Design and manufacturing method of negative electrode for high-specific-energy lithium metal battery

By forming an artificial SEI layer of polyethylene oxide and polyhedral silsesquioxane copolymer on the negative electrode surface of the lithium metal battery, the safety hazards and performance degradation caused by the reaction of lithium dendrites and electrolytes are solved, and the electrical power of lithium metal batteries is improved. Chemical properties and cycle life.

CN119050264APending Publication Date: 2024-11-29ZHEJIANG FUNLITHIUM NEW ENERGY TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411178354.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The uneven deposit of solid lithium metal negative electrode during the charging and discharging of the battery leads to the formation of lithium dendrites, causing safety hazards and degradation of battery performance, and strong reaction with the electrolyte, reducing cycle stability and service life.

Method used

Polyethylene oxide (PEO) segments and polyhedral silsesquioxane (POSS) copolymers are used to form an artificial stable interface layer (SEI). A uniform SEI layer is formed on the surface of metal lithium through free radical polymerization, which inhibits the growth of lithium dendrites. And improve lithium ion conduction performance.

Benefits of technology

The uniform deposition and stability of lithium metal batteries are achieved, the Coulomb efficiency and cycle life of the battery are improved, the safety is enhanced, and the dense SEI layer is formed to reduce side reactions and interface impedance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050264A_ABST
    Figure CN119050264A_ABST
Patent Text Reader

Abstract

The invention discloses a design and manufacturing method of a negative electrode for a high-specific-energy lithium metal battery, and the manufacturing method of the negative electrode for the high-specific-energy lithium metal battery comprises the following steps: S1, in an inert gas, adding a polyoxyethylene (PEO) chain segment, polyhedral oligomeric silsesquioxane (POSS) and an initiator into an organic solvent, heating and stirring until the materials are completely dissolved, so as to obtain a mixed solution; initiating free radical polymerization reaction through an initiator to form a first solution containing a PEO-POSS copolymer; s2, after the first solution is cooled to the room temperature, adding a binder into the first solution, and uniformly stirring at the room temperature to obtain a second solution; and S3, uniformly coating the surface of the metal lithium with the second solution, and obtaining the negative electrode with the artificial SEI layer for the high-specific-energy lithium metal battery after the organic solvent is completely volatilized, the method has the advantages that the cycle performance and coulombic efficiency of the solid-state lithium metal battery can be improved, and the safety is relatively good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium metal batteries, and in particular relates to a negative electrode design and manufacturing method for a high specific energy lithium metal battery. Background Art

[0002] With the increasing depletion of fossil energy and its serious impact on the environment, the development and application of new energy technologies have become an important issue in modern society. Solid-state lithium metal battery technology, as a leader in the field of new energy, has demonstrated its wide application potential in many fields. However, the energy density of existing lithium-ion batteries is relatively low. This limitation has, to a certain extent, restricted its application and development in high-performance energy storage devices. In order to overcome this technical bottleneck, scientific researchers are committed to developing electrode materials with higher energy density. The research on these materials can not only significantly improve the performance of batteries and meet the market demand for high-energy storage devices, but also is expected to promote technological progress and industrial upgrading of the entire new energy industry.

[0003] Among the many studies on negative electrode materials, metallic lithium has become the most popular candidate material due to its excellent specific capacity (up to 3860 mAh / g) and low reduction potential (-3.04 V relative to standard hydrogen electrode). This feature makes it an ideal negative electrode material for high-energy-density secondary batteries. However, solid-state lithium metal anodes still face some challenges in practical applications: (1) During the battery charging and discharging process, the deposition of metallic lithium on the current collector is often not uniform, which may lead to the formation of lithium dendrites. Lithium dendrites not only pierce the battery separator and cause internal short circuits, but may also cause battery overheating or even explosion, posing serious safety hazards; (2) The reactivity between metallic lithium and the electrolyte is strong, which not only continuously consumes the electrolyte, but also may form irreversible lithium deposition on the electrode surface. This deposition will lead to the pulverization of the electrode material and the formation of so-called "dead lithium", thereby reducing the overall cycle stability and service life of the battery. These challenges limit the widespread application of solid-state lithium metal anodes in high-energy-density secondary batteries and urgently need to be overcome through technological innovation.

