Method for preparing foam wave-absorbing material by using coal water slurry gasification slag as single raw material

By screening and reselecting, the coarse particles and fine particles in the water coal slurry gasification slag are separated, the fine particle carbon is ground and fixed in the coarse particle slag, and the thermal expansion of the water coal slurry gasification slag is solved by calculating in an inert atmosphere. The problem of underutilizing the bubble and residual carbon absorbing properties has achieved low density and excellent absorbing properties of coal gasified slag-based foam absorbing materials, which reduces costs and improves the processing performance of the materials.

CN119053140APending Publication Date: 2024-11-29CHINA UNIV OF MINING & TECH (BEIJING)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310610879.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art fails to fully utilize the thermal expansion foaming and residual carbon absorption properties of water-coal slurry gasification slag, resulting in insufficient utilization of high-value gasification slag and the introduction of magnetic particles to increase costs.

Method used

By sieving and reselecting, fine-grained carbon is separated, fine-grained carbon is ground and fixed in the bonding wall or pore of the coarse-grained residue, magnetic ferrite is prepared by calculating in an inert atmosphere to achieve the material Improved lightweight, moldability and wave absorption performance.

Benefits of technology

The low density, excellent wave absorption performance and synergistic effect of a single coal gasified slag-based foam absorbing material are achieved, which reduces costs and improves the processing performance and application prospects of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053140A_ABST
    Figure CN119053140A_ABST
Patent Text Reader

Abstract

The invention discloses a water-coal-slurry gasification slag-based foam wave-absorbing material which is prepared by doping fine-particle residual carbon obtained by reselection and grinding into coarse-particle slag according to a certain mass ratio and firing in an inert atmosphere. The preparation method comprises the following steps: drying and screening the coal water slurry gasification coarse slag to obtain coarse particle slag and fine particle slag, reselecting and grinding the fine particle slag to obtain fine particle residual carbon, filling the fine particle residual carbon into the coarse particle slag, paving in a mold, roasting in an inert atmosphere at 900-950 DEG C for 15-30 minutes, and cooling to obtain the foam wave-absorbing material. Coarse-particle slag with thermal expansion foaming characteristics is screened and enriched, fine-particle residual carbon with excellent wave absorbing performance is separated from the fine-particle slag through reselection, and finally, the residual carbon is fixed in foaming particle bonding walls or pore channels by roasting a mixture of the coarse-particle slag and the fine-particle residual carbon. The volume density is as low as 0.36 g / cm < 3 >, the compressive strength is as high as 1.82 MPa, and the cutting processability is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid waste utilization and the technical field of foam absorbing material preparation, and relates to a method for preparing a foam absorbing material by taking water-coal slurry gasification slag as a single raw material. Background Art

[0002] The water-coal slurry fluidized-bed gasification process is one of the mainstream coal gasification processes at present. Coal chemical bases widely distributed in Shandong, Shaanxi, Inner Mongolia, Ningxia and Xinjiang produce a huge amount of gasification slag every year. The difficulty and high cost of solid waste disposal have become a problem that plagues enterprises. Stockpiling and landfilling are the main means of disposing of gasification slag at present, but they will cause serious environmental risks and waste of land resources. Therefore, the development of adaptive utilization technology based on the composition and structural characteristics of gasification slag is the key to achieving its reduction and resource utilization. Studies have found that the high content of aluminosilicate glass phase and iron-calcium fluxing elements in water-coal slurry gasification slag, as well as the large amount of gas dissolved in the glass phase, make it expand and foam due to heat, which becomes the unique property of water-coal slurry gasification coarse slag. In addition, the residual carbon content in water-coal slurry gasification coarse slag is relatively high, and its distribution has obvious particle size effect, showing the characteristics of small particle size and high content, and the carbon ash particles are independently distributed and easy to separate. The residual carbon in the gasification slag has a high degree of graphitization and a rough and porous structure. It is an electromagnetic wave absorption material dominated by dielectric loss. In summary, the crude slag from coal-water slurry gasification has both the characteristics of thermal expansion and foaming for lightweighting and the excellent absorbing performance of residual carbon. Through thermal processing to stimulate the synergistic effect of the two components of ash and carbon, foam absorbing materials are prepared, which becomes a new method for high-value utilization of coal gasification slag. At present, the technical application of foamed ceramsite, foamed ceramsite, thermal insulation materials, lightweight concrete and other foamed materials using solid wastes such as coal gasification slag, fly ash, coal gangue, waste glass, iron tailings, ceramic powder and other solid wastes as main raw materials has been very extensive. Among them, the preparation method of composite foam absorbing materials loaded with graphite, carbon fiber and other absorbers has also appeared, but the preparation of foam absorbing materials using coal gasification slag as a single raw material has not been reported.

