Three-dimensional porous hollow nanofiber aerogel as well as preparation method and application thereof
The preparation of three-dimensional porous hollow nanofiber aerogel by coaxial dry spinning wet joint electrospinning method has solved the problem of insufficient mechanical properties of bone defect repair materials and difficult to regulate pore structure, and achieved the promotion of high strength, toughness and cell proliferation , provides excellent piezoelectric effects and biomedical applications.
Patent Information
- Application Number
- CN202411208420.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing bone defect repair materials have poor piezoelectric properties, insufficient mechanical properties, difficult to regulate the pore structure, brittle and easy to damage, and poor repair effect.
Coaxial dry spinning wet joint electrospinning method is used to prepare three-dimensional porous hollow nanofiber aerogel. After dissolving the piezoelectric polymer material and pore-forming materials, it is formed to form a mixed solution of nanofibers, and then filtered and added to cross-linked. The agent is sheared, frozen and solidified, forming a hollow nanofiber aerogel with a micro-nano-grade porous structure and a three-dimensional three-dimensional network structure.
Improve the mechanical properties of aerogels and cell adhesion and growth ability, enhance the strength and toughness of the material, realize the precise design of functionalized materials, promote cell proliferation and bone tissue regeneration, provide better piezoelectric effects and Prospects of biomedical application.
Smart Images

Figure CN119061505A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of bone defect repair materials, and more specifically, relates to a three-dimensional porous hollow nanofiber aerogel and a preparation method and application thereof. Background Art
[0002] Bioregenerative materials have application prospects in bone defect repair, joint repair and replacement, and bone scaffold materials, among which bone defect repair is the most common and widespread scenario. From the perspective of the use of bioregenerative materials, most materials are composed of granular or porous structural blocks of a certain geometric shape (such as columnar, blocky, cylindrical), which are used to fill non-load-bearing parts to achieve the filling and repair of hard bone tissue. In terms of material and composition, allogeneic materials, xenogeneic materials, and inorganic materials are the majority, mainly biphasic calcium phosphate ceramics, hydroxyapatite ceramics, β-tricalcium phosphate, and bioactive glass. In contrast, synthetic polymer materials account for a small proportion of approved products, but with the continuous advancement of materials science, their application prospects are still broad.
[0003] Common piezoelectric polymers include polyvinylidene fluoride, polyvinylidene fluoride-trifluoroethylene, polyvinyl fluoride, etc. They are soft and tough, can be made into large-area films, are easy to integrate on a large scale, have low mechanical impedance, and are easy to match with acoustic impedances such as water and the human body. Compared with inorganic piezoelectric materials, they have the advantages of lower dielectric constant, lower density, and higher flexibility, which makes them have good impact resistance and better piezoelectric sensitivity.
[0004] Aerogel materials made by traditional processes are often brittle, and it is difficult to ensure the integrity of the structure under external forces. Compared with traditional aerogels, hollow nanofiber aerogels have lower density, stronger porosity, and larger specific surface area. In particular, they have excellent compression resilience, so the application field of hollow nanofiber aerogels is wider. However, so far, three-dimensional nanofiber aerogels are mainly prepared by freeze-drying after the fragmentation and dispersion of two-dimensional spinning membranes, and the mechanical properties and porous structure of the aerogels obtained in this way are uncontrollable.
[0005] Therefore, existing bone defect repair materials still have problems such as poor piezoelectricity, difficult to control pore structure, brittle and easily damaged materials, and poor repair effect. Summary of the invention
[0006] In view of the above defects or improvement needs of the prior art, the present invention provides a three-dimensional porous hollow nanofiber aerogel and a preparation method and application thereof, the purpose of which is to prepare hollow nanofibers with a micro-nano graded porous structure and a three-dimensional network structure, so as to solve the problems of poor piezoelectricity, insufficient mechanical properties and poor repair effect of existing bone defect repair materials.