[0004] In order to solve the limitations of solid lithium metal anode in secondary battery applications, a common method is to promote the formation of a stable solid electrolyte interface (SEI) film by introducing additives into the electrolyte. For example, the H.Ota team (J.Electrochem.Soc., 2004, 151, A1778-A1788) published that by adding vinylene carbonate (VC) to the electrolyte, a stable interface layer was successfully formed on the surface of metallic lithium, thereby improving the deposition characteristics of lithium. The Cui team proposed a method for growing nano hollow carbon spheres on the surface of solid lithium metal anode in (Nature Nanotechnology, 2004, 9, 618-623) to inhibit the growth of lithium dendrites. Although this method shows potential in improving battery performance, its cost is relatively high. In terms of patent literature, CN2015100051525 proposed an in-situ protection treatment method to form a layer of silicon dioxide protective layer on the surface of metallic lithium. Although the preparation process is simple, the stability of the protective layer still needs to be improved. The US4359818A patent uses a pre-prepared thin film passivation layer and presses it on the metal lithium, but this method has the problem that the passivation layer is easy to separate and difficult to prepare. 2 The composite of poly(2-vinylpyridine) and poly(2-vinylpyridine) is used as a passivation layer to form a LiI protective layer, but the interface formed by this method is not stable enough and may introduce impurities, reducing the ionic conductivity of the interface. The CN2017102021773 patent adopts the strategy of organic-inorganic dual protective layer to form Li 3 N.Li x NO y A protective layer is formed to prevent uneven deposition of lithium ions and physically isolate the contact between metallic lithium and the electrolyte. Although this method improves battery performance to a certain extent, the introduction of impurities and easily soluble and detached small molecular organic matter limits its long-term application effect.

[0005] Therefore, in order to truly realize the large-scale production of solid-state lithium metal batteries, it is increasingly important to develop a solid-state lithium metal battery negative electrode that can not only uniformly deposit lithium to inhibit the formation of lithium dendrites, but also prevent the continuous reaction of lithium metal with the electrolyte. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a negative electrode design and manufacturing method for a high specific energy lithium metal battery, which helps to improve the cycle performance and coulombic efficiency of solid-state lithium metal batteries and has good safety.

[0007] The technical solution adopted by the present invention to solve the above technical problems is:

[0008] One of the purposes of the present invention is to provide a method for manufacturing a negative electrode for a high specific energy lithium metal battery, comprising the following steps:

[0009] S1, in an inert gas, adding a polyethylene oxide (PEO) segment, polyhedral silsesquioxane (POSS), and an initiator to an organic solvent, heating and stirring until completely dissolved, and initiating a free radical polymerization reaction by the initiator to form a first solution containing a PEO-POSS copolymer;

[0010] S2, after the first solution is cooled to room temperature, adding a binder to the first solution and stirring at room temperature to obtain a second solution;

[0011] S3. Uniformly coating the second solution on the surface of the metallic lithium, and after the organic solvent is completely volatilized, a negative electrode for a high-energy-density lithium metal battery having an artificial SEI layer is obtained.

[0012] Preferably, in step S1, the molecular weight of the polyethylene oxide (PEO) segment is 200-20000.

[0013] Preferably, in step S1, POSS is one or a mixture of at least two of POSS-octaacrylate, POSS-octavinyl and a structure containing a carbon-carbon double bond at the end of the POSS side chain; the initiator is one or a mixture of at least two of azobisisobutyronitrile (AIBN), azobisisobutyramidine hydrochloride (AIBA), and azobisisobutylimidazoline hydrochloride (AIBI); and the organic solvent is one or a mixture of at least two of tetrahydrofuran, ethanol, chloroform and acetonitrile.

[0014] Preferably, in step S1, the reaction molar ratio of polyethylene oxide (PEO) segment to polyhedral silsesquioxane (POSS) is 8:1.

[0015] Preferably, in step S1, the heating temperature is 65-85°C and the heating time is 10-12h.

[0016] Preferably, in step S2, the binder is one of polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA), polyvinylidene fluoride (PVDF), and carboxymethyl cellulose (CMC), or a mixture of at least two of them.

[0017] Preferably, in step S3, the thickness of the artificial SEI layer is 1-5 μm.

[0018] Preferably, in step S3, the artificial SEI layer contains 1-10% by mass of an adhesive.

