Monocrystalline silicon solar cell processing method

Through multiple dry etching and passivation film formation, the edge damage and fragility of single crystal silicon solar cell cells are solved, the conversion efficiency and flexibility are improved, and the preparation of high-efficiency flexible photovoltaic modules is realized.

CN119050202APending Publication Date: 2024-11-29LIUZHITAO NEW ENERGY TECH (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411167497.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-11
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Monocrystalline silicon solar cells are fragile during production and use, and the slicing process leads to edge damage and efficiency losses. The existing flexible photovoltaic technology is costly and difficult to achieve large-scale application.

Method used

Multiple dry etching methods are used to treat the edges of single crystal silicon solar cell, remove the functional film and structural damage layer, and perform smooth treatment to form a passivation film to improve flexibility and conversion efficiency.

Benefits of technology

It improves the conversion efficiency and reliability of single-crystal silicon solar cells, reduces the fragmentation rate and hidden cracking risks, imparts flexible characteristics, and realizes the preparation of high-efficiency flexible photovoltaic modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050202A_ABST
    Figure CN119050202A_ABST
Patent Text Reader

Abstract

The invention provides a monocrystalline silicon solar cell processing method, and the method comprises the steps: providing semiconductor processing equipment, stacking a plurality of monocrystalline silicon solar cells, and feeding the stacked monocrystalline silicon solar cells into the semiconductor processing equipment; the edge of the monocrystalline silicon solar cell piece is etched for multiple times, the etched monocrystalline silicon solar cell piece is obtained, the edge structure of the etched monocrystalline silicon solar cell piece is made to be smooth and free of a winding plating layer and a structural damage layer, and etching is dry etching; and passivating the edge of the etched monocrystalline silicon solar cell piece, and forming a passive film on the edge of the etched monocrystalline silicon solar cell piece. The problems of edge electric leakage, high fragmentation rate and easy subfissure of the monocrystalline silicon solar cell can be improved, the conversion efficiency and the flexibility of the monocrystalline silicon solar cell are improved, and the high-efficiency flexible monocrystalline silicon solar cell is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of solar cell processing, and in particular relates to a single crystal silicon solar cell processing method. Background Art

[0002] Crystalline silicon solar cells are the mainstream products of photovoltaics at present, accounting for more than 95%. The main development direction of crystalline silicon solar cells is high efficiency and low cost. In recent years, crystalline silicon solar cells have undergone a major change from polycrystalline to single crystal, from p-type to n-type, and have achieved mass production of various technical routes such as tunneling oxide passivation contact solar cells (PERC), tunneling oxide passivation contact solar cells (TOPCon), silicon heterojunction solar cells (HJT), and interdigitated back contact solar cells (IBC). The conversion efficiency has been greatly improved, with the highest conversion efficiency reaching more than 27%, and the mass production efficiency has gradually increased to more than 25%. The cost of solar cells and photovoltaic systems has dropped significantly. The application form of solar cells has also gradually developed from a single large-scale ground photovoltaic power station to a variety of application forms such as distributed photovoltaics, creating a good industrial and market ecological environment for the large-scale popularization of photovoltaic power generation.

[0003] However, monocrystalline silicon is a brittle material that is easily broken under external stress, and fragments are easily generated during the production process of monocrystalline silicon solar cells. During the production process of the components and during the transportation and use of the components after the production of the components, the cells encapsulated in the components will still produce hidden cracks or even breakage under the action of external stress, such as wind pressure generated by strong winds and mechanical stress during installation, resulting in reduced power generation or failure of the components. Therefore, reducing the fragments in the production of components and the hidden cracks and breakage of cells in the components is a technical problem to be solved in the photovoltaic industry.

[0004] At the same time, in the process of manufacturing photovoltaic modules, in order to reduce the heat loss caused by excessive current in the battery series, the photovoltaic industry has developed half-chip or even multi-chip slicing technology. When making the module, the cell is divided into half or three slices, and then the cell string is made, so that the output current of the cell string and the module is greatly reduced, the Joule heat loss caused by the current is greatly reduced, and the output power of the module is effectively improved. However, the efficiency loss caused by slicing has become a problem that cannot be ignored in the photovoltaic industry. It is mainly due to the damage of the passivation layer of the battery caused by laser or mechanical slicing, or the formation of structural defects such as dislocations in the single crystal silicon and the functional film on the surface, forming carrier recombination centers, causing open circuit voltage, fill factor and conversion efficiency losses. Especially in HJT cells, the efficiency loss of one slice is more than 0.2%, mainly because the high power density of laser slicing causes the crystallization of the amorphous silicon passivation layer, thereby losing the original passivation effect. At the same time, the exposed silicon wafer caused by slicing increases the surface carrier recombination loss. Therefore, passivation treatment of the edge of the cell after slicing is also a technical problem to be studied in photovoltaics.

[0005] On the other hand, with the development of information technology, the demand for flexible photovoltaics is increasing. For example, aerospace, wearable electronics, vehicle-mounted mobile energy, photovoltaic building integration and other fields require high-efficiency, lightweight flexible photovoltaics. Existing flexible photovoltaics mainly use flexible technology routes such as silicon thin film and copper indium gallium selenide. Not only is the conversion efficiency low, but the cost is also much higher than that of conventional single-crystal silicon solar cells. Recently, III-V compound multi-junction flexible thin-film solar cells have been developed using semiconductor ion implantation and stripping technology. Their conversion efficiency has reached more than 30%, the thickness is only tens of microns, and they have good flexibility. However, the material and manufacturing costs are extremely high, and the cost per watt reaches more than 100 yuan, making it difficult to form large-scale applications. Therefore, there is an urgent need to develop low-cost lightweight flexible photovoltaics.

[0006] Based on the above technical problems, a flexible processing technology for single crystal silicon wafers has emerged in the prior art, which solves the problem of single crystal silicon wafers being fragile. Flexible single crystal silicon wafers are processed into flexible single crystal silicon solar cells and lightweight flexible components. The references are as follows:

[0007] Invention patent, application number: CN202211090758.X;

[0008] Invention patent, application number: CN202310175757.3;

[0009] Invention patent, application number: CN202310136324.7.

