperature was 2.5MPa and the compressive shear strength at 1200°C was 0.5MPa.
[0126] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, and control the thickness to 0.10mm, and stick a breathable fluorine-free paint cloth on it. After pressurizing and curing at room temperature for 30 minutes, heat and cure at 80℃ for 2 hours. Figure 5 and Figure 6 After heating, the breathable fluorine-free paint cloth can be removed and a rapid heating test of 140°C / s can be carried out. When the temperature is raised to 1200°C, the sensor has excellent bonding effect, without bulging, cracks, falling off, etc. The thermal response is rapid. After two repeated tests, the test repeatability is good.
[0127] Table 7 Example 4 Phosphate solution ratio
[0128] raw material Dosage (weight) Phosphoric acid 100 Aluminum hydroxide 22 water 80
[0129] Table 8 Composite filler ratio of Example 4
[0130]
[0131]
[0132] Example 5
[0133] A sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock at 1200°C, the specific implementation steps are as follows:
[0134] The materials were weighed according to the formula shown in Table 9, refluxed at 100°C for 1.5 h, and then evaporated at 60°C for 1.5 h to obtain a density of 1.62 g / cm 3The materials are weighed according to the formula shown in Table 10, and ball-milled in a ball mill for 6 hours at a speed of 150 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 120°C; and naturally dried and cooled to obtain a composite filler.
[0135] The phosphate solution and the composite filler were mixed in a mass fraction ratio of 100:86 and stirred evenly to obtain a sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock of 1200°C and has an operating period of about 30 minutes.
[0136] The adhesive was cured at room temperature for 0.5 hours and then kept at 80℃ for 2 hours. The maximum thermal weight loss in air from room temperature to 1200℃ was 3.8%. A certain amount of the adhesive was used to bond graphite, and after curing at room temperature for 0.5 hours and then at 80℃ for 2 hours, the compressive shear strength at room temperature was 2.6MPa and the compressive shear strength at 1200℃ was 0.3MPa.
[0137] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, the thickness is controlled at 0.05mm, and stick on the breathable fluorine-four paint cloth. After pressurizing and curing at room temperature for 30 minutes, heat and cure at 80℃ for 2 hours. After heating, the breathable fluorine-four paint cloth can be removed, and a rapid heating test of 130℃ / s is carried out. When the temperature is raised to 1200℃, the sensor has excellent bonding effect, no bulging, cracks, shedding, etc., and the thermal response is rapid.
[0138] Table 9 Example 5 Phosphate solution ratio
[0139]
[0140]
[0141] Table 10 Composite filler ratio of Example 5
[0142] raw material Dosage (mass ratio) D50 particle size (μm) Fused Magnesium Oxide 10 3 Mullite fiber 4 9 Silicon dioxide 64 3.5 Titanium Dioxide 2.6 1.5
[0143] Example 6
[0144] A sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock at 1200°C, the specific implementation steps are as follows:
[0145] The materials were weighed according to the formula shown in Table 11, refluxed at 100°C for 1.5 h, and then evaporated at 60°C for 1.5 h to obtain a density of 1.62 g / cm 3The materials are weighed according to the formula shown in Table 12, and ball-milled in a ball mill for 6 hours at a speed of 150 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 120°C; and naturally dried and cooled to obtain a composite filler.
[0146] The phosphate solution and the composite filler were mixed in a mass fraction ratio of 100:86 and stirred evenly to obtain a sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock of 1200°C and has an operating period of about 30 minutes.
[0147] The adhesive was cured at room temperature for 0.5 hours and then kept at 80℃ for 2 hours. The maximum thermal weight loss in air from room temperature to 1200℃ was 3.8%. A certain amount of the adhesive was used to bond graphite, and after curing at room temperature for 0.5 hours and then at 80℃ for 2 hours, the compressive shear strength at room temperature was 2.6MPa and the compressive shear strength at 1200℃ was 0.3MPa.
