Adhesive, adhesive tape and preparation method and application thereof

The adhesive made of crosslinked adhesive composition, combined with weak alkaline solution removal technology, solves the problem of adhesiveness and difficulty in removing pyrolytic adhesive tape in multi-layer ceramic film cutting and processing, and realizes the stability of the ceramic film Adhesion and efficient cutting improve product quality.

CN119039930APending Publication Date: 2024-11-29CHAOZHOU THREE CIRCLE GRP CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411128831.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing pyrolytic adhesive tape cannot take into account the high viscosity during processing and the easy removal after processing in the cutting of multi-layer ceramic films, resulting in defects such as displacement of ceramic films, reduced processing accuracy and residual glue, which seriously reduces product goodness. Rate.

Method used

Provide an adhesive made of crosslinked adhesive composition, including organic acids, acrylates and photoinitiators, to remove the adhesive by soaking in weak alkaline solution, avoiding thermal detachment phenomenon, and is suitable for multi-layer ceramic films. Fixing and cutting.

Benefits of technology

The good adhesive and easy removal characteristics of the adhesive in the cutting and processing of multi-layer ceramic films are achieved, avoiding the reverse adhesive of the ceramic films when heat loss is lost, and improving processing accuracy and product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997240940000051
    Figure BDA0004997240940000051
  • Figure BDA0004997240940000061
    Figure BDA0004997240940000061
  • Figure BDA0004997240940000071
    Figure BDA0004997240940000071
Patent Text Reader

Abstract

The invention belongs to the field of adhesives, and particularly discloses an adhesive, an adhesive tape as well as a preparation method and application of the adhesive tape. The adhesive provided by the invention has proper viscosity, can be removed through simple soaking in a weakly alkaline solution after being bonded with a plurality of layers of ceramic films, does not need thermal viscosity loss, can avoid the anti-adhesion condition of the ceramic films during thermal viscosity loss, and has the characteristics of good viscosity and easiness in removal; the multi-layer ceramic film fixing device is suitable for fixing multi-layer ceramic films in multi-layer ceramic film cutting processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of adhesives, and in particular relates to an adhesive, an adhesive tape, and a preparation method and application thereof. Background Art

[0002] The preparation process of multilayer chip components, such as chip multilayer ceramic capacitors, inductors, resistors, filters, etc., includes: casting ceramic slurry on a release film to form a very thin ceramic film; cutting the film into small pieces and then printing the circuit; then stacking these ceramic films layer by layer, and after the stacking is completed, cutting them into small pieces of multilayer ceramic film components.

[0003] During the lamination process, in order to ensure that the ceramic films can be firmly bonded, each layer of ceramic film needs to be pressed with great pressure when it is stacked, and it needs to be constructed on a heating platform to soften the ceramic film. When each layer of ceramic film is stacked, it is necessary to ensure that each piece is accurately aligned, so there must be an adhesive tape on the heating platform to fix the ceramic film. Currently, a low-temperature debonding tape is mainly used. This tape adheres to the ceramic film at high temperature. After the lamination is completed, the viscosity decreases at low temperature and can be easily removed from the ceramic film.

[0004] After lamination, the multilayer ceramic film needs to be cut. At this time, it is also necessary to work on a heating platform to soften the ceramic and avoid damage to the blade. In order to prevent the displacement of small ceramic pieces during cutting, tape is also needed to fix the small ceramic pieces. After cutting, the fixing tape needs to be removed. Ordinary high-viscosity tape can ensure that it does not shift during cutting, but it is difficult to remove. At present, many manufacturers use pyrolytic adhesive tape when cutting. The characteristics of pyrolytic adhesive tape are: it has high viscosity at room temperature. After heating to a specific temperature, the expanding particles contained in the tape will expand, reducing the bonding area between the adhesive and the object to be attached, so that the viscosity is rapidly reduced, thereby achieving the effect of easy removal. This type of thermal debonding tape generally includes two categories: tape that loses adhesion at relatively high temperatures (the debonding temperature is as high as over 120°C) and tape that loses adhesion at relatively low temperatures (the debonding temperature is about 80-100°C). When using tape that loses adhesion at relatively high temperatures, since the debonding temperature is as high as over 120°C, the tape debonding process will cause the green body to stick back after cutting. When using tape that loses adhesion at relatively low temperatures, the viscosity will drop sharply at a cutting temperature of 80-90°C, which cannot meet the high-temperature cutting requirements of ceramic films.