[0007] To achieve the above object, according to a first aspect of the present invention, a method for preparing a three-dimensional porous hollow nanofiber aerogel is proposed, comprising the following steps:
[0008] S1, dissolving the piezoelectric polymer material and the pore-forming material in a solvent to obtain a shell layer spinning solution, and dissolving the core layer material in a solvent to obtain a core layer spinning solution;
[0009] S2, using a coaxial dry spinning wet electrospinning method, allowing the shell layer spinning solution and the core layer spinning solution to enter a coagulation bath to obtain a mixed solution with nanofibers;
[0010] S3, filtering the mixed solution containing nanofibers, adding a crosslinking agent, mixing, and shearing to obtain a short fiber dispersion;
[0011] S4. Degas the short fiber dispersion and freeze-solidify it to obtain a three-dimensional porous hollow nanofiber aerogel.
[0012] As further preferred, the concentration of the shell layer spinning solution is 10% to 20%, and the concentration of the core layer spinning solution is 5% to 15%.
[0013] As further preferred, in step S2, the flow rate of the shell layer spinning solution is 10-20 μL / min, and the flow rate of the core layer spinning solution is 2-10 μL / min; the distance from the spinning needle to the coagulation bath collecting plate is 10-20 cm, and the spinning voltage is 8-20 kV.
[0014] As a further preferred embodiment, after the three-dimensional porous hollow nanofiber aerogel is obtained in step S4, it is polarized; the polarization voltage is 1 to 10 kV, and the polarization time is 10 to 60 min.
[0015] As further preferred, in step S2, the coagulation bath is a mixed solution of tert-butanol, 1,4-dioxane and N,N-dimethylformamide; the volume ratio of tert-butanol, 1,4-dioxane and N,N-dimethylformamide in the coagulation bath is (30-45):(5-20):1.
[0016] As further preferred, in step S1, the pore-forming material accounts for 1 wt% to 10 wt% of the piezoelectric polymer material.
[0017] As further preferred, in step S1, the solvent is one of N,N-dimethylformamide, tetrahydrofuran, acetone, dichloroethane, tetrachloroethane, chlorobenzene, cyclohexanone, isopropanol, trifluoroethanol, and glacial acetic acid, or any combination of them; the piezoelectric polymer material includes one of polyvinylidene fluoride, polyvinylidene fluoride-trifluoroethylene, polyvinyl fluoride, polyvinyl chloride, poly-Y-methyl-L-glutamate, polycarbonate, nylon-11, and chitosan, or any combination of them; the pore-forming material is polyethylene glycol, polyvinyl pyrrolidone, polyvinyl alcohol, or cellulose acetate; the core layer material is polyethylene glycol, polyvinyl pyrrolidone, or polyvinyl alcohol.
[0018] As a further preferred embodiment, step S3 specifically includes the following steps: filtering the mixed solution containing nanofibers, then placing it in deionized water for soaking, filtering with filter paper and then washing the nanofibers with a solvent; then adding a crosslinking agent and mixing it evenly using ultrasound, and finally shearing the sample with a disperser to obtain a uniform short fiber dispersion.
[0019] According to a second aspect of the present invention, a three-dimensional porous hollow nanofiber aerogel is provided, which is prepared by the above-mentioned method for preparing the three-dimensional porous hollow nanofiber aerogel.
[0020] According to a third aspect of the present invention, there is provided an application of a three-dimensional porous hollow nanofiber aerogel, wherein the three-dimensional porous hollow nanofiber aerogel is used as a bone defect repair material.
[0021] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:
[0022] 1. The present invention obtains a three-dimensional hollow cage-like nanofiber aerogel through a coaxial dry-spinning wet-joint electrospinning process combined with a subsequent freeze-drying treatment. The three-dimensional hollow cage-like structure and high specific surface area give the aerogel excellent electrical properties. The high specific surface area of the aerogel and the nanoscale pores on the fibers are more conducive to cell adhesion and proliferation, thereby improving cell survival rate and accelerating cell growth.