[0148] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, the thickness is controlled at 0.05mm, and stick on the breathable fluorine-four paint cloth. After pressurizing and curing at room temperature for 30 minutes, heat and cure at 80℃ for 2 hours. After heating, the breathable fluorine-four paint cloth can be removed, and a rapid heating test of 150℃ / s is carried out. When the temperature is raised to 1200℃, the sensor has excellent bonding effect, no bulging, cracks, falling off, etc., and the thermal response is rapid.
[0149] Table 11 Example 6 Phosphate solution ratio
[0150] raw material Dosage (mass ratio) Phosphoric acid 100 Aluminum hydroxide 25 water 50 Chromium trioxide 15
[0151] Table 12 Composite filler ratio of Example 6
[0152] raw material Dosage (mass ratio) D50 particle size (μm) Fused Magnesium Oxide 10 3.5 Mullite fiber 4 3 Silicon dioxide 64 3.5 Titanium Dioxide 2.6 1.5
[0153] Example 7
[0154] A sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock at 1200°C, the specific implementation steps are as follows:
[0155] The materials were weighed according to the formula shown in Table 13, refluxed at 100°C for 1 h, and then evaporated at 50°C for 0.5 h to obtain a density of 1.60 g / cm 3 The materials are weighed according to the formula shown in Table 14, and ball-milled in a ball mill for 8 hours at a speed of 250 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 120°C; and naturally dried and cooled to obtain a composite filler.
[0156] The phosphate solution and the composite filler were mixed in a mass fraction ratio of 100:86 and stirred evenly to obtain a sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock of 1200°C and has an operating period of about 30 minutes.
[0157] The adhesive was cured at room temperature for 0.5 hours and then kept at 80°C for 2 hours. The maximum thermal weight loss in air from room temperature to 1200°C was 4.6%. A certain amount of the adhesive was used to bond graphite, and after curing at room temperature for 0.5 hours and then at 80°C for 2 hours, the compressive shear strength at room temperature was 2.7MPa and the compressive shear strength at 1200°C was 0.2MPa.
[0158] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, the thickness is controlled at 0.05mm, and stick on the breathable fluorine-four paint cloth. After pressurizing and curing at room temperature for 30 minutes, heat and cure at 80℃ for 2 hours. After heating, the breathable fluorine-four paint cloth can be removed, and a rapid heating test of 150℃ / s is carried out. When the temperature is raised to 1200℃, the sensor has excellent bonding effect, no bulging, cracks, falling off, etc., and the thermal response is rapid.
[0159] Table 13 Example 7 Phosphate solution ratio
[0160] raw material Dosage (mass ratio) Phosphoric acid 100 Aluminum hydroxide 22 water 80 Chromium trioxide 15
[0161] Table 14 Composite filler ratio of Example 7
[0162] raw material Dosage (mass ratio) D50 particle size (μm) Fused Magnesium Oxide 10 3.5 Mullite fiber 6 5 Silicon dioxide 88 6.5 Titanium Dioxide 4 3
[0163] Example 8
[0164] A sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock at 1200°C, the specific implementation steps are as follows:
[0165] The materials were weighed according to the formula shown in Table 15, refluxed at 120°C for 2 h, and then evaporated at 120°C for 4 h to obtain a density of 1.80 g / cm 3 The materials are weighed according to the formula shown in Table 16, and ball-milled in a ball mill for 8 hours at a speed of 250 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 120°C; and naturally dried and cooled to obtain a composite filler.
[0166] The phosphate solution and the composite filler were mixed in a mass fraction ratio of 100:86 and stirred evenly to obtain a sensor bonding high temperature resistant adhesive that can withstand rapid temperature shock of 1200°C and has an operating period of about 20 minutes.
