Electrolyte for improving high-temperature cycle performance of battery and preparation method
By using trimethylsilylamine modified 1,3-dioxolane compounds in lithium-ion battery electrolyte, forming high-quality SEI films and capturing HF, the electrolyte of lithium-ion batteries is solved in the high-temperature cycle. The problems of stability and side reactions have significantly improved the battery's high-temperature cycling performance.
Patent Information
- Application Number
- CN202411159200.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
During the high-temperature cycle of lithium-ion batteries, the electrolyte is unstable, producing HF and PF5, destroying the positive electrode material and SEI film, resulting in side reactions and increased internal resistance of the battery, and the SEI film on the negative electrode surface repeatedly breaks and repairs the electrolyte consumes. Impact battery performance.
Trimethylsilylamine modified 1,3-dioxolane compounds were used as characteristic additives in the electrolyte to form a high-quality SEI film, and HF in the electrolyte was captured to stabilize the positive electrode material and reduce side reactions.
It effectively improves the high-temperature cycling performance of lithium-ion batteries, reduces side reactions, and extends battery life, especially under high temperature conditions, which show significant performance improvements.
Smart Images

Figure SMS_1 
Figure FDA0005005954030000011
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrolytes, and in particular to an electrolyte for improving high temperature cycle performance of a battery and a preparation method thereof. Background Art
[0002] Lithium-ion batteries generally encounter the following problems during high-temperature cycling: (1) The electrolyte is unstable at high temperatures for a long time, and LiPF6 tends to decompose, producing HF and PF5, which will damage the positive electrode material and SEI film and trigger side reactions, thereby consuming the electrolyte; (2) At high temperatures, the dissolution of transition metals in the positive electrode is intensified, and they deposit on the surface of the negative electrode, triggering side reactions, consuming the electrolyte, and increasing the internal resistance of the battery; (3) During long-term cycling, the SEI film on the surface of the negative electrode undergoes a repeated "damage-repair" process, consuming the electrolyte, thickening the SEI film, and increasing the internal resistance of the battery.
[0003] In response to the above problems, the optimization strategy for the electrolyte is usually to increase the dosage of negative electrode film-forming additives and add acid and water removal agents. However, increasing the dosage of film-forming additives will cause the internal resistance of the battery to increase, and the acid and water removal additives will have a certain impact on the battery performance. Summary of the invention
[0004] The present invention aims to provide an electrolyte and a preparation method for improving the high temperature cycle performance of a battery, so as to solve the above problems.
[0005] To achieve the above object, the present invention provides a trimethylsilylamine-modified 1,3-dioxolane compound, the structure of the trimethylsilylamine-modified 1,3-dioxolane compound is:
[0006]
[0007] Here, n is a natural integer ranging from 2 to 8.
[0008] Trimethylsilylamine-modified 1,3-dioxolane compounds are not only good negative electrode film-forming additives and can form high-quality SEI films on the surface of silicon-based negative electrodes, but also have the function of capturing HF in the electrolyte and stabilizing the positive electrode material. Therefore, applying them to the electrolyte can effectively improve the high-temperature cycle performance of lithium-ion batteries.
[0009] The present invention provides an application of a 1,3-dioxolane compound modified by trimethylsilylamine, and the application of the 1,3-dioxolane compound modified by trimethylsilylamine in a lithium battery electrolyte.
[0010] The invention provides a lithium battery electrolyte, which comprises: a 1,3-dioxolane compound modified by trimethylsilylamine.
[0011] The invention provides a lithium battery electrolyte, which comprises the following components: 11-15% by mass of a lithium salt, 70-80% by mass of an organic solvent, 3-10% by mass of a trimethylsilylamine-modified 1,3-dioxolane compound, 5-10% by mass of fluoroethylene carbonate, and 0.5-3% by mass of vinylene carbonate.
[0012] The organic solvent includes at least one of the following: ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, 1,4-butyrolactone, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, 1,3-epoxypentane, tetrahydrofuran, acetonitrile, adiponitrile, succinonitrile, glutaronitrile, dimethyl sulfone, cyclopentane sulfone, trimethyl phosphate. Of course, any solvent that meets the dielectric constant and viscosity is acceptable.
[0013] The lithium salt includes at least one of the following: lithium hexafluorophosphate, lithium hexafluoroarsenic, lithium perchlorate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluoro(oxalatoborate), lithium trifluoromethanesulfonate, lithium pentafluoroethylsulfonate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide. Of course, any lithium salt may be used as long as it meets the solubility and lithium ion migration number requirements.