[0023] 2. The three-dimensional porous hollow nanofibers prepared by the present invention have excellent mechanical properties. Due to their micro-nano hierarchical porous structure and three-dimensional network structure, the material can exhibit better strength and toughness when subjected to external forces.
[0024] 3. The present invention can accurately control the core-shell structure of nanofibers through the coaxial dry spinning wet-joint electrospinning process; compared with the traditional electrospinning technology, the structure is more controllable, and the ratio, morphology and distribution of the core layer and the shell layer can be better adjusted, thereby realizing the precise design of functional materials. Specifically, the aerogel prepared by the coaxial dry spinning wet-joint electrospinning process has a rough fiber surface and is rich in nanopores; the piezoelectric polymer used can generate microcurrents to act on cells under external stimulation, and the porous structure is used to promote the transmission of external mechanical stimulation through the construction of graded porous morphology and hollow cage fibers, thereby increasing the deformation of the material itself, thereby strengthening the piezoelectric effect, making it output a larger and more stable piezoelectric electric field, and stimulating cells to accelerate growth.
[0025] 4. The concentration of the shell spinning solution is 10% to 20%. This concentration range can ensure that the shell has sufficient viscosity to form a stable shell, while avoiding the solution being too viscous, resulting in nozzle blockage or poor fiber morphology. If it is too thin, it will be difficult to form a stable shell. The concentration of the core spinning solution is 5% to 15%. The core solution needs to have a low enough viscosity to flow to the center of the fiber to form a hollow structure. A lower concentration helps control the formation of the core layer and ensure the hollow characteristics of the final fiber. Too high a concentration will cause the shell layer to be unable to wrap and it will be difficult to form a core layer.
[0026] 5. The flow rate of the shell spinning solution is 10-25 μL / min. The higher the flow rate of the shell solution, the better the integrity and mechanical strength of the shell, and is suitable for forming a strong shell structure. The flow rate of the core spinning solution is 2-10 μL / min. The lower the flow rate of the core solution, the better the hollow structure is, and the core layer is prevented from overfilling and affecting the formation of hollow fibers. The spacing from the spinning needle to the coagulation bath collection plate is 10-20 cm. The larger the spacing, the more time the fiber has to dry in the air during the spinning process, which has an important influence on the morphology and structure of the fiber. A smaller spacing may cause the fiber to enter the coagulation bath before it is fully solidified, thus affecting the morphology and pore structure of the fiber. The spinning voltage is 8-20 kV. Too high a voltage may lead to unstable jetting and irregular fiber formation. Too low a voltage may not form a stable jet. A moderate voltage helps to form uniform fibers and ensure the stability of the core-shell structure.
[0027] 6. The magnitude of the polarization voltage will affect the orientation of the electric dipoles inside the material. A voltage that is too high may cause electrical breakdown of the material, while a voltage that is too low may not be effectively polarized. The present invention can significantly improve the electrical properties of the three-dimensional porous hollow nanofiber aerogel by reasonably setting the polarization voltage and time, providing better performance guarantee for its application in the field of biomedical repair.
[0028] 7. The method for preparing three-dimensional porous hollow nanofiber aerogel of the present invention has a simple and feasible processing process, has no special requirements for equipment in the processing technology, is relatively easy to produce, can be directly implanted into bone defects or directly used in the culture of dental pulp cells, can regulate the electrical microenvironment, stimulate and promote cell proliferation, and promote bone tissue regeneration, and has great application prospects in the biomedical field.
[0029] 8. The three-dimensional porous hollow nanofiber aerogel prepared by the present invention has high flexibility and elasticity of compressive stress, and can still recover its original shape under the action of high pressure stress. The optimal output value of the nanogenerator device assembled from the aerogel is 162V.