[0167] The adhesive was cured at room temperature for 0.5 hours and then kept at 80°C for 2 hours. The maximum thermal weight loss in air from room temperature to 1200°C was 2.5%. A certain amount of the adhesive was used to bond graphite, and after curing at room temperature for 0.5 hours and then at 80°C for 2 hours, the compressive shear strength at room temperature was 2.9MPa and the compressive shear strength at 1200°C was 0.3MPa.
[0168] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, the thickness is controlled at 0.10mm, stick on the breathable fluorine-four paint cloth, pressurize and cure at room temperature for 30 minutes, and heat and cure at 80℃ for 2 hours. After heating, the breathable fluorine-four paint cloth can be removed, and a rapid heating test of 150℃ / s is carried out. When the temperature is raised to 1200℃, the sensor has excellent bonding effect, no bulging, cracks, shedding, etc., and the thermal response is rapid.
[0169] Table 15 Example 8 Phosphate solution ratio
[0170] raw material Dosage (mass ratio) Phosphoric acid 100 Aluminum hydroxide 33.3 water 48
[0171] Table 16 Example 8 Composite filler ratio
[0172] raw material Dosage (mass ratio) D50 particle size (μm) Fused Magnesium Oxide 10 5 Mullite fiber 6 9 Silicon dioxide 60 10 Titanium Dioxide 4 10
[0173] Comparative Example 1
[0174] The materials were weighed according to the formula shown in Table 17, and refluxed at 100°C for 0.5h to obtain a density of 1.51 g / cm 3 The materials are weighed according to the formula shown in Table 18, and ball-milled in a ball mill for 6 hours at a speed of 200 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 120°C; and naturally dried and cooled to obtain a composite filler.
[0175] The phosphate solution and the composite filler are mixed in a mass fraction ratio of 100:120, stirred evenly, and a high temperature resistant adhesive is obtained, and the operating period is about 50 minutes.
[0176] The difference between this comparative example and Example 4 is only that the density of the phosphate solution is different.
[0177] Table 17 Comparative Example 1 Phosphate Solution Ratio
[0178] raw material Dosage (weight) Phosphoric acid 100 Aluminum hydroxide 22 water 80
[0179] Table 18 Comparative Example 1 Composite Filler Ratio
[0180] raw material Dosage (weight) D50 particle size (μm) Fused Magnesium Oxide 16 1.5 Mullite fiber 6 7 Silicon dioxide 84 6.5 Titanium Dioxide 6 5 Chromium trioxide 4 3
[0181] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, and control the thickness to 0.10mm, and stick a breathable fluorine-free paint cloth on it. After pressurizing and curing at room temperature for 30 minutes, heat and cure at 80℃ for 2 hours. Figure 7 After heating, the breathable fluorine-free paint cloth can be removed and a rapid heating test of 140°C / s can be carried out. When the temperature is raised to 1200°C, the sensor is well bonded, but obvious bulging and falling off occur.
[0182] Comparative Example 2
[0183] The materials were weighed according to the formula shown in Table 19, refluxed at 100°C for 1 hour, and then evaporated at 40°C for 0.5 hour to obtain a density of 1.54 g / cm 3 The materials are weighed according to the formula shown in Table 20, and ball-milled in a ball mill for 4 hours at a speed of 150 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 120°C; and naturally dried and cooled to obtain a composite filler.
[0184] The phosphate solution and the composite filler are mixed in a mass fraction ratio of 100:100, stirred evenly, and a high temperature resistant adhesive is obtained, and the operation period is about 10 minutes.
[0185] The difference between this comparative example and Example 2 is that the density of the phosphate solution is different and the type of curing agent is different.
[0186] Table 19 Comparative Example 2 Phosphate Solution Ratio
[0187] raw material Dosage (weight) Phosphoric acid 100 Aluminum hydroxide 25 water 50
[0188] Table 20 Comparative Example 2 Composite Filler Ratio
[0189] raw material Dosage (weight) D50 particle size (μm) Ordinary magnesium oxide 14 1.5 Mullite fiber 7 7 Silicon dioxide 75 5 Titanium Dioxide 13 5 Alumina 5 5
[0190] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, and control the thickness to be 0.15mm. Paste the breathable fluorine-free paint cloth, pressurize and cure at room temperature for 30 minutes, and then heat and cure at 80℃ for 2 hours. Figure 8 After heating, the breathable fluorine-free paint cloth can be removed and a rapid heating test of 140°C / s can be carried out. When the temperature is raised to 1200°C, the sensor is well bonded, but obvious small bubbles and warping appear.
