Modified multilayer transparent conductive film suitable for copper gate heterojunction battery
By using modified multi-layer transparent conductive films with ITO, SnOx and SnOx-F-Cu layers in heterojunction solar cells, the problems of high cost and TCO film damage in traditional silver paste processes are solved, and cost reduction and efficiency improvement are achieved .
Patent Information
- Application Number
- CN202411510715.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The high cost caused by the traditional silver paste process and the impact of TCO film damage and high-temperature annealing on amorphous silicon films during copper gate preparation limit the industrial promotion of heterojunction solar cells.
A modified multi-layer transparent conductive film including ITO layer, SnOx layer and SnOx-F-Cu layer is used, and is deposited by magnetron sputtering technology to avoid vacuum high-temperature annealing, reduce costs and improve conductivity and adhesion.
It effectively reduces costs, improves the conversion efficiency and service life of the battery. Through the corrosion resistance of the SnOx layer and the electrical conductivity and toughness of the SnOx-F-Cu layer, the problem of insufficient adhesion of the copper gate wire is solved.
Smart Images

Figure CN119050175A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of heterojunction solar cells, and in particular to a modified multilayer transparent conductive film suitable for copper grid heterojunction cells and a silicon heterojunction solar cell. Background Art
[0002] Metallization is one of the key processes in the preparation of solar cells. The traditional process mainly uses silver paste to make solar cell electrodes. For various high-efficiency solar cell technologies, the cost of silver paste is second only to silicon wafers. The silver paste cost of Passivated Emitter Rear Cell (PERC) accounts for 10-11% of the battery cost, while for Tunnel O2ide Passivated Contact (TOPCON) and Heterojunction with Intrinsic Thin-film (HJT), the silver paste cost is further increased to more than 16%-24%. Such high cost expenditure has become an important factor restricting the industrialization and promotion of TOPCON and HJT batteries.
[0003] Transparent conductive film TCO (Transparent conducting o2ide) is an indispensable part of heterojunction solar cells as a lateral carrier transport layer.
[0004] Electroplating technology is the process of depositing a thin layer of metal, alloy or composite material on the surface of the conductive layer by electrochemical methods. Copper electroplating is a non-contact electrode metallization technology. The basic principle of the process is to deposit metallic copper on the surface of the base metal through electrolytic chemical reaction to make copper grid lines and collect carriers generated by the photovoltaic effect. The main difference between copper electroplating technology and traditional screen printing technology is after the TCO process. Traditional heterojunction production lines will print and cure silver paste after the TCO process; the copper electroplating process is mainly divided into two parts: the patterning and metallization of the grid lines. After the TCO film of the patterned part, silver paste printing is not used, but the electrode grid lines are prepared by electroplating copper. In this way, copper is used instead of silver as the grid line material, which significantly reduces the cost of battery metallization materials.
[0005] Moreover, compared with silver grid line printing technology, the electrode grid lines prepared by copper grid line electroplating technology have less light shielding and lower contact resistance, thus becoming one of the important ways to improve the photoelectric conversion efficiency of heterojunction cells. However, the original copper grid heterojunction has the following problems in the preparation process: (1) If high-temperature annealing is performed after the TCO film is deposited on the surface of the silicon wafer, the TCO film is easily damaged during the copper gate preparation process (the copper gate preparation process will come into contact with sulfuric acid and is easily etched); (2) In order to avoid damage to the TCO, the heterojunction battery semi-finished product (blue film) needs to be vacuum-annealed at high temperature (about 250°C) before the copper electroplating process. High-temperature annealing can easily have an adverse effect on the amorphous silicon film, thereby affecting the battery efficiency; (3) As the preferred TCO film, the price of indium is high in ITO film, which makes the cost of ITO film relatively high.
[0006] SnO x Thin film has good corrosion resistance and low cost. Partially replacing the ITO thin film with a tin oxide film to form a composite structure is expected to be a way to solve the above problems. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and to provide a modified multilayer transparent conductive film suitable for copper grid heterojunction batteries.
[0008] The technical solution adopted by the present invention is as follows: a modified multilayer transparent conductive film suitable for copper grid heterojunction battery, comprising an ITO layer, a SnO x layer.
[0009] Preferably, the thickness of the ITO layer is 30-50 nm, and the SnO x The thickness of the layer is 30-50 nm.
[0010] Preferably, it also includes depositing on the SnO x The SnO layer on the side away from the substrate surface x -F-Cu layer.
[0011] Preferably, the SnO x The thickness of the -F-Cu layer is 10-30 nm.