[0030] 9. High stability of preparation process:
[0031] Strong process repeatability: The key process parameters in this technical solution (such as spinning voltage, distance from needle to collecting plate, coagulation bath conditions, etc.) have been optimized to stably produce consistent and high-quality nanofibers, ensuring batch-to-batch consistency of the product.
[0032] Wide material compatibility: This technology can be applied to the preparation of a variety of polymers and composite materials, has strong adaptability, and can be applied in different fields through material selection and process control.
[0033] 10. Environmental friendliness:
[0034] Reduce solvent residue: During the dry spinning stage, the solvent in the spinning solution partially evaporates, reducing the solvent residue in the final product, which helps to improve the biocompatibility and environmental friendliness of the product.
[0035] Green preparation process: This process can further reduce the impact on the environment by selecting low-toxic, degradable solvents and materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 (a)-(c) are morphological images of PVDF aerogel fibers in Examples 1-3 of the present invention;
[0037] Figure 2 This is a 20,000-fold magnified SEM image of the surface fiber of the PVDF aerogel in an embodiment of the present invention;
[0038] Figure 3 This is a SEM image of the surface fiber of the PVDF aerogel according to the embodiment of the present invention magnified 100,000 times;
[0039] Figure 4 This is a schematic diagram of the activity of PVDF aerogel after contact with bone marrow mesenchymal stem cells according to an embodiment of the present invention. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0041] The present invention provides a method for preparing a three-dimensional porous hollow nanofiber aerogel, comprising the following steps:
[0042] S1. Dissolving the piezoelectric polymer material and the pore-forming material in a solvent to prepare a shell layer spinning solution, and dissolving the core layer material in a solvent to prepare a core layer spinning solution.
[0043] The role of the pore-forming material in the spinning solution is, on the one hand, to form nanopores on the fiber surface by doping-etching the pore-forming material, and on the other hand, to improve the hydrophilicity of the piezoelectric polymer, thereby increasing the compatibility of the fiber with the coagulation bath, so that it can be better dispersed in the coagulation bath.
[0044] S2. Based on the shell spinning solution and the core spinning solution, a coaxial dry spinning and wet joining electrospinning process is adopted to obtain a mixed solution with nanofibers.
[0045] The principle of the coaxial dry spinning wet joining electrospinning process is: using a coaxial nozzle, two different spinning solutions are extruded simultaneously to form a fiber with a core-shell structure. The inner nozzle is responsible for the core layer solution, and the outer nozzle is responsible for the shell layer solution; under the action of a high voltage electric field, the spinning solution forms a jet and is stretched to form a fiber during the jetting process. During the spinning process, the fiber is dried in the air, the solvent evaporates, and a preliminary solid fiber is formed. After dry spinning, the fiber passes through a wet joining area, that is, the fiber is introduced into a wet joining area containing a coagulant or other solution, so that the fiber is further processed or solidified to form a target structure, such as a hollow or porous nanofiber.
[0046] Specifically, the core layer and shell layer spinning solutions are loaded into the inner and outer tubes of the coaxial nozzle respectively. Under the action of high voltage, the solution is ejected from the nozzle to form a fiber with a core-shell structure. After the dry spinning process, the shell layer is usually in a partially solidified state. At this time, the solvent has partially volatilized, and the shell fiber has a certain mechanical strength, but still maintains a certain flexibility; in this way, when entering the coagulation bath, the shell layer can continue to solidify or shape to form a stable shell structure. Due to the low flow rate and low solution viscosity of the core layer, it is often still in a liquid or semi-liquid state when entering the coagulation bath. This state helps to form a hollow structure because the core layer solution can shrink and solidify rapidly in the coagulation bath to form a hollow core part. When entering the coagulation bath, the shell layer is in a semi-solidified state with a certain mechanical strength, while the core layer is closer to a liquid or semi-liquid state. Through the solvent exchange and solidification process in the coagulation bath, the two work synergistically to eventually form a hollow nanofiber with a micro-nano hierarchical porous structure and a three-dimensional network structure. Finally, the core-shell structured fibers are drawn into the coagulation bath area, and further processed in the coagulation bath to form porous or hollow structured fibers, thereby finally obtaining a mixed coagulation bath solution with porous hollow nanofibers.