[0191] Comparative Example 3
[0192] Weigh the materials according to the formula shown in Table 21, react at 100℃ for 1.5h, and evaporate at 50℃ for 2h to obtain a density of 1.58g / cm 3 The materials are weighed according to the formula shown in Table 22, and ball-milled in a ball mill for 6 hours at a speed of 250 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 110°C; and naturally dried and cooled to obtain a composite filler.
[0193] The phosphate solution and the composite filler are mixed in a mass fraction ratio of 100:86, stirred evenly, and a high temperature resistant adhesive is obtained, and the operation period is about 25 minutes.
[0194] The difference between this comparative example and Example 1 is that the density of the phosphate solution is different and mullite fiber is not added.
[0195] Table 21 Comparative Example 3 Phosphate Solution Ratio
[0196] raw material Dosage (weight) Phosphoric acid 100 Aluminum hydroxide 33 water 48
[0197] Table 22 Comparative Example 3 Composite Filler Ratio
[0198] raw material Dosage (weight) D50 particle size (μm) Fused Magnesium Oxide 10 5 Silicon dioxide 87 6.5 Titanium Dioxide 5 3 Chromium trioxide 3 3
[0199] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, and control the thickness to be 0.1mm. Paste it with breathable fluorine-free paint cloth, pressurize it at room temperature for 30 minutes, and heat it at 80℃ for 2 hours. Fig. 9 After heating, the breathable fluorine-free paint cloth can be removed and a rapid heating test of 140°C / s can be carried out. When the temperature is raised to 1200°C, the sensor is well bonded, but there are obvious large pieces falling off and warping.
[0200] Comparative Example 4
[0201] The materials were weighed according to the formula shown in Table 23, refluxed at 100°C for 1.5 h, and then evaporated at 50°C for 2 h to obtain a density of 1.58 g / cm 3 The materials are weighed according to the formula shown in Table 24, and ball-milled in a ball mill for 6 hours at a speed of 250 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 110°C; and naturally dried and cooled to obtain a composite filler.
[0202] The phosphate solution and the composite filler are mixed in a mass fraction ratio of 100:86, stirred evenly, and a high temperature resistant adhesive is obtained, and the operation period is about 25 minutes.
[0203] The difference between this comparative example and Example 1 is that the density of the phosphate solution is different and the ratio of the composite filler is different.
[0204] Table 23 Comparative Example 4 Phosphate Solution Ratio
[0205] raw material Dosage (weight) Phosphoric acid 100 Aluminum hydroxide 33 water 48
[0206] Table 24 Comparative Example 4 Composite Filler Ratio
[0207] raw material Dosage (weight) D50 particle size (μm) Fused Magnesium Oxide 10 5 Mullite fiber 5 9 Silicon dioxide 100 6.5 Titanium Dioxide 5 3 Chromium trioxide 5 3
[0208] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, the thickness is controlled at 0.1mm, and stick on the breathable fluorine-four paint cloth. After pressurizing and curing at room temperature for 30 minutes, heat and cure at 80℃ for 2 hours. After heating, the breathable fluorine-four paint cloth can be removed, and a rapid heating test of 140℃ / s is carried out. When the temperature is raised to 1200℃, the sensor is well bonded, but there is obvious large piece shedding and warping.