[0014] The present invention provides a method for preparing a lithium battery electrolyte, the method comprising:
[0015] Lithium salt, trimethylsilylamine-modified 1,3-dioxolane compound, fluoroethylene carbonate and vinylene carbonate are sequentially added into an organic solvent, and after stirring and dissolving, an electrolyte for improving high-temperature cycle performance of a battery is obtained.
[0016] The present invention introduces a 1,3-dioxolane compound modified with trimethylsilylamine as a characteristic additive into the electrolyte. The additive is not only a good negative electrode film-forming additive and can form a high-quality SEI film on the surface of the silicon-based negative electrode, but also has the functions of capturing HF in the electrolyte and stabilizing the positive electrode material, thereby reducing the side reactions of the battery during high-temperature cycling and effectively improving the high-temperature cycling performance of the lithium-ion battery.
[0017] The present invention provides a lithium battery, comprising: a positive electrode, a negative electrode and the above-mentioned electrolyte.
[0018] The material of the positive electrode includes at least one of the following: lithium cobalt oxide, lithium manganese oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium iron phosphate, and spinel nickel-manganese oxide.
[0019] The material of the negative electrode includes at least one of the following: graphite, coke, mesophase carbon microbeads, silicon-based compounds, and metallic lithium.
[0020] Technical effects and advantages of the present invention:
[0021] The present invention introduces a 1,3-dioxolane compound modified with trimethylsilylamine as a characteristic additive into the electrolyte. The additive is not only a good negative electrode film-forming additive and can form a high-quality SEI film on the surface of the silicon-based negative electrode, but also has the functions of capturing HF in the electrolyte and stabilizing the positive electrode material, thereby reducing the side reactions of the battery during high-temperature cycling and effectively improving the high-temperature cycling performance of the lithium-ion battery.
[0022] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The terms such as "upper", "lower", "left", "right", "middle" and "one" quoted in the specification are only for the convenience of description, and are not used to limit the scope of the implementation of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the implementation of the present invention without substantial changes in the technical content.
[0024] Example 1
[0025] In an inert atmosphere glove box with water content and oxygen content less than 5ppm, organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are prepared into an organic solvent in a mass ratio of 3:7, lithium hexafluorophosphate is slowly added to the prepared organic solvent until it dissolves, and then 1,3-dioxolane compounds modified by trimethylsilylamine and vinylene carbonate are added and stirred to completely dissolve to obtain a lithium-ion battery electrolyte. Among them, the mass fractions of lithium hexafluorophosphate, organic solvent, 1,3-dioxolane compounds modified by trimethylsilylamine, fluoroethylene carbonate, and vinylene carbonate are 13%, 76%, 5%, 5%, and 1%, respectively.
[0026] The graphite negative electrode and LiNi 0.6 Co 0.2 Mn 0.2O2 (NCM622) positive electrode was paired and assembled according to N / P=1.1 to obtain a 10Ah soft pack battery. The battery adopts constant current-constant potential charge / constant current discharge (CC-CV / CC) mode, with charge and discharge cut-off voltages of 4.20V and 2.5V respectively, and constant potential cut-off current of 0.05C. Each cycle of charge and discharge was left to stand for 30 minutes. The battery was cycled at 25℃ and 45℃ at a charge and discharge rate of 0.5 / 1C. The data is shown in Table 1.
[0027] Example 2
[0028] In an inert atmosphere glove box with water and oxygen contents below 5ppm, organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were prepared into an organic solvent in a mass ratio of 3:7, lithium hexafluorophosphate was slowly added to the prepared organic solvent until it dissolved, and then trimethylsilylamine-modified 1,3-dioxolane compounds and vinylene carbonate were added and stirred to completely dissolve to obtain a lithium-ion battery electrolyte. Among them, the mass fractions of lithium hexafluorophosphate, organic solvent, trimethylsilylamine-modified 1,3-dioxolane compounds, fluoroethylene carbonate, and vinylene carbonate were 13%, 71%, 5%, 10%, and 1%, respectively.
[0029] The graphite negative electrode and LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) positive electrode was paired and assembled according to N / P=1.1 to obtain a 10Ah soft pack battery. The battery adopts constant current-constant potential charge / constant current discharge (CC-CV / CC) mode, with charge and discharge cut-off voltages of 4.20V and 2.5V respectively, and constant potential cut-off current of 0.05C. Each cycle of charge and discharge was left to stand for 30 minutes. The battery was cycled at 25℃ and 45℃ at a charge and discharge rate of 0.5 / 1C. The data is shown in Table 1.