[0005] In addition, thermally-dispersible adhesive tapes have the following problems: (1) Thermally-dispersible adhesive tapes have high viscosity at room temperature. Such tapes are provided with a release film on the surface to protect the adhesive surface. When using the tapes, it is necessary to remove the release film, which makes it inconvenient for the robot to operate the tapes. (2) The adhesive layer of the thermally-dispersible adhesive tapes is too soft, and when the pressure is too high, it will cause adhesive overflow. And because the stacking and cutting processes are different, the requirements for the viscosity change of the tape are also different. The low-temperature debonding tape used in the above stacking process is not suitable for the cutting process. The specific reasons are as follows: during stacking, the peeling force requirement for the tape at high temperature is relatively low, and when removing, because it is removed in pieces, the requirement for the reduction in peeling force after low-temperature debonding is not very high; during cutting, the friction of the blade on the small ceramic pieces is very large, and a higher peeling force is required during high-temperature processes. After cutting, because the volume of the finished product after cutting is very small (a few millimeters or a few tenths of a millimeter), the requirement for the reduction in peeling force is very high. If the peeling force is slightly larger, the small ceramic pieces will be difficult to pick up, but the peeling force of the low-temperature debonding tape is difficult to reduce to a very low level, so it is not suitable to use the low-temperature debonding type in the cutting process, and picking failures often occur.

[0006] Based on the above situation, in the current multi-layer ceramic film cutting process, due to the lack of relatively suitable tapes, the tape adhesion during the processing is often poor, resulting in the displacement of the ceramic film and reducing the processing accuracy, or the tape on the multi-layer ceramic film is difficult to remove, resulting in residual adhesive in the ceramic film and other defects, which seriously reduces the yield of the cutting product. Summary of the invention

[0007] In view of the problem that the fixing tape used in the multilayer ceramic film cutting process involved in the above-mentioned prior art cannot take into account both high viscosity during processing and easy removal after processing, the present invention will provide an adhesive, a tape and a preparation method and application thereof.

[0008] To achieve the above purpose, the following technical solutions are specifically included:

[0009] In one aspect, the present invention provides an adhesive, which is prepared by cross-linking an adhesive composition, wherein the adhesive composition comprises the following components in percentage by weight: 4-16% of an organic acid, 15-70% of a first acrylate, 20-63% of a second acrylate, 2-9% of a third acrylate, and 0.3-5% of a photoinitiator;

[0010] The second acrylate includes polyurethane acrylate, and the third acrylate includes polyglycol diacrylate.

[0011] The adhesive of the present invention has suitable viscosity. After being bonded to the multi-layer ceramic film, it can be removed by simply soaking in a weak alkaline solution without thermal debonding. This can avoid the reverse sticking of the ceramic film during thermal debonding. It can have both good viscosity and easy removal characteristics, and is suitable for fixing the multi-layer ceramic film during the cutting process of the multi-layer ceramic film.

[0012] Preferably, the organic acid comprises at least one of an organic phosphoric acid and an organic carboxylic acid.

[0013] Preferably, the organic acid includes at least one of methacrylic acid, acrylic acid and maleic acid.

[0014] Organic acid contains acidic groups. In the adhesive, when the content of organic acid is less than 4wt%, the adhesive is too sticky and difficult to remove. When the content of organic acid is greater than 16wt%, the adhesive is too sticky and its hygroscopicity deteriorates, resulting in poor bonding effect and inability to bond and fix multilayer ceramic films.

[0015] The first acrylate, the second acrylate, and the third acrylate are each selected from different acrylates.

[0016] Preferably, the first acrylic acid ester includes at least one of n-butyl acrylate, ethyl methacrylate, n-butyl methacrylate, isooctyl methacrylate, lauryl methacrylate, tetrahydrofuran acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and cyclohexyl acrylate.

[0017] In the adhesive, if the first acrylate content is too low, the viscosity of the adhesive composition is too high, the thickness of the adhesive layer obtained by casting is uneven, and it is difficult to cast a qualified adhesive layer; if the first acrylate content is too high, the adhesive has low viscosity and the peel strength of the adhesive layer will be reduced.