[0010] However, the above-mentioned prior art still cannot effectively solve the problem of efficiency loss caused by edge damage of single crystal silicon solar cell slices and fragility caused by weak edge mechanics. Summary of the invention

[0011] In view of the problems in the prior art of single crystal silicon solar cell fragmentation, high hidden crack rate, lack of flexibility, edge damage during processing and slicing of the cell, leakage and insufficient reliability, the present invention provides a single crystal silicon solar cell processing method for processing single crystal silicon solar cells, which includes the following steps:

[0012] Step S1, providing a semiconductor processing equipment, stacking a number of single crystal silicon solar cells and sending them into the semiconductor processing equipment;

[0013] Step S2, etching the edge of the single crystal silicon solar cell piece multiple times, so that the edge structure of the single crystal silicon solar cell piece after etching is smooth, without a coating layer and a structural damage layer;

[0014] Step S3, passivating the edge of the single crystal silicon solar cell after etching, and forming a passivation film on the edge of the single crystal silicon solar cell after etching;

[0015] Step S4, taking out the processed single crystal silicon solar cell from the semiconductor processing equipment.

[0016] Furthermore, in the step S2, a dry etching process is used to etch the edges of the stacked monocrystalline silicon solar cells multiple times.

[0017] Further, the step S2 includes:

[0018] Step S2.1, removing the functional films on the front, back and sides of the edge of the single crystal silicon solar cell by dry etching process, wherein the single crystal silicon solar cell after removing the functional films includes a plurality of light trapping microstructures.

[0019] Furthermore, in the step S2.1, the functional film removed includes:

[0020] One or more of a transparent oxide semiconductor (TCO) film of a silicon heterojunction solar cell (HJT), an amorphous silicon film of a silicon heterojunction solar cell (HJT), and a microcrystalline silicon film of a silicon heterojunction solar cell (HJT); or

[0021] One or more of the aluminum oxide film of tunneling oxide passivation contact solar cells (TOPCon), the polysilicon film of tunneling oxide passivation contact solar cells (TOPCon), and the silicon nitride film of tunneling oxide passivation contact solar cells (TOPCon).

[0022] Furthermore, the step S2 further includes:

[0023] Step S2.2: removing the structural damage layer on the front, back and side of the edge of the single crystal silicon solar cell by dry etching process.

[0024] Furthermore, the step S2 further includes:

[0025] Step S2.3: smoothing the light trapping microstructure at the edge of the single crystal silicon solar cell by dry etching process, and removing the mechanically weak areas of the light trapping microstructure at the front, back and side of the edge of the single crystal silicon solar cell.

[0026] Further, in step S2.3:

[0027] The edge width of the rounded area is no greater than 5 mm; and / or

[0028] The light trapping microstructure includes a pyramid structure, and the mechanically weak area includes: a V-shaped depression and a sharp groove at the bottom of the pyramid structure. After the rounding treatment, the curvature radius of the V-shaped depression and the sharp groove at the bottom of the pyramid structure is not less than 50 nanometers.

[0029] Furthermore, in step S3,

[0030] The passivation film is formed by using thin film deposition technology, and the passivation film covers the exposed areas on the front, back and side of the edge of the single crystal silicon solar cell sheet after etching;

[0031] Wherein, the passivation film is a dielectric film containing fixed positive charges or fixed negative charges or free hydrogen atoms.

[0032] Further, in step S3,

[0033] The process gas used in the thin film deposition process includes a mixture of two or more gases selected from Ar, SiH4, NO2, NH3, and H2; and / or

[0034] The passivation film includes one of an amorphous silicon film, a microcrystalline silicon film, a silicon oxide film, a silicon nitride film, and a silicon oxynitride film, or a mixed phase of the above films.

[0035] Furthermore,

[0036] In the step S1, the stacked plurality of monocrystalline silicon solar cell sheets form a monocrystalline silicon solar cell sheet group, in which the position deviation of adjacent monocrystalline silicon solar cell sheets is less than 0.3 mm, and the pressure applied by each monocrystalline silicon solar cell sheet to the adjacent monocrystalline silicon solar cell sheet below it is 2-5 N; and / or

[0037] The monocrystalline silicon solar cell is a silicon heterojunction solar cell (HJT), a tunneling oxide passivation contact solar cell (TOPCon), a back contact solar cell (BC), or a tunneling oxide passivation contact solar cell (PERC).

[0038] The present invention can bring at least one of the following beneficial effects:

[0039] 1. By etching the edge of the monocrystalline silicon solar cell, the coating around the edge of the monocrystalline silicon solar cell is eliminated to avoid leakage caused by the coating around the edge, which is beneficial to improve the conversion efficiency and reliability of the monocrystalline silicon solar cell;

[0040] 2. By etching the edge of the monocrystalline silicon solar cell, the structural defects at the edge of the monocrystalline silicon solar cell are eliminated, especially the structural damage in the passivation layer and the monocrystalline silicon wafer caused by slicing, which is beneficial to improve the conversion efficiency of the solar cell;

[0041] 3. By etching the edge of the monocrystalline silicon solar cell, the mechanical weak areas such as the V-shaped grooves, sharp grooves, and sharp protrusions of the edge pyramid are eliminated, so that the monocrystalline silicon solar cell has flexibility and can be used to prepare foldable flexible photovoltaic modules;

[0042] 4. Through continuous deposition of passivation film, the etched area at the edge of the solar cell is passivated to form a good passivation effect, which is beneficial to improve the conversion efficiency of the solar cell;

[0043] 5. The above passivation film has a covering and protective effect on the edge of the solar cell, which can resist the erosion of water vapor and oxygen, and is beneficial to improving the environmental resistance reliability of solar cells and modules.

[0044] In summary, through the above-mentioned multiple continuous etching and passivation film deposition, edge structural defects and mechanical weak areas are eliminated, and a passivation film is deposited to make the single crystal silicon solar cell flexible, while improving the conversion efficiency and reliability of the solar cell.