[0030] Example 3
[0031] In an inert atmosphere glove box with water content and oxygen content less than 5ppm, organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are prepared into an organic solvent in a mass ratio of 3:7, lithium hexafluorophosphate is slowly added to the prepared organic solvent until it dissolves, and then 1,3-dioxolane compounds modified by trimethylsilylamine and vinylene carbonate are added and stirred to completely dissolve to obtain a lithium-ion battery electrolyte. Among them, the mass fractions of lithium hexafluorophosphate, organic solvent, 1,3-dioxolane compounds modified by trimethylsilylamine, fluoroethylene carbonate, and vinylene carbonate are 11%, 80%, 3%, 5.5%, and 0.5%, respectively.
[0032] The graphite negative electrode and LiNi 0.6 Co0.2 Mn 0.2 O2 (NCM622) positive electrode was paired and assembled according to N / P=1.1 to obtain a 10Ah soft pack battery. The battery adopts constant current-constant potential charge / constant current discharge (CC-CV / CC) mode, with charge and discharge cut-off voltages of 4.20V and 2.5V respectively, and constant potential cut-off current of 0.05C. Each cycle of charge and discharge was left to stand for 30 minutes. The battery was cycled at 25℃ and 45℃ at a charge and discharge rate of 0.5 / 1C. The data is shown in Table 1.
[0033] Example 4
[0034] In an inert atmosphere glove box with water and oxygen contents below 5ppm, organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were prepared into an organic solvent in a mass ratio of 3:7, lithium hexafluorophosphate was slowly added to the prepared organic solvent until it dissolved, and then trimethylsilylamine-modified 1,3-dioxolane compounds and vinylene carbonate were added and stirred to completely dissolve to obtain a lithium-ion battery electrolyte. Among them, the mass fractions of lithium hexafluorophosphate, organic solvent, trimethylsilylamine-modified 1,3-dioxolane compounds, fluoroethylene carbonate, and vinylene carbonate were 13%, 70%, 10%, 5%, and 2%, respectively.
[0035] The graphite negative electrode and LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) positive electrode was paired and assembled according to N / P=1.1 to obtain a 10Ah soft pack battery. The battery adopts constant current-constant potential charge / constant current discharge (CC-CV / CC) mode, with charge and discharge cut-off voltages of 4.20V and 2.5V respectively, and constant potential cut-off current of 0.05C. Each cycle of charge and discharge was left to stand for 30 minutes. The battery was cycled at 25℃ and 45℃ at a charge and discharge rate of 0.5 / 1C. The data is shown in Table 1.
[0036] Example 5
[0037] In an inert atmosphere glove box with water and oxygen contents below 5ppm, organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were prepared into an organic solvent in a mass ratio of 3:7, lithium hexafluorophosphate was slowly added to the prepared organic solvent until it dissolved, and then 1,3-dioxolane compounds modified with trimethylsilylamine and vinylene carbonate were added and stirred to completely dissolve to obtain a lithium-ion battery electrolyte. Among them, the mass fractions of lithium hexafluorophosphate, organic solvent, 1,3-dioxolane compounds modified with trimethylsilylamine, fluoroethylene carbonate, and vinylene carbonate were 15%, 74%, 3%, 5%, and 3%, respectively.
[0038] The graphite negative electrode and LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) positive electrode was paired and assembled according to N / P=1.1 to obtain a 10Ah soft pack battery. The battery adopts constant current-constant potential charge / constant current discharge (CC-CV / CC) mode, with charge and discharge cut-off voltages of 4.20V and 2.5V respectively, and constant potential cut-off current of 0.05C. Each cycle of charge and discharge was left to stand for 30 minutes. The battery was cycled at 25℃ and 45℃ at a charge and discharge rate of 0.5 / 1C. The data is shown in Table 1.
[0039] Comparative Example 1
[0040] In an inert atmosphere glove box with water content and oxygen content below 5ppm, organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were prepared into an organic solvent in a mass ratio of 3:7, lithium hexafluorophosphate was slowly added to the prepared organic solvent until it dissolved, and then vinylene carbonate was added and stirred to completely dissolve it to obtain a lithium-ion battery electrolyte. The mass fractions of lithium hexafluorophosphate, organic solvent, fluoroethylene carbonate, and vinylene carbonate were 13%, 81%, 5%, and 1%, respectively.
[0041] The graphite negative electrode and LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) positive electrode was paired and assembled according to N / P=1.1 to obtain a 10Ah soft pack battery. The battery adopts constant current-constant potential charge / constant current discharge (CC-CV / CC) mode, with charge and discharge cut-off voltages of 4.20V and 2.5V respectively, and constant potential cut-off current of 0.05C. Each cycle of charge and discharge was left to stand for 30 minutes. The battery was cycled at 25℃ and 45℃ at a charge and discharge rate of 0.5 / 1C. The data is shown in Table 1.