[0019] One of the purposes of the present invention is to provide a negative electrode for a high-energy-density lithium metal battery, which is prepared by the above-mentioned method for manufacturing a negative electrode for a high-energy-density lithium metal battery.

[0020] Compared with the prior art, the advantages of the present invention are:

[0021] 1. Through the free radical reaction between PEO chain segments and POSS, an organic-inorganic composite artificial SEI material (PEO-POSS) is formed, which can exist stably in the electrolyte;

[0022] 2. The PEO segment in the artificial SEI material (PEO-POSS) is an organic part and a flexible polymer that can form a uniform artificial SEI layer on the surface of lithium metal, adapting to the volume change of lithium metal during the charge and discharge process, thereby avoiding the fall-off of the binder. At the same time, PEO has a high lithium ion conductivity, especially after being compounded with lithium salts, it can achieve good ion conductivity at room temperature. Moreover, PEO can form a relatively stable interface with lithium metal, reduce the occurrence of side reactions and reduce interface impedance. In addition, PEO is easy to process into a thin film, which is convenient for forming a uniform artificial SEI layer on the surface of lithium metal;

[0023] 3. POSS in the artificial SEI material (PEO-POSS) is an inorganic part. The hydrophobic cavity inside POSS has a binding effect on the charge, which can effectively improve the ionic conductivity and concentration polarization phenomenon, effectively prevent the migration of anions in the electrolyte, increase the migration number of lithium ions, and contribute to the uniform deposition of lithium. The stable SEI film formed by uniform deposition helps to alleviate the corrosion of the electrolyte to the lithium metal negative electrode, thereby inhibiting the growth of lithium dendrites;

[0024] 4. The negative electrode for high specific energy lithium metal battery of the present invention has high coulombic efficiency and can stably optimize the solid electrolyte protective layer (SEI). The formed SEI layer can be evenly and densely stabilized on the surface of lithium metal and has relatively small impedance, thereby improving the safety of solid-state lithium metal battery, and further improving the electrochemical performance and cycle life of solid-state lithium metal battery;

[0025] 5. Polyhedral silsesquioxane (POSS) can reduce the crystallinity of polyethylene oxide (PEO) chain segments, which helps to improve its conductivity;

[0026] 6. The POSS-based PEO segments contained in the present invention have certain limitations in terms of molding, such as low viscosity and poor plasticity, and usually need to be modified to improve their processing properties. Therefore, the present invention adopts a solution method, and tetrahydrofuran, ethanol, chloroform and acetonitrile are selected as organic solvents, which have good mutual solubility with the PEO segments and the POSS-based, and thus facilitate the modification and film-forming of PEO-POSS, and the preparation method is simple and feasible.

[0027] 7. The artificial SEI material (PEO-POSS) has a uniform and dense modified layer and can be tightly combined with lithium metal. It can be applied to different battery systems and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The cycle performance of the solid-state lithium metal battery composed of Example 2 and Comparative Example 3;

[0029] Figure 2 The battery rate curves of the lithium metal batteries composed of Example 2 and Comparative Example 3;

[0030] Figure 3 The lithium metal battery composed of Example 2 and Comparative Example 3 is 3 mA / cm 2 Scanning electron microscopy image of lithium metal deposition after 30 cycles at the current density;

[0031] Figure 4 The lithium metal battery composed of Example 2 and Comparative Example 3 is 3 mA / cm 2 Scanning electron microscopy cross-sectional image of lithium metal deposition after 30 cycles at the same current density. DETAILED DESCRIPTION

[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.

[0033] Example

[0034] A method for manufacturing a negative electrode for a high specific energy lithium metal battery comprises the following steps:

[0035] S1. In an inert gas, a polyethylene oxide (PEO) segment, polyhedral silsesquioxane (POSS), and an initiator are added to an organic solvent, heated and stirred at a heating temperature of 65-85° C. for a heating time of 10-12 h until completely dissolved, and a free radical polymerization reaction is initiated by the initiator to form a first solution containing a PEO-POSS copolymer, wherein the reaction molar ratio of the polyethylene oxide (PEO) segment to the polyhedral silsesquioxane (POSS) is 8:1;

[0036] S2, after the first solution is cooled to room temperature, adding a binder to the first solution and stirring at room temperature to obtain a second solution;

[0037] S3. Uniformly coating the second solution on the surface of the metallic lithium, and after the organic solvent is completely volatilized, a negative electrode for a high-energy-density lithium metal battery having an artificial SEI layer is obtained.