[0045] The present invention not only improves the most critical cell conversion efficiency by processing the edges on the basis of the original structure of the single crystal silicon solar cell, and reduces the fragmentation rate of the solar cell during component manufacturing and use, but also improves the flexibility of the single crystal silicon solar cell, making the solar cell have better flexibility, getting rid of the "brittleness" problem, achieving "elasticity" of the solar cell, and providing a high-efficiency flexible photovoltaic solution. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The preferred implementation scheme will be described below in a clear and understandable manner with reference to the accompanying drawings to further illustrate the above-mentioned characteristics, technical features, advantages and their implementation methods.

[0047] Figure 1(a) is an image of the appearance of the edge of a HJT solar cell;

[0048] FIG1( b ) is a schematic diagram of an ultra-thin solar cell sheet bending under its own weight;

[0049] Figure 2(a) is a fluorescent PL image of a HJT solar cell before non-destructive laser slicing;

[0050] Figure 2(b) is a fluorescent PL image of a HJT solar cell after non-destructive laser slicing;

[0051] Figure 2(c) is a SEM image of the cross-sectional microstructure of a HJT solar cell after non-destructive laser slicing;

[0052] Figure 2(d) is a SEM image of the cross-sectional microstructure of a HJT solar cell after conventional laser slicing;

[0053] FIG. 3( a ) is a schematic diagram of a process flow chart of an embodiment of a method for processing a single crystal silicon solar cell according to the present invention;

[0054] FIG3( b ) is a schematic diagram of the steps included in step S2 of the embodiment of the method for processing a single crystal silicon solar cell proposed by the present invention;

[0055] Figure 4 This is a schematic diagram of a plurality of single crystal silicon solar cell sheets stacked together for edge dry etching processing in an embodiment of the single crystal silicon solar cell processing method proposed by the present invention;

[0056] FIG5(a) is a schematic diagram of the microstructure of a HJT solar cell sheet before edge processing in an embodiment of the method for processing a single crystal silicon solar cell proposed by the present invention;

[0057] FIG5( b ) is a SEM photo of the pyramid microstructure of the front and side edges of a HJT solar cell before edge processing in an embodiment of the method for processing a single crystal silicon solar cell proposed by the present invention;

[0058] FIG6( a ) is a schematic diagram of the microstructure of a HJT solar cell after edge etching in an embodiment of the method for processing a single crystal silicon solar cell proposed by the present invention;

[0059] FIG6( b ) is a SEM photo of the front and side microstructures of the edge of a HJT solar cell after edge etching in an embodiment of the method for processing a single crystal silicon solar cell proposed by the present invention;

[0060] Figure 7 This is a schematic diagram of the structure of the HJT solar cell after the edge passivation film is deposited in the embodiment of the single crystal silicon solar cell processing method proposed by the present invention;

[0061] Figure 8(a) is a schematic diagram of the three-point bending test principle;

[0062] FIG8( b ) is a comparison of three-point bending test results before and after edge etching and passivation film deposition in an embodiment of the single crystal silicon solar cell processing method proposed by the present invention;

[0063] FIG9 is a foldable flexible HJT solar cell obtained through edge etching and edge passivation in an embodiment of the single crystal silicon solar cell processing method proposed by the present invention, and the cell thickness is 80 microns;

[0064] Fig.10 A foldable flexible component is prepared from a foldable flexible HJT solar cell sheet obtained according to an embodiment of the single crystal silicon solar cell processing method proposed in the present invention. DETAILED DESCRIPTION

[0065] Various aspects of the present invention are described in further detail below.

[0066] Unless otherwise defined or indicated, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein can be applied to the present invention.

[0067] The following is an explanation of the terms.

[0068] Unless otherwise clearly specified and limited, the "or" mentioned in the present invention includes the relationship of "and". The "and" is equivalent to the Boolean logic operator "AND", the "or" is equivalent to the Boolean logic operator "OR", and "AND" is a subset of "OR".

[0069] It is to be understood that although the terms "first", "second", etc. may be used herein to describe different elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. Therefore, the first element may be referred to as the second element without departing from the teachings of the present invention.

[0070] In the present invention, the terms "comprising", "including" or "comprising" indicate that various components can be applied together in the mixture or composition of the present invention. Therefore, the term "consisting mainly of..." is included in the terms "comprising", "including" or "comprising".

[0071] Unless otherwise clearly specified and limited, the terms "connected", "connected" and "connection" in the present invention should be understood in a broad sense, for example, it can be a fixed connection, or it can be connected through an intermediary medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0072] For example, if an element (or component) is referred to as being on, coupled to, or connected to another element, the element may be directly formed on, coupled to, or connected to the other element, or there may be one or more intervening elements between them. In contrast, if the expressions "directly on," "directly coupled to," and "directly connected to" are used herein, then no intervening elements are indicated. Other words used to describe the relationship between elements should be similarly interpreted, such as "between" and "directly between," "attached" and "directly attached," "adjacent" and "directly adjacent," and the like.

[0073] It should also be noted that the words "front", "rear", "left", "right", "upper" and "lower" used in the following description refer to directions in the drawings. The words "inner" and "outer" used refer to directions toward or away from the geometric center of a particular component, respectively. It can be understood that these terms are used here to describe the relationship of one element, layer or region relative to another element, layer or region as shown in the drawings. In addition to the orientations described in the drawings, these terms should also include other orientations of the device.

[0074] Other aspects of the present invention will be apparent to those skilled in the art in view of the disclosure herein.

[0075] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the specific implementation methods of the present invention will be described below with reference to the accompanying drawings. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings and other implementation methods can be obtained based on these drawings without creative work.

[0076] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show the components related to the present application and are not drawn according to the number, shape and size of the components in actual implementation. The type, quantity and proportion of each component in actual implementation may be changed arbitrarily, and the component layout may also be more complicated. For example, the thickness of the components in the drawings may be exaggerated for the sake of clarity.