[0209] Comparative Example 5
[0210] The materials were weighed according to the formula shown in Table 25, refluxed at 100°C for 1.5 h, and then evaporated at 50°C for 2 h to obtain a density of 1.58 g / cm 3 The materials are weighed according to the formula shown in Table 26, and ball-milled in a ball mill for 6 hours at a speed of 250 rpm; the powder is then sieved, and dried in an oven for 2 hours at a temperature of 110°C; and naturally dried and cooled to obtain a composite filler.
[0211] The phosphate solution and the composite filler are mixed in a mass fraction ratio of 100:86, stirred evenly, and a high temperature resistant adhesive is obtained, and the operation period is about 25 minutes.
[0212] The difference between this comparative example and Example 1 is that the density of the phosphate solution is different and the coating thickness is different.
[0213] Table 25 Comparative Example 5 Phosphate Solution Ratio
[0214] raw material Dosage (weight) Phosphoric acid 100 Aluminum hydroxide 33 water 48
[0215] Table 26 Comparative Example 5 Composite Filler Ratio
[0216] raw material Dosage (weight) D50 particle size (μm) Fused Magnesium Oxide 10 5 Mullite fiber 5 9 Silicon dioxide 87 6.5 Titanium Dioxide 5 3 Chromium trioxide 3 3
[0217] Take a certain amount of the adhesive and mix it in a mortar, stir it evenly, apply a small amount of adhesive on the bonding area of the sensor site corresponding to the substrate to be bonded, place the sensor on the surface of the substrate to be bonded, apply a layer of adhesive with a brush, the thickness is controlled at 0.6mm, and stick on the breathable fluorine-four paint cloth. After pressurizing and curing at room temperature for 30 minutes, heat and cure at 80℃ for 2 hours. After heating, the breathable fluorine-four paint cloth can be removed, and a rapid heating test of 140℃ / s is carried out. When the temperature is raised to 1200℃, the sensor is not well bonded, and large pieces fall off and warping occur.
[0218] It can be seen from the above test results that the inorganic phosphate special high temperature resistant adhesive provided by the present invention is a special high temperature resistant adhesive for sensor pasting that needs to undergo rapid temperature shock under high temperature environment. It undergoes a rapid heating process of 100-150℃ / s from room temperature to 1200℃, and is firmly bonded to the bonding substrate without falling off, breakage, cracks, bulging and other poor contact phenomena. The effect rate of high temperature test is fast, and the repeatability of multiple high temperature tests is good. It has a long operation period of 15-30min at room temperature, and can be quickly dried on the surface of the substrate after being coated on the surface of the substrate. The adhesive can be cured by curing at room temperature for 1h and then at 80℃ for 2h, or curing at room temperature for 1 day, and the curing temperature and curing process are simple. After curing, the thermal weight loss in air from room temperature to 1200℃ is ≤5%, and the compressive shear strength at room temperature is 0.5-3MPa, and the compressive shear strength at 1200℃ is 0.2-1MPa. After the test, the high temperature glue is easy to remove from the surface without damaging the test substrate. The adhesive does not corrode the test sample and does not affect its mechanical properties.
[0219] In summary, the adhesive of the present invention has suitable bonding strength at both room temperature and high temperature environment (room temperature RT ~ 1200°C) after curing, and is suitable for sensor pasting in high temperature environment, especially for high temperature resistant pasting of sensors that need to undergo rapid heating of 100 ~ 150°C / s.
[0220] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
[0221] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.
Claims
1. A high temperature resistant adhesive for bonding sensors, characterized in that: It includes a phosphate solution and a composite filler, wherein the mass ratio of the phosphate solution to the composite filler is 100:85-120; The density of phosphate solution is 1.60~1.80g / cm 3 ; The composite filler comprises an auxiliary filler and a curing agent, wherein the auxiliary filler comprises mullite fiber and silicon dioxide, and further comprises one or more of aluminum oxide, titanium dioxide or chromium trioxide.
2. The sensor bonding high temperature resistant adhesive according to claim 1, characterized in that: The phosphate solution is one or more of an aluminum phosphate solution or a chromium aluminum phosphate solution.