[0003] Chinese patent application CN114181663A discloses a method for extracting high-purity carbon from coal gasification slag by a two-step acid leaching process. The prepared high-purity carbon has significant electromagnetic wave absorption performance. The RL of electromagnetic waves min Reached -44.1dB (5.19GHz), the corresponding matching thickness is 4.7mm; Chinese patent application CN111817020B discloses a method for preparing porous ceramic composite absorbing materials by chemical impregnation-in-situ carbon thermal reduction of loaded magnetic alloy using coal gasification furnace slag purified by two-step acid leaching as raw material, wherein the roasting temperature is 700-1000℃, the time is 1-3h, and the RL of electromagnetic waves minReach -32dB (4.4GHz), the corresponding coating thickness is 5.5mm; Chinese patent application CN112533467A discloses a magnetic composite absorbing material loaded with Fe / FeC or single Fe, which is prepared by mixing red mud and coal gasification residue in a certain proportion and then calcining in an inert atmosphere. The absorbing material has excellent RL of electromagnetic waves. min Reach -48dB (8.5GHz), the corresponding coating thickness is 2.5mm; Chinese patent application CN111817021A discloses a method for preparing a composite microwave absorbing material by chemical impregnation-in-situ carbon thermal reduction loading Fe2O3, Fe3O4, Fe or Fe3C using coal gasification furnace slag with high specific surface area modified by two-step acid leaching as raw material, wherein the roasting temperature is 300-900℃, the time is 2-3h, and the RL of the electromagnetic wave min Reaching -25dB (8.5GHz), the corresponding coating thickness is 2mm, and the effective bandwidth is 4.5GHz; Chinese patent application CN114436671A discloses a method for preparing a foam ceramic-based interference-type absorbing material by using ceramic powder and carbon fiber film as raw materials through blank making and sintering, wherein the sintering temperature is 710-750°C, the time is 20-30min, and the average reflectivity of the material to electromagnetic waves in the 8-18GHz frequency band is as low as -11.2--10.1dB.

[0004] Some of the above methods utilize the in-situ reduction characteristics of residual carbon in coal gasification slag, some develop the absorbing properties of residual carbon, and some utilize the specific surface area and pore structure of coal gasification slag to load magnetic particles to enhance the absorbing performance. However, these methods do not fully utilize the foaming and bonding molding characteristics of water-coal slurry gasification slag during thermal processing, which is very helpful for the lightweight, formability and absorbing performance improvement of solid waste-based absorbing materials. Summary of the invention

[0005] The present invention is based on the characteristics of high-temperature thermal expansion and foaming, thermomagnetic conversion of coarse slag from water-coal slurry gasification, and the wave absorption performance of residual carbon. The in-situ preparation of magnetic ferrite and the loading of residual carbon are completed by roasting in an inert atmosphere, thereby achieving the lightweight, formability, and coordinated absorption of electromagnetic waves by magnetic and dielectric losses of the material. In the preparation process, the coarse-grained slag with thermal expansion and foaming characteristics is enriched by screening, and then the fine-grained residual carbon with excellent wave absorption performance is separated from the fine-grained slag by gravity selection, and the fine-grained carbon is further ground to increase the specific surface area and enhance the wave absorption performance. At the same time, it can also weaken the hindering effect of the residual carbon particle size on the bonding between mineral foaming particles. Finally, the ground fine-grained residual carbon is fixed in the bonding wall or pore generated by the thermal expansion and foaming of the coarse-grained slag by roasting, and a single coal gasification slag-based molded foam wave absorbing material is obtained. In addition, the honeycomb multi-level pore structure of the foam material improves impedance matching, increases the effective distance of electromagnetic waves propagating inside the material, and enhances the effect on electromagnetic wave loss. In order to achieve the purpose of the above invention, the present invention provides the following technical solutions:

[0006] (1) Drying and screening the crude slag from water-coal slurry gasification to obtain coarse slag particles (1 to 3 mm) and fine slag particles (0.25 to 1 mm);

[0007] (2) The fine-grained slag obtained in step (1) is re-selected with heavy liquids of different densities to separate fine-grained carbon residues, and the fine-grained carbon residues stained with the heavy liquid are washed with water, dried, and then ground to obtain carbon residues with a particle size of less than 0.05 mm;

[0008] (3) adding the residual carbon after grinding in step (2) to the coarse granular slag obtained in step (1) at a certain mass ratio, and spreading the mixture in a firing mold;

[0009] (4) The mold containing the material in step (3) is heated to 900-950° C. in an inert atmosphere, calcined for 15-30 min, and then cooled to obtain a foamed absorbing material.

[0010] Preferably, the coarse slag is water-coal slurry gasification coarse slag, the loss on ignition is greater than 12%, and the content of SiO2+Al2O3+Fe2O3+CaO is not less than 85wt%.

[0011] Preferably, the density of the heavy liquid is 1.70 g / L to 1.90 g / L, and it is prepared from zinc bromide powder.

[0012] Preferably, the fine particles of carbon residue separated by gravity separation have a loss on ignition of more than 80wt%, a particle size after grinding of less than 0.05mm, and a wave absorption performance of: RL of electromagnetic wave minThe RL of the electromagnetic wave is -29.4dB (5.6GHz), the corresponding matching thickness is 4.5mm, and the effective bandwidth is 3.5GHz. Preferably, the amount of fine carbon residue added is 0% to 2%, and the absorbing performance of the foam absorbing material with an addition amount of 0% is: min Reaching -22.5dB (16.8GHz), the corresponding matching thickness is 7mm and the effective bandwidth is 2GHz.

[0013] Preferably, the inert gas is N2 and the heating device is a horizontal atmosphere tube furnace.

[0014] Compared with the prior art, the present invention has the following advantages:

[0015] A single solid waste coal gasification coarse slag is used as the production raw material, and the coarse slag and fine carbon residue are separated by simple screening and re-selection, and the difference in the particle size of the components is fully utilized to fix the ground carbon residue in the bonding wall or pore generated by the thermal expansion and foaming of the coarse slag to complete the composite of the two components. At the same time, the in-situ preparation of magnetic ferrite is completed during the roasting process, which solves the problem that the foam absorbing material needs to introduce magnetic particles to increase the cost, and the honeycomb multi-level pore structure of the foam material can improve impedance matching and enhance the effect on electromagnetic wave loss. The present invention realizes the lightweight, formability and coordination of magnetic and dielectric loss absorption of electromagnetic waves, taking into account solid waste disposal and material preparation. A single coal gasification slag-based foam absorbing material with low density, certain strength and excellent wave absorbing performance can be prepared by simple physical sorting (screening, re-selection) and roasting method, and the material has excellent cutting and processing performance, and can be processed into plates of different specifications according to the matching thickness of electromagnetic waves and other requirements, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is the preparation flow chart of the present invention, Figures 2 to 5 This is a physical picture of the foam absorbing material prepared in Examples 1 to 4 of the present invention. Figure 6 The XRD diagrams of gasified slag raw materials and foam absorbing materials are shown in Figure 2. Figure 7 is the reflection loss value of the foam material when the fine particle residual carbon addition amount is 0%, Figure 8 It is the reflection loss value of fine particle carbon residue. DETAILED DESCRIPTION