[0077] The following description takes HJT solar cells as an example. Those skilled in the art will understand that the following description is only used to explain the purpose of the invention and related feasibility of the present application, and the specific examples given below cannot be used to limit the scope of protection of the present invention.

[0078] In current HJT solar cells, the following are common scenarios that lead to new problems, as well as common solutions in existing technologies:

[0079] At present, at the cell end, the original thickness of mass-produced HJT solar cells is about 110 microns. Due to the advantages of the low-temperature process and the double-sided symmetrical structure during the manufacturing of HJT solar cells, the cells will not produce stress due to the difference between the surface and back functional film layers and electrode materials. In the future, the thickness of single-crystal silicon wafers may be further reduced to 80 microns or even thinner. However, when the thickness of HJT solar cells is reduced to a certain range, the lateral support strength of the cells becomes smaller and can be bent under the condition of deadweight. As shown in Figure 1(b), when the lateral support strength of the silicon wafer becomes smaller, it is difficult to control the clamping and handling strength of the silicon wafer. If the clamping strength is increased, the stress at the bend will be large, resulting in a high fragmentation rate of HJT solar cells.

[0080] In the structural design of all single-crystal silicon solar cell devices, in order to reduce the surface light reflection loss, a pyramid-shaped light-trapping microstructure is usually prepared on the surface of the silicon wafer. This step is called "texturing". The pyramid-shaped light-trapping microstructure can change the transmission path of the once reflected light so that it is absorbed multiple times on the cell surface. Facts have proved that under normal circumstances, the surface reflection loss of single-crystal silicon wafers without pyramid-shaped light-trapping microstructures is greater than 30%. In contrast, the surface reflection loss of single-crystal silicon wafers with pyramid-shaped light-trapping microstructures is less than 10%. However, during the texturing process, since the silicon wafer is completely immersed in the etching solution, a pyramid structure is formed not only on the surface of the silicon wafer, but also on the side of the silicon wafer. Research has found that, as shown in Figure 1(a), the V-shaped valley bottom and sharp depressions of the pyramid-shaped light-trapping microstructure at the edge of the silicon wafer are the mechanical weak areas of the single-crystal silicon wafer, which is equivalent to forming a front "hidden crack" notch at the edge of the silicon wafer. When the silicon wafer is bent, vibrated, or the temperature changes drastically due to external forces, the stress is concentrated at the notch position, causing the silicon wafer to break. Therefore, the V-shaped valley bottom and sharp depressions of the pyramid-shaped light-trapping microstructure on the front, back and side of the edge of the single-crystal silicon wafer are the root causes of silicon wafer breakage.

[0081] Further research found that, as in the schemes in the three reference invention patents cited in the background technology, the edge of the single-crystal silicon wafer is selectively smoothed to remove the V-shaped valley bottom and sharp depressions, spurs and sharp corners of the pyramid-shaped light-trapping microstructure on the front, back and side of the edge, so that the single-crystal silicon wafer has flexibility. The flexible HJT solar cell is prepared using this flexible single-crystal silicon wafer. Even if the thickness of the single-crystal silicon wafer is reduced to 60 microns, the prepared HJT solar cell is not easy to break. However, in the process of making HJT cells, due to the friction and collision between the silicon wafer and mechanical devices such as trays, suction cups, and conveyor belts, new gaps and depressions are easily generated on the edge, which destroys the mechanical properties of the silicon wafer and causes the single-crystal silicon wafer to lose its flexibility.

[0082] In the process of module manufacturing, half-cut slices are generally used to connect the cells in series to reduce the heat loss caused by the current of the cell string and increase the output power of the module. On the one hand, whether conventional laser slicing or lossless laser slicing is used, slicing loss will occur, and the efficiency loss of one slice is about 0.2% or more. This is mainly due to the high power density of laser slicing, which causes the amorphous silicon passivation layer and charge collection layer in the HJT solar cell to crystallize, thereby losing the original passivation effect. At the same time, the exposed silicon slices caused by slicing increase the surface carrier recombination loss. As shown in Figures 2(a) and 2(b), by using lossless laser slicing, comparing the fluorescent PL spectrum before and after cell slicing, it is easy to see that the PL at the cut becomes black, showing a line mark with a width of about 2 mm, indicating that lossless laser slicing causes the passivation function of the passivation layer to be destroyed, causing structural damage. On the other hand, as shown in Figures 2(c) and 2(d), after laser slicing, the microstructure of the end face becomes rough, and new microstructural defects appear, causing the solar cell to lose flexibility and easily break or crack during bending, module manufacturing process and use.

[0083] In order to further improve the conversion efficiency of HJT solar cells, the carrier collection layer of HJT solar cells has been upgraded from amorphous silicon to microcrystalline silicon. However, when preparing surface passivation silicon films, planar plasma enhanced chemical vapor deposition technology (PECVD) is usually used. The film is first deposited on the front of the silicon wafer, then taken out of the coating chamber and turned over to deposit the film on the back. Since the silicon wafers are placed flat on the carrier during flat PECVD coating, there is no mask to block the edge side. Therefore, when a thin film is deposited on the surface of the silicon wafer, it is inevitable that a thin film will be deposited on the side of the silicon wafer, resulting in side wrap-around plating. This wrap-around plating becomes a leakage channel on the front and back, forming a leakage current, which affects the conversion efficiency and reliability of the solar cell.

[0084] In addition, in order to effectively isolate the transparent conductive film TCO on the upper surface from the direct short-circuit connection with the TCO on the lower surface, when physical vapor deposition (PVD) is used to prepare TCO, a hollow carrier with edge shielding is generally used to coat the front and back sides on the same coating machine. This can avoid the complex process of breaking the air and turning over, and can also effectively isolate the upper and lower surfaces. However, similar to PECVD coating, when PVD is used to coat the TCO on the front side, TCO is also deposited on the side of the silicon wafer. In addition, due to the accumulation of multiple factors such as the processing accuracy error of the isolation area of ​​the carrier, the offset of the automated film loading, the warping of the self-weight after thinning, and the vibration offset during the coating transmission process, the edge leakage caused by TCO wrapping during the actual production process accounts for more than 3%. This wrapping phenomenon also affects the conversion efficiency and reliability of solar cells, not only lowering the average indicators of the production line, but also bringing potential reliability and quality risks.