[0012] Preferably, SnO x In the -F-Cu layer, the content of F is 0.1-2%, and the content of Cu is 0.5-5%.
[0013] Preferably, the preparation method comprises the following steps: (1) ITO coating: Using ITO target and magnetron sputtering technology, a process gas containing Ar gas is introduced into a high vacuum chamber. The Ar gas dissociates under the action of the electric field to produce Ar + ,Ar + The ITO target is bombarded under the action of an electric field, so that the ITO is separated from the target surface and deposited on the substrate surface to form an ITO layer; (2) SnO platingx Layer: Using tin oxide target and magnetron sputtering technology, a process gas containing Ar gas is introduced into a high vacuum chamber. Ar gas dissociates under the action of an electric field to produce Ar + ,Ar + The tin oxide target is bombarded under the action of the electric field, causing the tin oxide to separate from the target surface and deposit on the substrate surface to form SnO x layer; Preferably, in step (1), an ITO target is used, and the vacuum chamber is heated to 150-250°C. When the vacuum degree in the vacuum chamber reaches 1×10 -5 When the pressure is below 0.1 Pa, process gas is introduced into the vacuum chamber, and the gas pressure is controlled between 0.1 and 10 Pa; a pulsed negative bias is applied to the substrate in the range of -100 to -500 V to cause glow discharge in the gas, and the sample is glow cleaned for 10 to 50 minutes; the flow rate of the protective gas is adjusted to make the pressure in the vacuum chamber 0.2 to 5.0 Pa, and the ITO target arc source is turned on at the same time, the arc current is 60 to 200 A, the pulsed negative bias is adjusted to -50 V to -500 V, and the duty cycle of the pulsed negative bias is adjusted to 30% to 70%, and the ITO layer is deposited.
[0014] Preferably, in step (2), a tin oxide target is used, and the tin oxide target arc source and the axial magnetic field device are turned on at the same time, the arc current is 30 to 150A, the pulse negative bias is adjusted to -50V to -500V, the pulse negative bias duty cycle is adjusted to 30% to 70%, the magnetic field coil current is adjusted to 0.3 to 4A, and the tin oxide target current is adjusted to 30 to 150A to deposit SnO x layer; Preferably, the method further comprises step (3), (3) SnO plating x -F-Cu layer: Fluorine-doped tin oxide target and copper target are used. Using magnetron sputtering technology, a process gas containing Ar gas is introduced into a high vacuum chamber. Ar gas dissociates under the action of an electric field to produce Ar + ,Ar + The fluorine-doped tin oxide target and copper target are bombarded under the action of an electric field, so that the fluorine-doped tin oxide and copper are separated from the target surface and deposited on the substrate surface to form SnO x -F-Cu layer.
[0015] Preferably, in step (3), a fluorine-doped tin oxide target and a copper target are used, a pulsed negative bias voltage of -50V to -300V is applied to the substrate, and the duty cycle of the pulsed negative bias voltage is 15% to 80%; the axial magnetic field device is turned on, and the current of the magnetic field coil is adjusted to 0.3 to 4A; the target current of the fluorine-doped tin oxide target and the copper target is adjusted to 30 to 150A to deposit SnO2-F-Cu surface.
[0016] The beneficial effects of the present invention are as follows: 1. The present invention prepares a layer of SnO on the surface of the heterojunction battery semi-finished product x Since tin oxide has good corrosion resistance, it can ensure corrosion resistance without annealing operation, and the vacuum annealing process of ITO film can be omitted. x The material price is low, which can effectively reduce costs.
[0017] 2. SnO x The conductive performance is poor, but the line width of the copper grid line is small. The use of a dense grid pattern can better avoid the efficiency loss of the copper grid heterojunction battery. However, the copper-plated grid line is affected by stress, and the adhesion of the copper-plated grid line is insufficient, and it is easy to fall off, resulting in grid line contact problems, affecting the later use of the battery and the component. The present invention further selects SnO x The SnO2-F-Cu layer is composited on the layer, and the hydrophilic F element is added to the SnO x On the one hand, the wettability of the SnO2 layer can be improved, so that the copper grid line can be better attached to the modified multi-layer transparent conductive film, thereby increasing its bonding force with the copper grid line, making the copper grid line less likely to fall off, and improving the service life of the battery and components; on the other hand, F - Will replace O 2- Or, the interstitial fluorine atoms are formed on the basis of the original tin oxide crystal structure, thereby significantly increasing the carrier concentration in the film, so the conductivity of the tin oxide film can be greatly improved; x Immiscible Cu is added to the SnO2-F layer, and Cu segregates in the SnO x At the grain boundary, SnO x phase, while Cu is mostly precipitated in nanocrystalline or amorphous structure, which is similar to SnO x Together they form a nano-composite structure, which improves the toughness of the surface, reduces the internal stress of the surface, improves the fracture toughness of the surface, and relieves impact, wear and lubricates the thin film layer between it and the surface of the heterojunction battery semi-finished product, reduces the friction coefficient, and further improves the service life of the battery and components.