[0042] Comparative Example 2
[0043] In an inert atmosphere glove box with water content and oxygen content less than 5ppm, organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were prepared into an organic solvent in a mass ratio of 3:7, lithium hexafluorophosphate was slowly added to the prepared organic solvent until it dissolved, and then vinylene carbonate was added and stirred to completely dissolve it to obtain a lithium-ion battery electrolyte. The mass fractions of lithium hexafluorophosphate, organic solvent, fluoroethylene carbonate, and vinylene carbonate were 13%, 76%, 10%, and 1%, respectively.
[0044] The graphite negative electrode and LiNi 0.6 Co 0.2 Mn 0.2O2 (NCM622) positive electrode was paired and assembled according to N / P=1.1 to obtain a 10Ah soft pack battery. The battery adopts constant current-constant potential charge / constant current discharge (CC-CV / CC) mode, with charge and discharge cut-off voltages of 4.20V and 2.5V respectively, and constant potential cut-off current of 0.05C. Each cycle of charge and discharge was left to stand for 30 minutes. The battery was cycled at 25℃ and 45℃ at a charge and discharge rate of 0.5 / 1C. The data is shown in Table 1.
[0045] Table 1. Cycle data of batteries of Examples 1-5 and Comparative Examples 1-2
[0046] 25℃ cycle life@80% 45℃ cycle life @80% Example 1 2120 1890 Example 2 2215 2105 Example 3 2125 1655 Example 4 2250 1785 Example 5 2180 1965 Comparative Example 1 2055 1205 Comparative Example 2 2130 1385
[0047] From the cycle data of the batteries of Examples 1-5 and Comparative Examples 1-2, it can be observed that the electrolyte disclosed in the present invention for improving the high temperature cycle performance of batteries has no obvious improvement in room temperature cycling for NCM622 / C system lithium-ion batteries, but can improve the high temperature cycle performance by up to 700 weeks (56.8%).
[0048] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A 1,3-dioxolane compound modified with trimethylsilylamine, It is characterized in that The structure of the trimethylsilylamine-modified 1,3-dioxolane compound is: Here, n is a natural integer ranging from 2 to 8.
2. The use of the trimethylsilylamine-modified 1,3-dioxolane compound according to claim 1, It is characterized in that Application of the trimethylsilylamine-modified 1,3-dioxolane compound in lithium battery electrolyte.
3. A lithium battery electrolyte, It is characterized in that The electrolyte includes: a 1,3-dioxolane compound modified by trimethylsilylamine.
4. The lithium battery electrolyte according to claim 3, Features The electrolyte comprises the following components: 11-15% by mass of lithium salt, 70-80% by mass of organic solvent, 3-10% by mass of 1,3-dioxolane compound modified by trimethylsilylamine, 5-10% by mass of fluoroethylene carbonate, and 0.5-3% by mass of vinylene carbonate.
5. The lithium battery electrolyte according to claim 4, Features ,, the organic solvent includes at least one of the following: ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, 1,4-butyrolactone, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, 1,3-epoxypentane, tetrahydrofuran, acetonitrile, adiponitrile, succinonitrile, glutaronitrile, dimethyl sulfone, cyclopentane, trimethyl phosphate.
6. The lithium battery electrolyte according to claim 5, It is characterized in that The lithium salt includes at least one of the following: lithium hexafluorophosphate, lithium hexafluoroarsenic, lithium perchlorate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium trifluoromethanesulfonate, lithium pentafluoroethylsulfonate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, and lithium bis(fluorosulfonyl)imide.
7. A method for preparing a lithium battery electrolyte according to any one of claims 4 to 6, It is characterized in that The method comprises: Lithium salt, trimethylsilylamine-modified 1,3-dioxolane compound, fluoroethylene carbonate and vinylene carbonate are sequentially added into an organic solvent, and after stirring and dissolving, an electrolyte for improving high-temperature cycle performance of a battery is obtained.
8. A lithium battery, It is characterized in that The lithium battery comprises: a positive electrode, a negative electrode and an electrolyte as claimed in any one of claims 3 to 6.
9. The lithium battery according to claim 8, It is characterized in that The material of the positive electrode includes at least one of the following: lithium cobalt oxide, lithium manganese oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium iron phosphate, and spinel nickel-manganese oxide.
10. The lithium battery according to claim 8, It is characterized in that The material of the negative electrode includes at least one of the following: graphite, coke, mesophase carbon microbeads, silicon-based compounds, and metallic lithium.
Citation Information
Patent Citations
Electrolyte and secondary battery
CN107732299A
Lithium ion battery electrolyte and lithium ion battery
CN109524714A
Lithium ion battery electrolyte for high-voltage system
CN111211353A
High-voltage electrolyte for lithium battery
CN114156526A
Lithium battery
JP1998189007A