[0085] Improved technical means

[0086] In view of the above problems, referring to FIG. 3( a ), the present invention proposes a HJT solar cell processing method for processing HJT solar cells, which includes the following steps:

[0087] Step S1, providing a semiconductor processing equipment, stacking a number of HJT solar cells and sending them into the semiconductor processing equipment;

[0088] Step S2, etching the edge of the HJT solar cell piece multiple times, so that the edge structure of the etched HJT solar cell piece is smooth, without a circumferential coating and a structural damage layer;

[0089] Step S3, passivating the edge of the etched HJT solar cell sheet, and forming a passivation film on the edge of the etched HJT solar cell sheet;

[0090] Step S4, taking out the processed HJT solar cell from the etching chamber.

[0091] As a preferred embodiment, the plurality of HJT solar cells in step S1 may be one piece. If the number of the plurality of HJT solar cells is greater than 1, the plurality of HJT solar cells are stacked and arranged neatly, such as Figure 4 As shown, a HJT solar cell group is obtained. Based on this, further, in step S1, when the stacked HJT solar cells form a HJT solar cell group, the position deviation of adjacent HJT solar cells in a HJT solar cell group can be made less than 0.3mm, and the pressure applied by each HJT solar cell to the adjacent HJT solar cell below it is 2-5N.

[0092] Based on the above technical solution, further, in step S2, a dry etching process can be used to etch the edges of the stacked HJT solar cells multiple times.

[0093] As a preferred embodiment, the dry etching process can be physical dry etching, chemical dry etching, chemical-physical dry etching, or one or more combinations of plasma etching PE, ion beam etching IBE, reactive ion etching RIE, and inductively coupled plasma etching ICP.

[0094] Those skilled in the art will understand that the above-mentioned etching processes are merely examples and are not intended to limit the scope of protection of the present application. As long as they do not limit the purpose of the invention of the present application, any form of addition, deletion or equivalent modification should be included in the spirit of the present invention.

[0095] Based on the above technical solution, further, as shown in FIG3( b ), step S2 may include:

[0096] Step S2.1: Remove the functional films on the front, back and sides of the edges of the HJT solar cell by dry etching process.

[0097] In the above technical solution, by removing the functional films on the front, back and sides of the edge of the HJT solar cell, the pyramid-shaped light-trapping microstructure formed by "texturing" on the HJT solar cell is exposed. As a preferred embodiment, in the embodiment of processing HJT solar cells, in step S2.1, the functional films removed may include: one or more of the transparent oxide semiconductor (TCO) film of silicon heterojunction solar cells (HJT), the amorphous silicon film of silicon heterojunction solar cells (HJT), and the microcrystalline silicon film of silicon heterojunction solar cells (HJT).

[0098] Those skilled in the art can understand that the above technical solution can also be undoubtedly extended to the processing solutions of other single-crystal silicon solar cells. For example, when the processing object is a TOPCon solar cell, in step S2.1, the functional film to be removed may include: an aluminum oxide film of a tunneling oxide passivation contact solar cell (TOPCon), a polysilicon film of a tunneling oxide passivation contact solar cell (TOPCon), and a silicon nitride film of a tunneling oxide passivation contact solar cell (TOPCon). The above-mentioned removal objects are only examples and are not intended to limit the scope of protection of this application. As long as they do not limit the purpose of the invention of this application, any form of addition, deletion or equivalent transformation should be included in the subject matter of the present invention.

[0099] As a preferred embodiment, taking the removal of TCO film in HJT solar cells as an example, in step S2.1, the neatly stacked HJT solar cells can be sent into the etching chamber, and the TCO film on the front, back and side of the silicon edge of each HJT solar cell in the etching chamber can be removed.

[0100] Preferably, taking ICP etching as an example, the etching process can be carried out using a Cl-containing - The reactive gas for ions can be a mixed gas of Ar, Cl2, and BCl3.

[0101] On this basis, preferably, the total gas flow rate in the etching chamber can be set to 45-55 sccm, preferably, it can be set to 50 sccm;

[0102] The etching pressure can be set to 12-18 mTorr, preferably 15 mTorr;

[0103] The ICP power supply can be set to 300-400W, and preferably 350W;

[0104] The frequency can be set to 12-15MHz, preferably 13.56MHz;

[0105] The bias power can be set to 180-220W, preferably 200W;

[0106] The etching time can be set to at least 90s.

[0107] Further preferably, after the etching process for removing the TCO film is completed, the etching chamber may be purged with nitrogen, and the purging time may be maintained for at least 30 seconds.

[0108] When it is necessary to remove the amorphous silicon and microcrystalline silicon films on the front, back and side edges of HJT solar cells, as a preferred embodiment, the neatly stacked HJT solar cells can be sent into an etching chamber, and the amorphous silicon film and / or microcrystalline silicon film on the front, back and side edges of each HJT solar cell in the etching chamber can be etched to remove the amorphous silicon film and / or microcrystalline silicon film.

[0109] Preferably, still taking ICP etching as an example, the etching process gas may be a reactive gas containing F- ions, and a mixed gas of CF4 and Ar may be selected.

[0110] Further preferably, the total gas flow rate in the etching chamber can be set to 45-55 sccm, preferably, it can be set to 50 sccm;

[0111] The etching pressure can be set to 18-22 mTorr, preferably, it can be set to 20 mTorr;

[0112] The ICP power supply can be set to 90-110W, and preferably 100W;

[0113] The frequency can be set to 12-15MHz, preferably 13.56MHz, and the bias power can be set to 90-110W, preferably 100W;

[0114] The etching time can be set to at least 30s.

[0115] Further preferably, after the etching process for removing the amorphous silicon film and / or the microcrystalline silicon film is completed, the etching chamber may be purged with nitrogen, and the purging time may be maintained for at least 30 seconds.