[0018] 3. The present invention adopts magnetic field enhanced arc ion plating, which not only has a faster deposition rate, but also makes the obtained film layer denser, with good toughness, impact resistance and wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, without paying creative labor, other drawings obtained based on these drawings still belong to the scope of the present invention.
[0020] Figure 1 This is a schematic diagram of the structure of Embodiment 1 of the present invention; Figure 2 It is a schematic diagram of the structure of the invention embodiment 2-4; Figure 3 This is a static contact angle diagram of the modified multilayer transparent conductive film deposited in Example 1 of the present invention; Figure 4 This is a static contact angle diagram of the modified multilayer transparent conductive film deposited in Example 2 of the present invention; Figure 5 This is a static contact angle diagram of the modified multilayer transparent conductive film deposited in Example 3 of the present invention; Figure 6 This is a static contact angle diagram of the modified multilayer transparent conductive film deposited in Example 4 of the present invention; DETAILED DESCRIPTION In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.
[0021] Example 1 like Figure 1 As shown in the structure, the method for preparing the transparent conductive film of this embodiment includes the following steps: S1. Cleaning the substrate: Place the substrate (blue film) in acetone, isopropanol, ethanol and deionized water for ultrasonic cleaning in turn. Each cleaning time is 20 minutes and the cleaning temperature is 50°C. After ultrasonic cleaning, take out the substrate, wipe it clean with a dust-free cloth, and place it on the sample stage of the vacuum chamber to prepare for sputtering. S2. Sputtering: (1) Wait until the vacuum degree in the vacuum chamber reaches 5×10 -6 Pa, the vacuum chamber was heated to 200 ° C, the gas mass flow controller was turned on, and a mixture of argon and oxygen was introduced into the vacuum chamber. The ratio of argon and oxygen was 2:1, the gas flow rate was set to 280sccm, the gas pressure was controlled at 0.8Pa, a pulsed negative bias of -210V was applied to the substrate, the arc enhanced glow discharge ion source was turned on to make the gas glow discharge, and the sample was glow cleaned for 25 minutes; the flow rates of argon and oxygen were adjusted to make the vacuum chamber pressure 0.5Pa, and the ITO target arc source was turned on at the same time, the arc current was 90A, the pulsed negative bias was adjusted to -120V, and the pulsed negative bias duty cycle was 65%, and a 40 nm thick ITO layer was deposited; (2) Turn off the ITO target arc source, turn on the tin oxide target arc source, set the arc current to 100A, adjust the pulse negative bias to -90V, and the pulse negative bias duty cycle to 55%. Deposit a 40 nm thick SnO x layer.
[0022] After the deposition is completed, the arc is stopped, the substrate pulse negative bias voltage is stopped, the gas is stopped, the axial magnetic field device is turned off, and the vacuum is continued. The workpiece is cooled to room temperature with the furnace, the vacuum chamber is opened, the workpiece is taken out, and the coating process is completed. In this embodiment, the tin oxide target is a tin dioxide target.
[0023] The total thickness of the film prepared in this embodiment is 80 nm.
[0024] Example 2 like Figure 2 As shown in the structure, this embodiment further includes step S2.(3) based on embodiment 1: The arc source of the tin oxide target was turned off, the copper target was turned on, and a pulsed negative bias of -150 V was applied to the substrate, with a pulsed negative bias duty cycle of 45%. The current of the magnetic field coil was adjusted to 1.5 A. The current of the fluorine-doped tin oxide target and the copper target was adjusted to 95 A, and a 10 nm thick SnO was deposited. x -F-Cu layer.
[0025] In this embodiment, the fluorine-doped tin oxide target is a powder target obtained by mixing and drying a mixture of tin dioxide powder and fluoride, and the fluoride is an ammonium fluoride solution, wherein the content of F is 1.2%.
[0026] The total thickness of the film prepared in this embodiment is 90 nm.
[0027] Example 3 The difference between this embodiment and embodiment 2 is that the SnO layer with a thickness of 20 nm is deposited. x -F-Cu layer.