[0047] S3. Filter the mixed solution containing nanofibers, and then put it into deionized water to soak for a period of time, filter it with filter paper, and wash the fibers with solvent several times, then add a cross-linking agent and use an ultrasonic instrument to mix it evenly, and finally use a disperser to shear the sample at high speed to obtain a uniform short fiber dispersion.
[0048] S4. After ultrasonically degassing the short fiber dispersion, place it in a refrigerator to stand, freeze it to solidify, and finally place it in a freeze dryer for freeze drying to obtain a three-dimensional porous hollow nanofiber aerogel material.
[0049] S5. Apply a high voltage electric field to the three-dimensional porous hollow nanofiber aerogel material to polarize it for a period of time.
[0050] The obtained three-dimensional porous hollow nanofiber aerogel has a three-dimensional porous structure, the fiber surface is covered with nano-scale voids, the fibers are interlaced to form a network structure, and the fiber surface is rough and has multiple through holes.
[0051] Furthermore, the pore-forming material accounts for 1wt%-10wt% of the piezoelectric polymer material; in the total mass of the aerogel finally obtained, the piezoelectric polymer material accounts for 90%-99%, and the cross-linking agent accounts for 1%-10%.
[0052] Furthermore, in step S1, the concentration of the shell layer spinning solution is 10% to 20%, and the concentration of the core layer spinning solution is 5% to 15%; further preferably, the concentration of the shell layer spinning solution is 15%, and the concentration of the core layer spinning solution is 10%.
[0053] Further, in step S1, the solvent is one of N,N-dimethylformamide (DMF), tetrahydrofuran (THF), acetone, dichloroethane, tetrachloroethane, chlorobenzene, cyclohexanone, isopropanol, trifluoroethanol, and glacial acetic acid, or any combination of them; the piezoelectric polymer material includes one of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-trifluoroethylene (PVDF-TrFE), polyvinyl fluoride (PVF), polyvinyl chloride (PVC), poly-Y-methyl-L-glutamate (PMLG), polycarbonate (PC), nylon-11, and chitosan, or any combination of them; the pore-forming material is polyethylene glycol (PEG), polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA), or cellulose acetate (CA); and the core layer material is polyethylene glycol (PEG), polyvinyl pyrrolidone (PVP), or polyvinyl alcohol (PVA).
[0054] Furthermore, in step S2, the coagulation bath is a mixed solution of tert-butanol, 1,4-dioxane and N,N-dimethylformamide; the volume ratio of tert-butanol, 1,4-dioxane and N,N-dimethylformamide in the coagulation bath is preferably (30-45):(5-20):1.
[0055] Further, in step S2, the flow rate of the shell spinning solution in the syringe is 10 to 25 μL / min, and the flow rate of the core spinning solution is 2 to 10 μL / min. The flow rate ratio of the shell and core spinning solutions is 1.5:1 to 4:1. A higher shell flow rate can ensure the structural stability of the fiber, while a lower core flow rate helps to form a clear hollow structure. The distance from the spinning needle to the coagulation bath collection plate is 10 to 20 cm, and the spinning voltage is 8 to 20 kV. Ensure that the fiber enters the coagulation bath stably and continuously.
[0056] Further, in step S3, a cross-linking agent dispersion is weighed according to 1% to 5% (w / v) of the mass of the nanofibers obtained by spinning; the cross-linking agent is used as a cross-linking agent for aerogel, including gelatin, aqueous polyurethane, chitosan, collagen, hyaluronic acid, fibrin, alginate, cellulose, agarose, dextran, guar gum, etc.