3. The sensor bonding high temperature resistant adhesive according to claim 1, characterized in that: The curing agent is fused magnesium oxide; The mass ratio of the curing agent to the auxiliary filler is 0.1 to 0.
2.
4. The sensor bonding high temperature resistant adhesive according to claim 1, characterized in that: The mass ratio of the phosphate solution to the composite filler is 100:86-100.
5. The sensor bonding high temperature resistant adhesive according to claim 2, characterized in that: The synthesis method of aluminum phosphate solution comprises: Phosphoric acid with a concentration of ≥85%, aluminum hydroxide and water are mixed and refluxed at 90-120°C for 0.5-2h to obtain an aluminum dihydrogen phosphate solution; the mass ratio of phosphoric acid, aluminum hydroxide and water is 100:20-33.3:48-80; The aluminum dihydrogen phosphate solution is evaporated at a temperature of 50 to 120° C. for 0.5 to 4 hours, and the density of the solution is adjusted to a desired density to obtain an aluminum phosphate solution having a desired density; The synthesis method of aluminum chromium phosphate solution comprises: Phosphoric acid with a concentration of ≥85%, aluminum hydroxide, chromium oxide and water are mixed and refluxed at 90-120° C. for 0.5-2 hours to obtain a chromium aluminum phosphate solution; the mass ratio of phosphoric acid, aluminum hydroxide, chromium oxide and water is 100:20-33.3:10-20:48-80. The aluminum chromium phosphate solution is evaporated at a temperature of 50 to 120° C. for 0.5 to 4 hours, and the density of the solution is adjusted to a desired density to obtain an aluminum chromium phosphate solution with a desired density.
6. The sensor bonding high temperature resistant adhesive according to claim 1, characterized in that: The particle size of the composite filler is 0.5 to 10 μm.
7. The sensor bonding high temperature resistant adhesive according to claim 1, characterized in that: The preparation method of the composite filler comprises: The curing agent and the auxiliary filler are mixed and ball-milled in a ball mill for 4 to 8 hours to obtain a powder; the rotation speed of the ball mill is 100 to 250 rpm; The powder is sieved and dried in an oven for 1 to 5 hours at a drying temperature of 100 to 200°C; The composite filler is obtained by natural drying and cooling.
8. A method for using a high temperature resistant adhesive for bonding a sensor according to any one of claims 1 to 7, characterized in that: include: Under room temperature, the phosphate solution and the composite filler are mixed and stirred to obtain an adhesive; Apply adhesive on the surface of the substrate to be bonded, and bond the sensor to the surface of the substrate to be bonded; The sensor surface is covered with breathable fluorine-free varnished cloth, and a pressurizing mechanism acts on the breathable fluorine-free varnished cloth to perform pressurized curing; Remove the breathable fluorocarbon paint cloth and the bonding is completed.
9. The method for using the high temperature resistant adhesive for bonding sensors according to claim 8, characterized in that: At room temperature, the phosphate solution and the composite filler are repeatedly ground and mixed in a mortar to be uniform; The thickness of the adhesive applied on the surface of the substrate to be bonded is 0.05 to 0.3 mm; Methods of pressure curing include: After pressurizing and curing at room temperature for 30 minutes to 1 hour, pressurize and cure at 80°C ± 5°C for 1 to 3 hours or pressurize and cure at room temperature for 1 to 2 days; during the curing process, maintain the pressure at 0.01 to 0.05 atmospheres.
10. The method for using a high temperature resistant adhesive for bonding a sensor according to claim 8, characterized in that: The sensor is a sensor that can withstand rapid temperature shock at 1200°C; the rapid temperature shock at 1200°C means that the sensor undergoes a rapid temperature rise process of 100-150°C / s from room temperature to 1200°C.
Citation Information
Cited By
Bonding material for packaging quantum current sensor, sensor and process manufacturing method
CN122445290A
Adhesive material for quantum current sensor package, sensor and process of making
CN122445290B