[0038] In step S1, the molecular weight of the polyethylene oxide (PEO) segment is 200-20000, preferably 2000; POSS is one or a mixture of at least two of POSS-octaacrylate, POSS-octavinyl and a structure containing a carbon-carbon double bond at the end of the POSS branch chain; the initiator is one or a mixture of at least two of azobisisobutyronitrile (AIBN), azobisisobutyramidine hydrochloride (AIBA), and azobisisobutylimidazoline hydrochloride (AIBI); the organic solvent is one or a mixture of at least two of tetrahydrofuran, ethanol, chloroform and acetonitrile.

[0039] In step S2, the binder is one of polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA), polyvinylidene fluoride (PVDF), and carboxymethyl cellulose (CMC), or a mixture of at least two of them.

[0040] In step S3, the thickness of the artificial SEI layer is 1-5 μm, and the artificial SEI layer contains 1-10% by mass of an adhesive.

[0041] Embodiment 1,

[0042] A method for manufacturing a negative electrode for a high specific energy lithium metal battery comprises the following steps:

[0043] S1, in an inert gas, a polyethylene oxide (PEO) segment with a molecular weight of 200, POSS-octaacrylate, and azobisisobutyronitrile (AIBN) are added to a tetrahydrofuran (THF) organic solvent, heated and stirred at a heating temperature of 70° C. for a heating time of 12 h until completely dissolved, and a free radical polymerization reaction is initiated by an initiator to form a first solution containing 1 g of a PEO-POSS copolymer;

[0044] S2. After the first solution is cooled to room temperature, 5% by mass of polyvinyl butyral (PVB) is added to the first solution and stirred evenly at room temperature to obtain a second solution;

[0045] S3. The second solution is uniformly coated on the surface of the metallic lithium by spraying, and then dried in a vacuum oven at room temperature to remove the organic solvent, so as to obtain a negative electrode for a high specific energy lithium metal battery having an artificial SEI layer, wherein the thickness of the artificial SEI layer is 2.5 μm.

[0046] Embodiment 2,

[0047] The rest is the same as Example 1, except that the molecular weight of the polyethylene oxide (PEO) segment is 2000.

[0048] Embodiment 3,

[0049] The rest is the same as Example 1, except that the molecular weight of the polyethylene oxide (PEO) segment is 5,000.

[0050] Embodiment 4,

[0051] The rest is the same as Example 1, except that the molecular weight of the polyethylene oxide (PEO) segment is 10,000.

[0052] Embodiment 5,

[0053] The rest is the same as Example 1, except that the molecular weight of the polyethylene oxide (PEO) segment is 20,000.

[0054] Embodiment 6,

[0055] The rest is the same as in Example 1, except that the POSS is POSS-octavinyl.

[0056] Comparative Example 1

[0057] Conventional metallic lithium anode without artificial SEI layer.

[0058] Comparative Example 2

[0059] Dissolve 1g of PEO in 15ml of tetrahydrofuran, stir evenly to make it completely dissolved, then add 5% by mass of PVB to form a uniform solution, and then use a spraying method to form a film on the surface of metallic lithium, and then dry it at room temperature in a vacuum oven to remove the tetrahydrofuran, to obtain a lithium metal negative electrode with an artificial SEI layer.

[0060] Among them, the molecular weight of PEO is 200.

[0061] Comparative Example 3

[0062] The rest is the same as Comparative Example 2, except that the molecular weight of PEO is 2,000.

[0063] Comparative Example 4

[0064] The rest is the same as Comparative Example 2, except that the molecular weight of PEO is 5,000.

[0065] Comparative Example 5

[0066] The rest is the same as Comparative Example 2, except that the molecular weight of PEO is 10,000.

[0067] Comparative Example 6

[0068] The rest is the same as Comparative Example 2, except that the molecular weight of PEO is 20,000.

[0069] Comparative Example 7

[0070] 1 g of POSS-octaacrylate was dissolved in 15 ml of tetrahydrofuran, stirred evenly to make it completely dissolved, and then 5% by mass of PVB was added to form a uniform solution. A film was formed on the surface of metallic lithium by spraying, and then dried at room temperature in a vacuum oven to remove the tetrahydrofuran, thereby obtaining a lithium metal negative electrode with an artificial SEI layer.