[0057] Further, in step S3, the fiber is placed in deionized water and allowed to stand and soak for 5 to 36 hours, and tert-butyl alcohol or 1,4-dioxane is used as the solvent for cleaning the fiber; during ultrasonic mixing, the ultrasonic time is 5 to 60 minutes (ultrasonic power is 130 W), and the speed of the disperser is 2000 to 8000 r / min.
[0058] Furthermore, in step S4, during ultrasonic defoaming, the ultrasonic time is 5 to 60 minutes; and the freeze-drying time is 12 to 72 hours.
[0059] Furthermore, in step S5, the polarization voltage is 1 to 10 kV, and the polarization time is 10 to 60 min.
[0060] The aerogel prepared by the present invention has advantages such as nano-level three-dimensional hollow nanofiber structure, excellent piezoelectric properties and high flexibility. It can respond to tiny movements and convert mechanical energy into electrical energy. Implanting the three-dimensional porous hollow nanofiber aerogel into bone defects or directly applying it to the culture of dental pulp cells can regulate the electrical microenvironment, stimulate and promote cell proliferation, and promote bone tissue regeneration, which has great application prospects in the biomedical field.
[0061] The following are specific embodiments:
[0062] Example 1
[0063] (1) Preparation of spinning solution: Weigh PVDF and PVP, add appropriate amounts of N,N-dimethylformamide and tetrahydrofuran to prepare a shell spinning solution with a concentration of 10% (w / v); weigh a certain amount of PEG and dissolve it in tetrahydrofuran to prepare a core spinning solution with a concentration of 5% (w / v); then magnetically stir the solution at 50°C for 12 h and then let it stand for 1 h, and use a vacuum pump to slowly evacuate the shell and core spinning solutions for multiple times to remove bubbles, and finally obtain a uniform spinning solution.
[0064] (2) Preparation of hollow nanofibers: The prepared spinning solutions were then placed in two 10 mL syringes, and the flow rates of the shell solution and the core solution were controlled to be 20 μL / min and 10 μL / min respectively by the syringe pump. A water bath with a coagulation bath was used as the receiving end, the distance between the coaxial needle and the bottom of the water bath was fixed to 15 cm, and the spinning voltage was set to 15 kV. The solution in the coagulation bath at the receiving end was a mixed solvent (4:1:0.1) consisting of tert-butyl alcohol, 1,4-dioxane and DMF. The role of DMF was to improve the compatibility of the spinning fiber with the coagulation bath solvent, reduce the surface tension of the spinning fiber when entering the coagulation bath, and thus reduce the beading phenomenon during nanofiber spinning. Since the piezoelectric polymer is insoluble in tert-butyl alcohol and 1,4-dioxane, solvent phase separation will occur after the spinning fiber enters the coagulation bath, causing the nanofibers to precipitate and accumulate into a three-dimensional structure in the coagulation bath. PVP and PEG are dissolved in tert-butyl alcohol and 1,4-dioxane, so hollow nanofibers can be obtained, and nanopores are generated on their surfaces.
[0065] (3) The mixed solution obtained by electrospinning was filtered with filter paper and washed with 1,4-dioxane several times to remove the organic solvent remaining in the spinning process; the obtained fiber was soaked in deionized water for a period of time; after filtering, the crosslinker dispersion was weighed according to 3% (w / v) of the mass of the fiber obtained by spinning, and a certain amount of 1,4-dioxane was added, and the mixed solution was ultrasonicated for 10 minutes (ultrasonic power was 130W) to obtain a 1,4-dioxane / crosslinker homogeneous system; the 1,4-dioxane crosslinker homogeneous system was added to the filtered hollow fiber, and the sample was sheared at high speed for 30 minutes using a homogenizer disperser to obtain short fibers (speed 5000r / min), and the dispersed solution was placed in an ultrasonic cleaner for cleaning for 20 minutes, and the bubbles in the solution were removed by vacuum pump, and finally placed in a refrigerator for 1 hour.