[0018] The second acrylate is polyurethane acrylate, and there is no strict requirement for the structure of polyurethane. Polyurethane is polymerized by polyol and isocyanate, and the polyol is not limited to polyester polyol or polyether polyol, and the isocyanate is not limited to aliphatic or aromatic. The polyurethane acrylate is a polyurethane acrylate prepolymer terminated with hydroxyethyl acrylate with unsaturated double bonds, and the prepolymer monomer elongation is required to be ≥120%, preferably ≥200%.

[0019] In the adhesive, if the content of the second acrylate is too low, the adhesive will shrink greatly upon curing, and the adhesive layer obtained by casting will be deformed, affecting the appearance of the adhesive layer and significantly reducing the peeling force of the cast adhesive layer; if the content of the second acrylate is too high, the viscosity of the adhesive composition will be too high, and the adhesive layer obtained by casting will be uneven in thickness, making it difficult to cast a qualified adhesive layer, and it will also be difficult to form, which cannot meet actual needs.

[0020] Preferably, the polyglycol diacrylate includes at least one of polyethylene glycol diacrylate and propoxylated neopentyl glycol diacrylate.

[0021] Preferably, the weight average molecular weight of the polyglycol diacrylate is 400-600;

[0022] Preferably, based on the polymerization degree of the polyoxyethylene groups, the polymerization degree of the polyoxyethylene groups in the polyglycol diacrylate is ≥6.

[0023] In the adhesive, if the content of the third acrylate is too small, the adhesive will be fluid at higher temperatures and will not be suitable for cutting ceramic green bodies. The adhesive layer will easily adhere to the product when peeling. If the content of the third acrylate is too high, the wettability of the adhesive to the substrate will deteriorate and the peeling force of the adhesive layer will be significantly reduced.

[0024] Preferably, the photoinitiator includes at least one of phosphine oxides and hydroxybenzophenones; further preferably, the photoinitiator includes at least one of trimethylbenzoyl-diphenylphosphine oxide (TPO), bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (819), 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173), and hydroxycyclohexane phenone (184). In the adhesive, if the content of the photoinitiator is too low, the adhesive will not be completely cured, which will seriously affect the adhesion of the adhesive layer; if the content of the photoinitiator is too high, it will cause waste and may also cause violent polymerization in some cases.

[0025] In a second aspect, the present invention provides an adhesive tape comprising a base film, a release film, and an adhesive layer between the base film and the release film, wherein the adhesive layer is composed of the adhesive.

[0026] Preferably, the base film comprises PET, PC or PI.

[0027] Preferably, the isolation film comprises a PET film coated with an isolation silicone oil layer on one side.

[0028] The base film is the carrier of the adhesive; when not in use, the isolation film is used to protect the adhesive layer to prevent contamination of the adhesive layer. The upper surface of the isolation film is coated with isolation silicone oil to ensure that the adhesive layer is not contaminated.

[0029] In a third aspect, the present invention provides a method for preparing the adhesive tape, comprising the following steps:

[0030] (1) mixing an organic acid, a first acrylate, a third acrylate and a photoinitiator uniformly, and then adding the second acrylate and mixing uniformly to obtain an adhesive composition;

[0031] (2) The adhesive composition is coated on a base film, covered with a release film, and then light-cured to obtain the adhesive tape.

[0032] Preferably, in step (1), the uniform mixing is achieved by stirring, the stirring time is 1-5 h, and the stirring rate is 10-100 rpm.

[0033] Preferably, in step (2), the coating thickness is 15-100 μm. If the coating thickness is less than 15 μm, the peeling force of the adhesive layer is reduced, and if the coating thickness is greater than 100 μm, it will lead to cost waste.

[0034] Preferably, during the light curing, the light intensity is 1800-3000 mW / cm 2 .

[0035] In a fourth aspect, the present invention further provides a use of the adhesive or the tape in preparing a multilayer ceramic thin film element.

[0036] Preferably, when the adhesive tape is used in the preparation of a multilayer ceramic thin film element, the isolation film on the adhesive tape is removed, the adhesive layer is attached to the ceramic green body, and cutting is performed. After the cutting is completed, the multilayer ceramic film containing the adhesive layer is immersed in a stripping agent. After the multilayer ceramic film and the adhesive layer are separated, the multilayer ceramic film is dried to obtain a multilayer ceramic thin film element.