[0071] Comparative Example 8

[0072] The rest is the same as Comparative Example 7, except that the POSS is POSS-octavinyl.

[0073] The high specific energy lithium metal battery negative electrode prepared in Examples 1-6 and the lithium metal negative electrode prepared in Comparative Examples 1-8 were respectively assembled into solid-state lithium metal batteries. The positive electrode of the solid-state lithium metal battery was LiCoO 2 The electrolyte is LiPF 6 / EC:DMC(1:1), all solid-state lithium metal batteries were subjected to charge and discharge cycle tests, the test environment was 25°C, the voltage test range was 3.0V~4.35V, the charge rate was 1.0C, the discharge rate was 1.0C, and the capacity retention rate and coulombic efficiency were recorded after 400 cycles, as shown in the following table:

[0074]

[0075] As can be seen from the table, the capacity retention rate and coulombic efficiency of the solid-state lithium metal batteries composed of Examples 1-6 are significantly higher than those of the solid-state lithium metal batteries composed of Comparative Examples 1-8. Among them, the capacity retention rate and coulombic efficiency of the solid-state lithium metal battery with an artificial SEI layer in Example 2 are the highest among all the examples, that is, when the molecular weight of the PEO segment is 2000, the effect of the artificial SEI layer is better. Figure 1 , Example 2 can still maintain a high coulombic efficiency of 99.6% after 400 charge and discharge cycles, and the capacity retention rate is 94.8%, while Comparative Example 3 can only maintain a coulombic efficiency of 98.6% after 400 charge and discharge cycles, and the capacity retention rate is only 58%.

[0076] By comparing Examples 1-6 and Comparative Examples 1-8, it can be concluded that coating PEO-POSS on the surface of the solid-state lithium metal negative electrode can limit the cyclic volume fluctuation of the lithium negative electrode, make the SEI layer more stable and strong, and make the lithium deposition more uniform. It can effectively inhibit the generation of lithium dendrites, help to uniformly transport lithium ions, improve the electrochemical performance of the solid-state lithium metal battery, and also improve the safety performance and cycle performance.

[0077] The lithium metal negative electrode prepared in Example 2 and the lithium metal negative electrode prepared in Comparative Example 3 are respectively used to form a lithium metal battery. The lithium metal battery uses LiTFSI / DOL:DME (1:1) as the electrolyte and contains an initiator LiPF 6 (lithium hexafluorophosphate) electrolyte is injected into the interior of the lithium metal battery to ensure that the electrolyte is in full contact with the lithium metal negative electrode, and then the lithium metal battery is heated to 70°C and thermally cured in an inert atmosphere (such as argon or nitrogen).

[0078] The lithium metal batteries composed of Example 2 and Comparative Example 3 were subjected to charge and discharge cycle tests, and the test current density was 3 mA / cm 2 , and 30 cycles of charge and discharge are performed. The battery rate curve is as follows Figure 2 As shown, a corresponds to the lithium metal battery composed of Example 3, and b corresponds to the lithium metal battery composed of Example 2. Figure 2 The gray area in the figure is from 1mA / cm 2 Increase to 3mA / cm 2 When 3mA / cm 2 During the cycle, the lithium metal battery composed of Comparative Example 3 showed voltage fluctuations, and it can be seen that the overpotential of the battery is very high, which indicates that the Li + The reversibility of ion insertion and extraction and the cycle stability are poor, which also indicates that the lithium-lithium metal battery composed of comparative example 3 may have serious dendrite growth, while the overpotential of the lithium-lithium metal battery composed of example 2 remains stable and is similar to the initial overpotential, indicating that the battery has good Li + Ion deintercalation reversibility and cycling stability.

[0079] Figure 3 For lithium metal batteries at 3 mA / cm 2 Scanning electron microscope lithium metal deposition image after 30 cycles at current density, a corresponds to the lithium metal battery composed of Example 3, b corresponds to the lithium metal battery composed of Example 2. The observation results show that Figure 3 In a, many large dendritic lithiums appeared on the surface of the lithium metal negative electrode, and large cracks appeared on the surface, the surface was uneven, and a large amount of dead lithium was produced. These dead lithiums would cause electrical isolation, resulting in excessive overpotential of the solid-state lithium metal battery, decreased coulombic efficiency, and seriously affected the cycle life of the battery. Figure 3 In b, the surface of the lithium metal negative electrode is relatively smooth, which will make the solid-state lithium metal battery have excellent cycle performance.