[0028] In this embodiment, the fluorine-doped tin oxide target is a powder target obtained by mixing and drying a mixture of tin dioxide powder and fluoride, and the fluoride is an ammonium fluoride solution, wherein the content of F is 1.2%.
[0029] The total thickness of the film prepared in this embodiment is 100 nm.
[0030] Example 4 The difference between this embodiment and embodiment 2 is that the SnO layer with a thickness of 30 nm is deposited. x -F-Cu layer.
[0031] In this embodiment, the fluorine-doped tin oxide target is a powder target obtained by mixing and drying a mixture of tin dioxide powder and fluoride, and the fluoride is an ammonium fluoride solution, wherein the content of F is 1.2%.
[0032] The total thickness of the film prepared in this example is 110 nm.
[0033] Comparative Example 1 The method for preparing the transparent conductive film of this comparative example comprises the following steps: S1. Cleaning the substrate: Place the substrate (blue film) in acetone, isopropanol, ethanol and deionized water for ultrasonic cleaning in turn. Each cleaning time is 20 minutes and the cleaning temperature is 50°C. After ultrasonic cleaning, take out the substrate, wipe it clean with a dust-free cloth, and place it on the sample stage of the vacuum chamber to prepare for sputtering. S2. Sputtering: (1) Wait until the vacuum degree in the vacuum chamber reaches 5×10 -6 Pa, the vacuum chamber is heated to 200°C, the gas mass flow controller is turned on, and a mixture of argon and oxygen is introduced into the vacuum chamber, the ratio of argon and oxygen is 2:1, the gas flow rate is set to 280sccm, the gas pressure is controlled at 0.8Pa, the substrate is subjected to a pulsed negative bias of -210V, the arc enhanced glow discharge ion source is turned on to cause the gas to glow discharge, and the sample is glow cleaned for 25 minutes; the flow rates of argon and oxygen are adjusted to make the vacuum chamber pressure 0.5Pa, and the ITO target arc source is turned on at the same time, the arc current is 90A, the pulsed negative bias is adjusted to -120V, and the pulsed negative bias duty cycle is 65%, and an 80 nm thick ITO layer is deposited. The total thickness of the film prepared in this embodiment is 80 nm.
[0034] The transparent conductive films prepared in Example 1 and Comparative Example 1 were subjected to annealing treatment and not subjected to annealing treatment, respectively, and the subsequent processes of preparing a copper seed layer and a copper grid were tested. The test results are shown in Table 1 below: Table 1 As shown in Table 1, we can see that: (1) Comparison between Scheme ① and Scheme ② shows that the electrical performance of the TCO single film of Scheme ① is similar, but the conversion efficiency is low after being made into a battery. This is mainly because the ITO has not been annealed and is damaged when etching the copper seed layer in the post-electroplating process, resulting in a large series resistance of the battery.
[0035] (2) Comparison between Scheme ① and Scheme ③ shows that the electrical performance of the TCO single film of Scheme ③ is worse, but after being made into a battery, the conversion efficiency is higher, mainly because SnO x The corrosion resistance is better. When the copper seed layer is etched in the post-electroplating process, the entire TCO surface is not damaged, which makes the series resistance of the battery smaller.
[0036] (3) Comparison between Scheme ② and Scheme ③ shows that the battery conversion efficiency of Scheme ③ is low, mainly because SnO x The poor electrical performance of the battery itself causes a large series resistance of the battery, forming a barrier to the transmission of carriers; this problem can be improved by using a dense grid pattern.
[0037] (4) Comparison between Scheme ③ and Scheme ④ shows that the problem in (3) can be improved by using dense grid patterns. x Thin film, the battery efficiency in Scheme ④ is close to the battery efficiency in Scheme ②.
[0038] (5) Comparison between Scheme ④ and Scheme ⑤ shows that the entire TCO film has better corrosion resistance due to the introduction of SnO x Regardless of whether the material has undergone vacuum annealing or not, the conversion efficiency remains basically the same after being made into a battery.
[0039] (6) The test error of the battery conversion efficiency tester itself is about 0.02%; if the absolute value of the battery conversion efficiency differs within 0.02%, it can be regarded that the battery efficiency is the same.
[0040] The transparent conductive films prepared in Examples 1-4 were tested for electrical properties, transmittance and wettability without annealing. The results are as follows: Figure 3-Figure 6 As shown in Table 2 below: Table 2 The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.
Claims
1. A modified multilayer transparent conductive film suitable for copper grid heterojunction battery, characterized in that: It includes an ITO layer, a SnO x layer, further comprising a SnO layer deposited on the x The SnO layer on the side away from the substrate surface x -F-Cu layer.