[0037] Preferably, the stripping agent is an alkaline solution, the alkaline solution contains 2-5% by mass of an alkaline reagent, the alkaline reagent includes ammonia water and bicarbonate; the bicarbonate includes sodium bicarbonate.

[0038] Preferably, the immersion time is 5-60 min.

[0039] Compared with the prior art, the present invention has the following beneficial effects: the adhesive of the present invention has suitable viscosity, and after being bonded to the multi-layer ceramic film, it can be removed by simply soaking in a weak alkaline solution without thermal debonding, which can avoid the anti-sticking phenomenon of the ceramic film during thermal debonding, and can take into account the characteristics of good viscosity and easy removal, and is suitable for fixing the multi-layer ceramic film during the cutting process of the multi-layer ceramic film. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic diagram of the structure of the adhesive tape of the present invention.

[0041] Figure 2 Schematic diagram of 180° peel strength test of adhesive layer (adhesive). DETAILED DESCRIPTION

[0042] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below through specific examples. The test methods used in the examples and / or comparative examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial channels unless otherwise specified. Among them, the polyurethane acrylates used below are all the same, namely commercially available DR-U384.

[0043] Examples 1-33 and Comparative Examples 1-19

[0044] A method for preparing an adhesive tape comprises the following steps:

[0045] (1) According to the ratio in Table 1, an organic acid, a first acrylate, a third acrylate and a photoinitiator are weighed in a stirring kettle, and stirred at a stirring rate of 45 rpm for 1.5 h; then the second acrylate is added, and stirred at a stirring rate of 10 rpm for 1.5 h, and then stirred at a stirring rate of 50 rpm for 3 h. After stirring, the mixture is discharged to obtain an adhesive composition;

[0046] (2) The adhesive composition was cast onto the base film using a doctor blade casting machine, and the isolation film (PET film with an isolation silicone oil layer on one side) was covered. 2 The adhesive composition is cross-linked and cured to form an adhesive layer with an adhesive function, thereby obtaining an adhesive tape;

[0047] The adhesive tape includes a base film, an adhesive layer and a separation film from bottom to top. Figure 1 As shown, the thickness of the adhesive layer and the material of the base film involved in each embodiment and comparative example are shown in Table 1.

[0048] Comparative Example 20

[0049] In this comparative example, a commercially available heat-debonding pressure-sensitive adhesive is used, and the peeling temperature is 120-150°C.

[0050] Table 1

[0051]

[0052]

[0053]

[0054]

[0055] Application example: When the adhesive tapes of the above embodiments and comparative examples are used in the preparation of multilayer ceramic thin film components, the isolation film on the adhesive tape is removed, the adhesive layer is attached to the ceramic green body, and cutting is performed. After the cutting is completed, the multilayer ceramic film containing the adhesive layer is immersed in a stripping agent, and after the multilayer ceramic film and the adhesive layer are separated, the multilayer ceramic film is dried to obtain a multilayer ceramic capacitor. The stripping agent is an alkaline solution, and the alkaline solution is a sodium bicarbonate solution containing 3% by mass, and the immersion time is 30 minutes.

[0056] The adhesive tapes in the above embodiments and comparative examples were subjected to the following performance tests:

[0057] (1) Initial adhesion: Tested according to GB / T4852-2002(A), the initial adhesion is qualified if the rolling distance is less than 5 cm;

[0058] (2) 180° peel strength: Cut a 10mm*250mm wide adhesive layer and attach it to an acrylic board with an attachment area of ​​10mm*80mm. Measure the 180° peel strength. Figure 2 As shown; 180° peel strength>40gf / 10mm is considered qualified;

[0059] (3) Evaluation of peeling effect: 2mm*2mm*2mm acrylic resin blocks were attached to the adhesive layer of each embodiment and comparative tape in an array of 100*100. The acrylic resin blocks would stick to each other when heated above 80°C. They were heated on a hot plate at 60°C for 1 min. During the heating process, the resin blocks were pressed with a roller. After cooling, they were set aside. A 5% by mass NaHCO 3 Place the tape with the acrylic resin block attached into the prepared NaHCO 3 In aqueous solution, observe the shedding condition every 5 minutes. The soaking time is less than 30 minutes. Then centrifuge and dehydrate, and observe the adhesion or appearance of the polypropylene resin block after detachment. When the time for all acrylic resin blocks to detach is ≤30 minutes, it is considered qualified. If the detachment condition in the following Table 2 is a time period, it means that the polypropylene resin block can be 100% detached within this time period. For example, 15 to 20 minutes means that the polypropylene resin block is not completely detached in 15 minutes, and it is 100% detached in 20 minutes. If it is a percentage, it indicates the percentage of polypropylene resin blocks that can be detached in 30 minutes. Because the adhesive layer of the tape has a greater viscosity when it is attached to the acrylic resin block than when it is attached to the ceramic film, if the peeling property of the acrylic resin block is relatively good, the peeling effect of the ceramic film product will be better.