[0080] Figure 4 For lithium metal batteries at 3 mA / cm 2Scanning electron microscope cross-sectional view of lithium metal deposition after 30 cycles at current density, a corresponds to the lithium-lithium metal battery composed of Example 3, b corresponds to the lithium-lithium metal battery composed of Example 2. The observation results show that Figure 4 In a, the cross section of the lithium metal anode is relatively rough, and part of the surface SEI layer breaks and peels off, while in Figure 4 In b, the cross section of the lithium metal negative electrode is relatively smooth and flat, indicating that the use of the artificial SEI layer of Example 2 can effectively inhibit the growth of lithium dendrites and make lithium ions deposit more evenly.

[0081] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the implementation of the present invention is not limited to the above-mentioned method. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A method for manufacturing a negative electrode for a high specific energy lithium metal battery, characterized in that: The following steps are involved: S1. In an inert gas, a polyethylene oxide (PEO) chain segment, polyhedral silsesquioxane (POSS), and an initiator are added to an organic solvent, heated and stirred until completely dissolved, and a free radical polymerization reaction is initiated by the initiator to form a first solution containing a PEO-POSS copolymer; S2, after the first solution is cooled to room temperature, adding a binder to the first solution and stirring evenly at room temperature to obtain a second solution; S3. Uniformly coating the second solution on the surface of the lithium metal, and after the organic solvent is completely volatilized, a negative electrode for a high-energy-density lithium metal battery with an artificial SEI layer is obtained.

2. The method for manufacturing a negative electrode for a high specific energy lithium metal battery according to claim 1, characterized in that: In the step S1, the molecular weight of the polyethylene oxide (PEO) segment is 200-20000.

3. The method for manufacturing a negative electrode for a high specific energy lithium metal battery according to claim 1, characterized in that: In the step S1, the POSS is one or a mixture of at least two of POSS-octaacrylate, POSS-octavinyl and a structure containing a carbon-carbon double bond at the end of a POSS side chain; The initiator is one of azobisisobutyronitrile (AIBN), azobisisobutyramidine hydrochloride (AIBA), and azobisisobutylimidazoline hydrochloride (AIBI), or a mixture of at least two thereof; The organic solvent is one of tetrahydrofuran, ethanol, chloroform and acetonitrile, or a mixture of at least two of them.

4. The method for manufacturing a negative electrode for a high specific energy lithium metal battery according to claim 1, characterized in that: In the step S1, the reaction molar ratio of the polyethylene oxide (PEO) segment to the polyhedral silsesquioxane (POSS) is 8:

1.

5. The method for manufacturing a negative electrode for a high specific energy lithium metal battery according to claim 1, characterized in that: In the step S1, the heating temperature is 65-85°C and the heating time is 10-12h.

6. The method for manufacturing a negative electrode for a high specific energy lithium metal battery according to claim 1, characterized in that: In the step S2, the binder is one of polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA), polyvinylidene fluoride (PVDF), and carboxymethyl cellulose (CMC), or a mixture of at least two of them.

7. The method for manufacturing a negative electrode for a high specific energy lithium metal battery according to claim 1, characterized in that: In step S3, the thickness of the artificial SEI layer is 1-5 μm.

8. The method for manufacturing a negative electrode for a high specific energy lithium metal battery according to claim 1, characterized in that: In step S3, the artificial SEI layer contains 1-10% by mass of an adhesive.

9. A negative electrode for a high specific energy lithium metal battery, characterized in that: The negative electrode is prepared by the method for manufacturing a negative electrode for a high-energy-density lithium metal battery according to any one of claims 1 to 8.

Citation Information

Cited By

  • Low-moisture solid electrolyte material and preparation method and application thereof

    CN119965329A

  • Lithium metal negative electrode containing multifunctional polymer brush protective layer, preparation method of lithium metal negative electrode and lithium metal battery

    CN122494584A

  • A lithium metal negative electrode containing a multifunctional polymer brush protective layer and a preparation method therefor, and a lithium metal battery

    CN122494584B