[0066] (4) The gel solution obtained after standing is frozen and solidified with ethanol / liquid nitrogen, and then placed in a freeze dryer. After 72 hours of freeze drying, the final three-dimensional porous hollow nanofiber aerogel material can be obtained.
[0067] (5) The obtained aerogel is polarized at 5 kV for 30 min to obtain the final high-performance three-dimensional porous hollow nanofiber aerogel.
[0068] (6) Hollow nanofiber porous aerogels were used in culture experiments of dental pulp cells and bone cells.
[0069] Example 2
[0070] The steps of this embodiment are the same as those of embodiment 1, except that:
[0071] The concentration of the shell layer spinning solution is configured to be 15% (w / v); the concentration of the core layer spinning solution is configured to be 10% (w / v).
[0072] Example 3
[0073] The steps of this embodiment are the same as those of embodiment 1, except that:
[0074] The concentration of the shell layer spinning solution is configured to be 20% (w / v); the concentration of the core layer spinning solution is configured to be 15% (w / v).
[0075] The morphology of the PVDF aerogel fibers in Examples 1-3 is as follows: Figure 1As shown, it can be seen that the fiber structure is uniform, the fiber surface quality is good, and the pore distribution is uniform, which helps to improve the mechanical properties and functional stability of the material, among which Example 2 is the best. In addition, the piezoelectric properties of the polarized aerogels were tested. At a vibration frequency of 30 Hz, the output voltages of the aerogels of Examples 1-3 were 148 V, 162 V, and 154 V, respectively; this indicates that the fiber has a good polarization effect, a stable electric dipole orientation, and a high piezoelectric coefficient, thus exhibiting a good piezoelectric effect. In addition, the compression resilience properties of the aerogels were tested using a compression testing machine, and all had good compression resilience, making them suitable for implantation in bone defects and the development of multifunctional composite materials.
[0076] The enlarged image of the fiber surface of the PVDF aerogel obtained in Example 1 is as follows Figure 2 and Figure 3 As shown, it can be clearly seen that the PVDF aerogel bone repair material has a porous structure and nanofiber pores, which makes the material conducive to cell adhesion, growth and reproduction. In addition, it can be seen that the fibers of the PVDF aerogel are hollow and porous cage-like structures with a high specific surface area, which is conducive to converting mechanical energy into electrical energy with high conversion efficiency. Therefore, small external stimuli can be converted into electrical energy to stimulate and promote cell proliferation, regulate the electrical microenvironment, and promote bone repair. Figure 4 It can be seen that the cell activity of the PVDF aerogel scaffold after high-voltage polarization activation is improved. From the cell activity results, it can be observed that the percentage of live cells from 1 to 7 days is above 80%, indicating that the aerogel material used is non-cytotoxic and has good biocompatibility.
[0077] Example 4
[0078] The steps of this embodiment are the same as those of embodiment 2, except that:
[0079] The shell layer spinning solution is prepared by using PVDF-TrFE as the shell layer material and PVA as the core layer material, and DMF and acetone as solvents; the core layer spinning solution is prepared by using PVP as the core layer material and THF as the solvent.
[0080] The flow rate of the shell solution was controlled to be 15 μL / min and the flow rate of the core solution was controlled to be 6 μL / min by the injection pump; the distance between the coaxial needle and the bottom of the water bath was fixed to be 13 cm, and the spinning voltage was set to be 12 kV. In this embodiment, the materials of the shell and core spinning solutions were changed, and the spinning process was made more gentle and stable by adjusting the spinning flow rate and the spinning voltage, which was conducive to the formation of fibers with better morphology and the generation of hollows and pores.