[0060] (4) Application product testing: The percentage of residual adhesive and product defects on 1,000 multilayer ceramic strip capacitors in each embodiment and comparative example of the application example was counted.

[0061] The performance test results are shown in Table 2.

[0062] Table 2

[0063]

[0064]

[0065]

[0066]

[0067] It can be seen from Examples 1-33 and Comparative Example 20 that the adhesive layer formed by the adhesive of the present invention has suitable viscosity. After being bonded to the multi-layer ceramic film, it can be removed by simply soaking in a weak alkaline solution without thermal debonding. This can avoid the reverse sticking of the ceramic film during thermal debonding. It can take into account both good viscosity and easy removal, and will not cause the product to be unqualified after peeling off the adhesive layer. It is very suitable for fixing multi-layer ceramic films in the multi-layer ceramic film cutting process.

[0068] It can be seen from the comparison between Examples 1-33 and Comparative Examples 1-2 and Comparative Examples 11-12 that if the organic acid content is too little, the adhesive film is uneven, the initial adhesion and peeling strength are large, the polypropylene resin block falls off poorly, the adhesive layer is too sticky, and it is difficult to remove the adhesive layer, resulting in a decrease in the qualified rate of products peeling the adhesive layer; if the organic acid content is too much, the viscosity is too low, and the adhesive layer is not sticky enough, which cannot meet the requirements of fixing the object to be bonded. Therefore, in the adhesive of the present invention, the content of organic acid is selected to be 4-16wt%. Within this range, the adhesive has appropriate viscosity and peeling strength, and will not cause the product to be unqualified.

[0069] By comparing Examples 1-33 with Comparative Examples 3-4 and 13-14, it can be seen that if the content of the first acrylate is too low, the viscosity of the adhesive composition is too high, the thickness of the adhesive layer obtained by casting is uneven, and it is difficult to form, the peel strength is too high, it is difficult to fall off, and the adhesive layer is difficult to remove, resulting in a decrease in the qualified rate of products with peeled adhesive layers, which cannot meet actual needs; if the content of the first acrylate is too high, the viscosity is low, the initial adhesion and peel strength are too low, it is very easy to fall off, and the adhesive layer cannot stabilize the multilayer ceramic film, resulting in a decrease in the qualified rate of products with peeled adhesive layers. Therefore, the content of the first polyacrylate of the present invention is selected to be 15-70wt%. Within this range, the viscosity and peel strength of the adhesive are appropriate, and the product will not be unqualified.

[0070] It can be seen from Examples 1-33 and Comparative Examples 5-6 and 13-14 that if the content of the second acrylate is too low, the adhesive will shrink greatly upon curing, and the adhesive layer obtained by casting will be deformed, affecting the appearance of the adhesive layer; if the peel strength is too low, the polypropylene resin block will fall off poorly and residual adhesive will be left behind, resulting in a decrease in the qualified rate of products after peeling the adhesive layer. If the content of the second acrylate is too high, the viscosity of the adhesive composition will be too high, and the thickness of the adhesive layer obtained by casting will be uneven, making it difficult to cast a qualified adhesive layer, and molding will be difficult. Although the initial adhesion and peel strength are qualified, the polypropylene resin block will fall off poorly and residual adhesive will be left behind, resulting in a decrease in the qualified rate of products after peeling the adhesive layer. Therefore, the content of the second polyacrylate of the present invention is selected to be 20-63wt%. Within this range, the viscosity and peel strength of the adhesive are appropriate, and the product will not be unqualified.