[0017] The embodiments are only used to illustrate the present invention and are not intended to limit the present invention. In the present invention, the coal gasification slag is preferably a coarse coal-water slurry gasification slag, with a loss on ignition of >12%, wherein the content of SiO2+Al2O3+Fe2O3+CaO is not less than 85wt%. In an embodiment of the present invention, the loss on ignition of the coal gasification slag is 16.9%, and the chemical composition preferably includes: SiO2 40.01%, Al2O3 12.84%, Fe2O3 19.99%, CaO 15.90%, K2O 1.34%, MgO 2.26%, Na2O 4.21%, TiO2 1.01% and other substances. The contents of heavy metals in gasification slag are Cr (516.8 mg / kg), Cu (62.1 mg / kg), Zn (13.8 mg / kg), Cd (0.06 mg / kg), and Pb (10.1 mg / kg), respectively, all of which are lower than the control values ​​specified in the "Soil Environmental Quality Agricultural Land Soil Pollution Risk Control Standard (Trial)" (GB 15618-2018); and the heavy metal leaching toxicity leaching contents are Cr (0.01 mg / L), Cu (0.08 mg / L), Zn (0.52 mg / L), Cd (not detected), and Pb (0.12 mg / L), respectively, all of which are lower than the emission limits specified in the "Coal Industry Pollutant Emission Standard" (GB 20426-2006). In addition, the electromagnetic parameters of the material are tested by using E5071C vector network analyzer and coaxial line method in the 1-18 GHz frequency range; the compressive strength and volume density of the material are tested in accordance with "Cellular Glass Insulation Products (JC / T 647-2005)". The present invention is described in detail below in conjunction with the accompanying drawings.

[0018] Embodiment 1:

[0019] (1) Screening: 3000 g of four-nozzle water-coal slurry gasification slag from Ningdong Coal Chemical Industry Base in Ningxia was placed in a forced air drying oven and dried at 105°C for 2 h. The dried slag was dry-screened using a vibrating screen to obtain coarse granular slag (1-3 mm) and fine granular slag (0.25-1 mm) for later use.

[0020] (2) Ingredients: 10 g of coarse granular slag, spread flat in a firing mold.

[0021] (3) Firing: The firing mold containing the material is placed in a horizontal atmosphere tube furnace, heated to 950°C at a heating rate of 8°C / min, and fired at a constant temperature for 30 minutes, and then cooled in the furnace to obtain a foam absorbing material, such as Figure 2 As shown. The volume density of this material is 0.36g / cm 3 , compressive strength is 1.82Mpa, wave absorption performance is: RL of electromagnetic wave minReaching -22.5dB (16.8GHz), the corresponding matching thickness is 7mm and the effective bandwidth is 2GHz.

[0022] Embodiment 2:

[0023] (1) Screening: 3000 g of four-nozzle water-coal slurry gasification slag from Ningdong Coal Chemical Industry Base in Ningxia was placed in a forced air drying oven and dried at 105°C for 2 h. The dried slag was dry-screened using a vibrating screen to obtain coarse granular slag (1-3 mm) and fine granular slag (0.25-1 mm) for later use.

[0024] (2) Gravity separation: Dissolve zinc bromide powder in water to prepare a heavy liquid with a density of 1.70 g / L. Pour about 200 g of fine slag into a beaker containing the heavy liquid, stir for 30 seconds and let stand for 10 minutes, then separate the light and heavy components, wash the light component with water several times to remove the zinc bromide heavy liquid on the particle surface and dry it. Grind the dried fine carbon residue to obtain carbon residue with a particle size of <0.05 mm. (3) Batching: 15 g of coarse slag and 0.3 g of ground carbon residue, mix and spread them flat in a firing mold.

[0025] (4) Firing: The firing mold containing the material is placed in a horizontal atmosphere tube furnace, heated to 950°C at a heating rate of 10°C / min, and fired at a constant temperature for 30 minutes, and then cooled in the furnace to obtain a foam absorbing material, such as Figure 3 As shown. The volume density of this material is 0.40g / cm 3 , the compressive strength is 1.56Mpa.

[0026] Embodiment 3:

[0027] (1) Screening: The coarse-grained slag and fine-grained slag obtained by screening in Example 1 were used.

[0028] (2) Gravity separation: Dissolve zinc bromide powder in water to prepare a heavy liquid with a density of 1.80 g / L. Pour about 200 g of fine slag into a beaker containing the heavy liquid, stir for 30 seconds and let stand for 10 minutes, then separate the light and heavy components, wash the light component with water several times to remove the zinc bromide heavy liquid on the particle surface and dry it, grind the dried fine granular carbon residue to obtain carbon residue with a particle size of <0.05 mm. (3) Ingredients: 10 g of coarse granular slag, 0.1 g of ground carbon residue, mix well and spread it flat in a firing mold.