[0116] Those skilled in the art will understand that the description of the above etching process is only an example, including but not limited to other etching gases and etching parameters, etc. As long as it does not limit the purpose of the invention, any form of addition, deletion or equivalent transformation should be included in the subject matter of the present invention.

[0117] Further, those skilled in the art can understand that the above-mentioned removal process of the TCO film and the removal process of the amorphous silicon film and / or microcrystalline silicon film can be continuous, such as the removal process of the amorphous silicon film and / or microcrystalline silicon film can be performed after the removal process of the TCO film is completed according to the method provided in the present application; as an optional embodiment, the removal process of the TCO film and the removal process of the amorphous silicon film and / or microcrystalline silicon film can also be independent of each other, such as the removal process of the TCO film can be completed only according to the method provided in the present application, or the removal process of the amorphous silicon film and / or microcrystalline silicon film can be completed only according to the method provided in the present application. Therefore, the protection scope of the present application should not be limited by the sequential relationship and / or combination relationship between the above-mentioned film removal processes.

[0118] Based on the above technical solution, further, as shown in FIG3(b), step S2 may further include:

[0119] Step S2.2: Remove the structural damage layer on the front, back and side of the edge of the HJT solar cell through a dry etching process.

[0120] The structural damage layer in the above technical solution may include a structural defect area formed in the edge passivation film of the HJT solar cell sheet and / or the single crystal silicon sheet due to slicing.

[0121] As a preferred embodiment, the HJT solar cell that has completed step S2.1 can be sent into the etching chamber, and each HJT solar cell in the etching chamber is subjected to an etching process to remove the structural damage layer on the front, back and side edges.

[0122] Preferably, still taking ICP etching as an example, the etching process gas can be selected to contain F - The reactive gas for ions can be a mixed gas of CF4 and Ar.

[0123] Further preferably, the total gas flow rate in the etching chamber can be set to 45-55 sccm, preferably, it can be set to 50 sccm;

[0124] The etching pressure can be set to 18-22 mTorr, preferably, it can be set to 20 mTorr;

[0125] The ICP power supply can be set to 90-110W, and preferably 100W;

[0126] The frequency can be set to 12-15MHz, preferably 13.56MHz;

[0127] The bias power can be set to 90-110W, preferably 100W;

[0128] The etching time can be set to at least 30s.

[0129] Further preferably, after the etching process for removing the structural damage layer is completed, the etching chamber may be purged with nitrogen, and the purging time may be maintained for at least 30 seconds.

[0130] It should be understood that the etching step in step S2.2 is only an example, including but not limited to other etching gases and etching parameters, etc. Any form of addition, deletion or equivalent transformation should be included in the subject matter of the present invention as long as it does not limit the purpose of the invention.

[0131] The above technical scheme, through steps S2.1 and S2.2, adopts a dry etching process to first remove the functional film and structural damage layer in the front, back and side areas of the edge of the HJT solar cell, thereby solving the problems of edge leakage and structural damage layer and reducing the discreteness of the gear distribution at the test sorting end.

[0132] Based on the above technical solution, further, as shown in FIG3(b), step S2 may further include:

[0133] Step S2.3, smoothing the light-trapping microstructures at the edges of the HJT solar cell by dry etching, and removing the mechanically weak areas of the light-trapping microstructures at the front, back, and sides of the edges of the HJT solar cell.

[0134] Preferably, in step S2.3, the edge width of the rounded area is no greater than 5 mm.

[0135] Preferably, the light trapping microstructure may include a pyramid structure, on this basis, the mechanically weak area may include: a V-shaped depression and a sharp groove at the bottom of the pyramid structure, and after rounding, the curvature radius of the V-shaped depression and the sharp groove at the bottom of the pyramid structure is not less than 50 nanometers.

[0136] Preferably, after the rounding process in step S2.3, the distance that the light-trapping microstructure extends inward from the edge is less than 2 mm.

[0137] Since the breakage of single-crystal silicon solar cells mainly starts from the edges, cracks will extend inwards until they break. Therefore, by rounding the edges of single-crystal silicon solar cells, stress concentration can be avoided in the mechanically weak areas formed by the pyramid-shaped light-trapping microstructure, which can reduce the risk of breakage in the edge areas of single-crystal silicon solar cells, thereby improving the mechanical strength of single-crystal silicon solar cells.

[0138] As a preferred embodiment, the HJT solar cell sheet that has completed step S2.2 can be sent into the etching chamber, and each HJT solar cell sheet in the etching chamber can be subjected to rounding processing on the front, back and side edges.

[0139] Preferably, still taking ICP etching as an example, the etching process gas can be selected to contain F - The reactive gas for ions can be a mixed gas of CF4 and Ar.

[0140] Preferably, the total gas flow rate in the etching chamber can be set to 45-55 sccm, preferably, it can be set to 50 sccm;

[0141] The etching pressure can be set to 18-22 mTorr, preferably, it can be set to 20 mTorr;

[0142] The ICP power supply can be set to 180-220W, and preferably 200W;

[0143] The frequency can be set to 12-15MHz, preferably 13.56MHz;

[0144] The bias power supply can be set to 130-170W, preferably 150W;

[0145] The etching time can be set to at least 120s.

[0146] Further preferably, after the etching process for smoothing the front, back and side surfaces of the edge is completed, the etching chamber may be purged with nitrogen, and the purging time may be maintained for at least 30 seconds.

[0147] It should be understood that the etching step in step S2.3 is only an example, including but not limited to other etching gases and etching parameters, etc. Any form of addition, deletion or equivalent transformation should be included in the subject matter of the present invention as long as it does not limit the purpose of the invention.

[0148] In the above technical scheme, the schematic diagram of the light-trapping microstructure of the HJT solar cell before the processing in step S2 and the light-trapping microstructure at the edge are shown in Figures 5(a) and 5(b), with an amorphous silicon passivation film and a TCO film at the edge, and thin film plating in some areas of the side. The schematic diagram of the structure after the etching process in step S2 and the light-trapping microstructure at the edge are shown in Figures 6(a) and 6(b), and the silicon film and TCO film at the edge and the damaged layer of the edge structure are removed by the etching process. The V-shaped valley bottom, the valley bottom of the groove, the sharp protrusions, etc. of the pyramid-shaped light-trapping microstructure at the edge are all rounded, and the radius of curvature of the groove is greater than 50nm.