[0071] It can be seen from Examples 1-33 and Comparative Examples 7-8, 15-16 that if the content of the third acrylate is too small, the initial viscosity is large and the peel strength is small, the polypropylene resin block is difficult to fall off and residual adhesive will be left, the adhesive will have fluidity at a higher temperature, and it is not suitable for cutting ceramic green bodies. When the adhesive layer is peeled off, it is easy to adhere to the product, resulting in a decrease in the qualified rate of products with peeled adhesive layers. If the content of the third acrylate is too high, although the initial viscosity is appropriate, the peel strength is significantly reduced, the wettability of the adhesive to the substrate becomes poor, and the multi-layer ceramic film cannot be fixed, resulting in a decrease in the qualified rate of products with peeled adhesive layers. Therefore, the content of the third polyacrylate of the present invention is selected to be 2-9wt%. Within this range, the viscosity and peel strength of the adhesive are appropriate, and the product will not be unqualified.

[0072] It can be seen from Examples 1-33 and Comparative Examples 9-10, 17-18 that if the photoinitiator is too little, the initial viscosity and peeling strength are small, the polypropylene resin block is easy to fall off, and the adhesive layer has a strong smell and is sticky, and the multi-layer ceramic film cannot be fixed, resulting in a decrease in the qualified rate of the product with peeled adhesive layer; if the photoinitiator content is too much, the adhesive film shrinks severely, there is scorching in the middle, and the polypropylene resin block locally explodes to form small bubbles, which cannot be used. Therefore, the content of the photoinitiator of the present invention is selected to be 0.3-5wt%. Within this range, the viscosity and peeling strength of the adhesive are appropriate, and the product will not be unqualified.

[0073] It can be seen from Examples 1-33 and Comparative Example 19 that if the thickness of the adhesive layer is too small, the initial adhesion and peeling strength are very small, and the acrylic resin block is seriously adhered, which easily leads to residual adhesive in the product, resulting in a decrease in the qualified rate of the product after peeling the adhesive layer. Therefore, it is more appropriate to select a thickness of ≥15μm for the adhesive layer.

[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. An adhesive, It is characterized in that The adhesive composition is prepared by cross-linking, wherein the adhesive composition comprises the following components in percentage by weight: 4-16% organic acid, 15-70% first acrylate, 20-63% second acrylate, 2-9% third acrylate, and 0.3-5% photoinitiator; The second acrylate includes polyurethane acrylate, and the third acrylate includes polyglycol diacrylate.

2. The adhesive according to claim 1, It is characterized in that The organic acid includes at least one of organic phosphoric acid and organic carboxylic acid.

3. The adhesive according to claim 1, It is characterized in that The first acrylic acid ester includes at least one of n-butyl acrylate, ethyl methacrylate, n-butyl methacrylate, isooctyl methacrylate, lauryl methacrylate, tetrahydrofuran acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and cyclohexyl acrylate.

4. The adhesive according to claim 1, It is characterized in that The polyglycol diacrylate includes at least one of polyethylene glycol diacrylate and propoxylated neopentyl glycol diacrylate.

5. The adhesive according to claim 1, It is characterized in that Include at least one of the following: The weight average molecular weight of the polyglycol diacrylate is 400-600; Calculated by the polymerization degree of the polyoxyethylene groups, the polymerization degree of the polyoxyethylene groups in the polyglycol diacrylate is ≥6.

6. The adhesive according to claim 1, It is characterized in that The photoinitiator includes at least one of phosphine oxides and hydroxybenzophenones.

7. An adhesive tape, It is characterized in that The invention comprises a base film, an isolation film and an adhesive layer between the base film and the isolation film, wherein the adhesive layer is composed of the adhesive according to any one of claims 1 to 6.

8. A method for preparing the adhesive tape according to claim 7, It is characterized in that The steps include: (1) mixing an organic acid, a first acrylate, a third acrylate and a photoinitiator uniformly, and then adding the second acrylate and mixing uniformly to obtain an adhesive composition; (2) The adhesive composition is coated on a base film, covered with a release film, and then light-cured to obtain the adhesive tape.

9. The method for preparing the adhesive tape according to claim 8, It is characterized in that In step (2), the coating thickness is 15-100 μm.

10. Use of the adhesive according to any one of claims 1 to 6 or the adhesive tape according to claim 7 in the preparation of a multilayer ceramic thin film element.

Citation Information

Cited By

  • Adhesive sheet for back-grinding wafer

    TWI914208B