[0029] (4) Firing: The firing mold containing the material is placed in a horizontal atmosphere tube furnace, heated to 930°C at a heating rate of 10°C / min, and fired at a constant temperature for 20 minutes, and then cooled in the furnace to obtain a foam absorbing material, such as Figure 4 As shown. The volume density of this material is 0.39g / cm 3, the compressive strength is 1.67Mpa.

[0030] Embodiment 4:

[0031] (1) Screening: The coarse-grained slag and fine-grained slag obtained by screening in Example 1 were used.

[0032] (2) Gravity separation: Dissolve zinc bromide powder in water to prepare a heavy liquid with a density of 1.90 g / L. Pour about 200 g of fine slag into a beaker containing the heavy liquid, stir for 30 seconds and let stand for 10 minutes, then separate the light and heavy components, wash the light component with water several times to remove the zinc bromide heavy liquid on the particle surface and dry it, grind the dried fine carbon residue to obtain carbon residue with a particle size of <0.05 mm. (3) Ingredients: 10 g of coarse slag, 0.05 g of ground carbon residue, mix well and spread them flat in a firing mold.

[0033] (4) Firing: The firing mold containing the material is placed in a horizontal atmosphere tube furnace, heated to 950°C at a heating rate of 15°C / min, and fired at a constant temperature for 15 minutes, and then cooled in the furnace to obtain a foam absorbing material, such as Figure 5 As shown. The volume density of this material is 0.39g / cm 3 , the compressive strength is 1.78Mpa.

[0034] As described above, the embodiments of the present invention are described in detail, but it is obvious to those skilled in the art that many variations are possible without departing from the inventive point and effect of the present invention. Therefore, all such variations are also included in the protection scope of the present invention.

Claims

1. A method for preparing a foamed wave absorbing material using coal-water slurry gasification slag as a single raw material, characterized in that: The coarse slag ore obtained by screening and the fine carbon residue obtained by gravity separation and grinding are mixed in a certain mass ratio and then fired at 900-950° C. for 15-30 minutes in an inert atmosphere to obtain a molded foam absorbing material, which specifically includes the following steps: (1) Drying and screening the crude slag from coal-water slurry gasification to obtain coarse slag particles (1 to 3 mm) and fine slag particles (0.25 to 1 mm); (2) the fine-grained slag obtained in step (1) is subjected to gravity separation using heavy liquid to separate fine-grained carbon residue, and the fine-grained carbon residue after washing and drying is further ground; (3) adding the fine-grained carbon residue obtained after grinding in step (2) to the coarse-grained slag obtained in step (1) at a certain mass ratio and then flattening the mixture in a mold; (4) The mold containing the material in step (3) is heated to 900-950° C. in an inert atmosphere, calcined for 15-30 min, and then cooled to obtain a foamed absorbing material.

2. The method according to claim 1, characterized in that The coarse slag is coarse slag from gasification of water-coal slurry, with a loss on ignition greater than 12% and a content of SiO2+Al2O3+Fe2O3+CaO not less than 85wt%.

3. The method according to claim 1, characterized in that The heavy liquid has a density of 1.70 g / L to 1.90 g / L and is prepared from widely used raw materials such as zinc bromide and sodium polytungstate.

4. The method according to claim 1, characterized in that: The fine particles of residual carbon separated by gravity separation have a ignition loss of >80wt%, a particle size after grinding of <0.05mm, and a wave absorption performance of: RL of electromagnetic wave min It reaches -29.4dB (5.6GHz), the corresponding matching thickness is 4.5mm, and the effective bandwidth is 3.5GHz.

5. The method according to claim 1, characterized in that The amount of fine carbon residue added is 0% to 2%. The absorbing performance of the foam absorbing material with an addition amount of 0% is: RL of electromagnetic wave min Reaching -22.5dB (16.8GHz), the corresponding matching thickness is 7mm and the effective bandwidth is 2GHz.

6. The method according to claim 1, characterized in that The inert gas includes but is not limited to N2, Ar2, etc., and the heating device includes but is not limited to a horizontal atmosphere tube furnace, etc.