[0149] Based on the above technical solution, further, in step S3,

[0150] Thin film deposition technology can be used to form a passivation film, and the passivation film can cover the exposed areas on the front, back and side of the edge of the HJT solar cell after etching;

[0151] The passivation film is a dielectric film containing fixed positive charges or fixed negative charges or free hydrogen atoms.

[0152] As a preferred embodiment, the passivation film can be formed by physical vapor deposition (PVD) or chemical vapor deposition (CVD). The formed passivation film can include one of an amorphous silicon film, a microcrystalline silicon film, a silicon oxide film, a silicon nitride film, a silicon oxynitride film, or a mixed phase of the above films. Preferably, the thickness of the passivation film can be 50-200 nm.

[0153] As a preferred implementation, the HJT solar cell sheet that has completed step S2 can be sent into a deposition chamber, and a passivation process is performed on the front edge, back edge and side of the silicon substrate of each HJT solar cell sheet.

[0154] Preferably, the passivation process gas can be a mixed gas of two or more gases selected from Ar, SiH4, NO2, NH3, and H2.

[0155] Preferably, the total gas flow rate in the deposition chamber can be set to 180-220 sccm, preferably, it can be set to 200 sccm;

[0156] The etching pressure can be set to 450-550 mTorr, preferably 500 mTorr;

[0157] The ICP power supply can be set to 250-350W, and preferably 300W;

[0158] The frequency can be set to 12-15MHz, preferably 13.56MHz;

[0159] The coating time of the passivation film can be set to at least 120s.

[0160] After the passivation process is completed, the deposition chamber can be purged with nitrogen, and the purging time can be maintained for at least 90 seconds.

[0161] In the above technical solution, step S3 forms a passivation film to passivate the edge of the etched HJT solar cell, thereby solving the problem of efficiency loss of the exposed HJT solar cell after etching and improving the cell conversion efficiency. Figure 7 Schematic diagram showing the microstructure of an HJT cell after edge etching and passivation.

[0162] Based on the above technical solution, step S4 may further include:

[0163] Break through the air to purify the HJT solar cell group and take out several processed HJT solar cell pieces from the semiconductor processing equipment.

[0164] The above technical solution discusses the feasibility of the technical solution of the present application from the processing perspective of HJT solar cells. Those skilled in the art can understand that the above technical solution can undoubtedly be extended to the processing solutions of all single-crystal silicon solar cells, including but not limited to silicon heterojunction solar cells (HJT), tunneling oxide passivated contact solar cells (TOPCon), back contact solar cells (BC), or tunneling oxide passivated contact solar cells (PERC).

[0165] 2000 HJT solar cells were taken for processing test of the invention method. After the edge of the HJT solar cell was processed by the technical solution proposed by the invention, the average conversion efficiency of the HJT solar cell with a thickness of 80 microns reached 24.98%, and the leakage current of the HJT solar cell was reduced from 0.061A to 0.008A, the leakage problem was significantly improved, and the low-efficiency battery caused by edge short circuit was eliminated. The battery conversion efficiency level was reduced from 9 levels to 4 levels (the battery conversion efficiency difference of 0.1% is one level), and the battery conversion efficiency consistency was significantly improved, as shown in the following Table 1:

[0166] index Quantity (pieces) Fragmentation rate (%) Conversion efficiency (%) Limit bending radius (mm) Leakage current(A) Number of gears Original battery cell 2000 3.50 24.89 30.56 0.061 9 This embodiment 2000 0.05 24.98 10.05 0.008 4

[0167] Table 1 Comparison of original HJT solar cells, solar cells processed by the processing method of this embodiment and parameters

[0168] Attached Figures 8(a) and 8(b) show the mechanical characteristic curves of the HJT solar cell obtained by testing the embodiment of the technical solution of the present invention using the three-point bending test method. Compared with the unprocessed cell, the deformation of the HJT solar cell processed in steps S2 and S3 is nearly doubled, the mechanical properties are significantly improved, and good flexibility is given. As shown in Attached Figures 9(a) and 9(b) , the bending of the 80-micron thick HJT solar cell obtained in the embodiment of the technical solution of the present invention can be bent arbitrarily like paper, and the bending limit diameter is close to 15mm.

[0169] The HJT flexible solar cell of the embodiment of the technical solution of the present invention is used to prepare a foldable lightweight flexible component, as shown in the attached Fig.10 As shown, the lightweight flexible components prepared by flexible material packaging have a bending radius of less than 5 cm and a surface density of less than 600 g / cm2. They can be widely used in aerospace, automotive mobile energy, wearable electronics, photovoltaic building integration and other fields.

[0170] The above comparative test is introduced in detail using HJT solar cells as an example. It should be understood that the technical solution of the present invention can also be applied to the processing of other types of single-crystal silicon solar cells, for example, it can be applied to tunneling oxide passivated contact solar cells (TOPCon), back contact solar cells (BC), or tunneling oxide passivated contact solar cells (PERC), etc., to reduce the breakage rate of silicon wafers when the silicon wafers of the cells are thinned, improve the conversion efficiency and flexibility of the cells, give single-crystal silicon solar cells flexibility, and make lightweight and flexible components.

[0171] In summary, the present invention has achieved the following effects:

[0172] The present invention proposes a processing method for monocrystalline silicon solar cells, which comprises the following steps: firstly stacking monocrystalline silicon solar cell sheets, and then removing the coating and structural damage at the edges of the monocrystalline silicon solar cell sheets by etching for multiple times, thereby effectively improving the leakage of the edges of the monocrystalline silicon solar cell sheets; then rounding the edges of the monocrystalline silicon solar cell sheets to disperse external stress, thereby solving the problems of high fragmentation rate and easy occurrence of hidden cracks caused by the cell thinning technology, improving the mechanical properties of the monocrystalline silicon solar cells, making the monocrystalline silicon solar cells flexible, and successfully preparing flexible monocrystalline silicon solar cell sheets; finally, passivating the etched areas at the edges of the monocrystalline silicon solar cell sheets to improve the cell conversion efficiency of the solar cells.