2. The modified multi-layer transparent conductive film suitable for copper grid heterojunction battery according to claim 1, characterized in that: The thickness of the ITO layer is 30-50 nm, and the SnO x The thickness of the layer is 30-50 nm.
3. The modified multi-layer transparent conductive film suitable for copper grid heterojunction battery according to claim 1, characterized in that: The SnO x The thickness of the -F-Cu layer is 10-30 nm.
4. The modified multi-layer transparent conductive film suitable for copper grid heterojunction battery according to claim 1, characterized in that: SnO x In the -F-Cu layer, the content of F is 0.1-2%, and the content of Cu is 0.5-5%.
5. A modified multi-layer transparent conductive film suitable for copper grid heterojunction battery according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) ITO coating: Using ITO target and magnetron sputtering technology, a process gas containing Ar gas is introduced into a high vacuum chamber. The Ar gas dissociates under the action of the electric field to produce Ar + ,Ar + The ITO target is bombarded under the action of an electric field, so that the ITO is separated from the target surface and deposited on the substrate surface to form an ITO layer; (2) SnO plating x Layer: Using tin oxide target and magnetron sputtering technology, a process gas containing Ar gas is introduced into a high vacuum chamber. Ar gas dissociates under the action of an electric field to produce Ar + ,Ar + The tin oxide target is bombarded under the action of the electric field, causing the tin oxide to separate from the target surface and deposit on the substrate surface to form SnO x layer.
6. The modified multi-layer transparent conductive film suitable for copper grid heterojunction battery according to claim 5, characterized in that: In step (1), an ITO target is used and the vacuum chamber is heated to 150-250°C. When the vacuum degree in the vacuum chamber reaches 1×10 - 5 When the pressure is below 0.1 Pa, process gas is introduced into the vacuum chamber, and the gas pressure is controlled between 0.1 and 10 Pa; a pulsed negative bias is applied to the substrate in the range of -100 to -500 V to cause glow discharge in the gas, and the sample is glow cleaned for 10 to 50 minutes; the flow rate of the protective gas is adjusted to make the pressure in the vacuum chamber 0.2 to 5.0 Pa, and the ITO target arc source is turned on at the same time, the arc current is 60 to 200 A, the pulsed negative bias is adjusted to -50 V to -500 V, and the duty cycle of the pulsed negative bias is adjusted to 30% to 70%, and the ITO layer is deposited.
7. The modified multi-layer transparent conductive film suitable for copper grid heterojunction battery according to claim 5, characterized in that: In step (2), a tin oxide target is used, and the tin oxide target arc source and the axial magnetic field device are turned on at the same time. The arc current is 30 to 150A, the pulse negative bias voltage is adjusted to -50V to -500V, the pulse negative bias voltage duty cycle is adjusted to 30% to 70%, the magnetic field coil current is adjusted to 0.3 to 4A, and the tin oxide target current is adjusted to 30 to 150A to deposit SnO x layer.
8. The modified multi-layer transparent conductive film suitable for copper grid heterojunction battery according to claim 5, characterized in that: It also includes step (3), (3) SnO plating x -F-Cu layer: Fluorine-doped tin oxide target and copper target are used. Using magnetron sputtering technology, a process gas containing Ar gas is introduced into a high vacuum chamber. Ar gas dissociates under the action of an electric field to produce Ar + ,Ar + The fluorine-doped tin oxide target and copper target are bombarded under the action of an electric field, so that the fluorine-doped tin oxide and copper are separated from the target surface and deposited on the substrate surface to form SnO x -F-Cu layer.
9. The modified multi-layer transparent conductive film suitable for copper grid heterojunction battery according to claim 8, characterized in that: In step (3), a fluorine-doped tin oxide target and a copper target are used to apply a pulsed negative bias voltage of -50V to -300V to the substrate, and the duty cycle of the pulsed negative bias voltage is 15% to 80%; the axial magnetic field device is turned on, and the current of the magnetic field coil is adjusted to 0.3 to 4A; the target current of the fluorine-doped tin oxide target and the copper target is adjusted to 30 to 150A to deposit the SnO2-F-Cu layer.
Citation Information
Patent Citations
Transparent conductive substrate for solar cell
CN101527325A
Copper doped tin oxide transparent conductive membrane and preparation method thereof
CN103137717A
Double-layer transparent conducting thin film and preparation method thereof
CN103993282A
Heterojunction solar cell and preparation method thereof
CN104752561A
Solar cell and preparation method thereof
CN118213418A