[0173] The present invention not only improves the most critical cell conversion efficiency on the basis of the original single crystal silicon solar cell structure, makes the single crystal silicon solar cell flexible, but also reduces the fragmentation rate of the solar cell. The edge-processed single crystal silicon solar cell has a significantly improved limit bending diameter, making the solar cell have a certain flexibility, getting rid of "brittleness", achieving "plasticization" of the solar cell, improving the mechanical strength of the solar cell, and significantly improving the performance parameters of the single crystal silicon solar cell.

[0174] Based on this application, it should be understood by those skilled in the art that one aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0175] Those skilled in the art know that, in addition to realizing the system and its various devices, modules, and units provided by the present invention in a purely computer-readable program code, it is entirely possible to realize the same functions in the form of logic gates, switches, application-specific integrated circuits, programmable logic controllers, and embedded microcontrollers by logically programming the method steps. Therefore, the system and its various devices, modules, and units provided by the present invention can be considered as a hardware component, and the devices, modules, and units included therein for realizing various functions can also be regarded as structures within the hardware component; the devices, modules, and units for realizing various functions can also be regarded as both software modules for realizing the method and structures within the hardware component.

[0176] It should be noted that the above embodiments can be freely combined as needed. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention.

[0177] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as reference separately. In addition, it should be understood that after reading the above content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A method for processing a single crystal silicon solar cell, for processing a single crystal silicon solar cell, It is characterized in that The following steps are involved: Step S1, providing a semiconductor processing equipment, stacking a number of single crystal silicon solar cells and sending them into the semiconductor processing equipment; Step S2, etching the edge of the single crystal silicon solar cell piece multiple times, so that the edge structure of the single crystal silicon solar cell piece after etching is smooth, without a coating layer and a structural damage layer; Step S3, passivating the edge of the single crystal silicon solar cell after etching, and forming a passivation film on the edge of the single crystal silicon solar cell after etching; Step S4, taking out the processed single crystal silicon solar cell from the semiconductor processing equipment.

2. The method for processing a single crystal silicon solar cell according to claim 1, It is characterized in that In the step S2, the edges of the stacked single crystal silicon solar cell sheets are etched multiple times using a dry etching process.

3. The method for processing a single crystal silicon solar cell according to claim 1, It is characterized in that The step S2 includes: Step S2.1, removing the functional films on the front, back and sides of the edge of the single crystal silicon solar cell by dry etching process, wherein the single crystal silicon solar cell after removing the functional films includes a plurality of light trapping microstructures.

4. The method for processing a single crystal silicon solar cell according to claim 3, It is characterized in that In the step S2.1, the functional film removed includes: One or more of a transparent oxide semiconductor (TCO) film of a silicon heterojunction solar cell (HJT), an amorphous silicon film of a silicon heterojunction solar cell (HJT), and a microcrystalline silicon film of a silicon heterojunction solar cell (HJT); or One or more of the aluminum oxide film of tunneling oxide passivation contact solar cells (TOPCon), the polysilicon film of tunneling oxide passivation contact solar cells (TOPCon), and the silicon nitride film of tunneling oxide passivation contact solar cells (TOPCon).

5. The method for processing a single crystal silicon solar cell according to claim 3, It is characterized in that The step S2 also includes: Step S2.2: removing the structural damage layer on the front, back and side of the edge of the single crystal silicon solar cell by dry etching process.

6. The method for processing a single crystal silicon solar cell according to claim 3 or 5, It is characterized in that The step S2 also includes: Step S2.3: smoothing the light trapping microstructure at the edge of the single crystal silicon solar cell by dry etching process, and removing the mechanically weak areas of the light trapping microstructure at the front, back and side of the edge of the single crystal silicon solar cell.

7. The method for processing a single crystal silicon solar cell according to claim 6, It is characterized in that In step S2.3: The edge width of the rounded area is no greater than 5 mm; and / or The light trapping microstructure includes a pyramid structure, and the mechanically weak area includes: a V-shaped depression and a sharp groove at the bottom of the pyramid structure. After the rounding treatment, the curvature radius of the V-shaped depression and the sharp groove at the bottom of the pyramid structure is not less than 50 nanometers.

8. The method for processing a single crystal silicon solar cell according to claim 1, It is characterized in that In the step S3, The passivation film is formed by using thin film deposition technology, and the passivation film covers the exposed areas on the front, back and side of the edge of the single crystal silicon solar cell sheet after etching; Wherein, the passivation film is a dielectric film containing fixed positive charges or fixed negative charges or free hydrogen atoms.

9. The method for processing a single crystal silicon solar cell according to claim 8, It is characterized in that In step S3, The process gases used in the thin film deposition process include Ar, SiH 4 、NO 2 NH 3 , H 2 A mixture of two or more gases; and / or The passivation film includes one of an amorphous silicon film, a microcrystalline silicon film, a silicon oxide film, a silicon nitride film, and a silicon oxynitride film, or a mixed phase of the above films.

10. The method for processing a single crystal silicon solar cell according to any one of claims 1 to 9, It is characterized in that In the step S1, the stacked plurality of monocrystalline silicon solar cell sheets form a monocrystalline silicon solar cell sheet group, in which the position deviation of adjacent monocrystalline silicon solar cell sheets is less than 0.3 mm, and the pressure applied by each monocrystalline silicon solar cell sheet to the adjacent monocrystalline silicon solar cell sheet below it is 2-5 N; and / or The monocrystalline silicon solar cell is a silicon heterojunction solar cell (HJT), a tunneling oxide passivation contact solar cell (TOPCon), a back contact solar cell (BC), or a tunneling oxide passivation contact solar cell (PERC).