[0081] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a three-dimensional porous hollow nanofiber aerogel, characterized in that: The steps include: S1, dissolving the piezoelectric polymer material and the pore-forming material in a solvent to obtain a shell layer spinning solution, and dissolving the core layer material in a solvent to obtain a core layer spinning solution; S2, using a coaxial dry spinning wet electrospinning method, allowing the shell layer spinning solution and the core layer spinning solution to enter a coagulation bath to obtain a mixed solution with nanofibers; S3, filtering the mixed solution containing nanofibers, adding a crosslinking agent, mixing, and shearing to obtain a short fiber dispersion; S4. Degas the short fiber dispersion and freeze-solidify it to obtain a three-dimensional porous hollow nanofiber aerogel.
2. The method for preparing the three-dimensional porous hollow nanofiber aerogel according to claim 1, characterized in that: The concentration of the shell layer spinning solution is 10% to 20%, and the concentration of the core layer spinning solution is 5% to 15%.
3. The method for preparing the three-dimensional porous hollow nanofiber aerogel according to claim 1, characterized in that: Step S2, the flow rate of the shell layer spinning solution is 10-20 μL / min, the flow rate of the core layer spinning solution is 2-10 μL / min; the distance from the spinning needle to the coagulation bath collecting plate is 10-20 cm, and the spinning voltage is 8-20 kV.
4. The method for preparing the three-dimensional porous hollow nanofiber aerogel according to claim 1, characterized in that: After the three-dimensional porous hollow nanofiber aerogel is obtained in step S4, it is polarized; the polarization voltage is 1 to 10 kV, and the polarization time is 10 to 60 minutes.
5. The method for preparing the three-dimensional porous hollow nanofiber aerogel according to claim 1, characterized in that: In step S2, the coagulation bath is a mixed solution of tert-butanol, 1,4-dioxane and N,N-dimethylformamide; the volume ratio of tert-butanol, 1,4-dioxane and N,N-dimethylformamide in the coagulation bath is (30-45):(5-20):
1.
6. The method for preparing the three-dimensional porous hollow nanofiber aerogel according to claim 1, characterized in that: Step S1, the pore-forming material accounts for 1wt% to 10wt% of the piezoelectric polymer material.
7. The method for preparing the three-dimensional porous hollow nanofiber aerogel according to claim 1, characterized in that: Step S1, the solvent is one of N,N-dimethylformamide, tetrahydrofuran, acetone, dichloroethane, tetrachloroethane, chlorobenzene, cyclohexanone, isopropanol, trifluoroethanol, glacial acetic acid, or any combination of them; the piezoelectric polymer material includes one of polyvinylidene fluoride, polyvinylidene fluoride-trifluoroethylene, polyvinyl fluoride, polyvinyl chloride, poly-Y-methyl-L-glutamate, polycarbonate, nylon-11, and chitosan, or any combination of them; the pore-forming material is polyethylene glycol, polyvinyl pyrrolidone, polyvinyl alcohol, or cellulose acetate; the core layer material is polyethylene glycol, polyvinyl pyrrolidone, or polyvinyl alcohol.
8. The method for preparing the three-dimensional porous hollow nanofiber aerogel according to any one of claims 1 to 7, characterized in that: Step S3 specifically includes the following steps: filtering the mixed solution containing nanofibers, then placing it in deionized water for soaking, filtering with filter paper and then washing the nanofibers with a solvent; then adding a crosslinking agent and mixing it evenly using ultrasound, and finally shearing the sample with a disperser to obtain a uniform short fiber dispersion.
9. A three-dimensional porous hollow nanofiber aerogel, characterized in that: The three-dimensional porous hollow nanofiber aerogel is prepared by the preparation method of any one of claims 1 to 8.
10. An application of the three-dimensional porous hollow nanofiber aerogel as claimed in claim 9, characterized in that: The three-dimensional porous hollow nanofiber aerogel is used as a bone defect repair material.
Citation Information
Patent Citations
Preparation method of efficient oil-absorbing nanofiber aerogel
CN111135771A
Nanofiber 3D porous aerogel and preparation method and application thereof
CN113730662A
Cited By
Flame-retardant and heat-insulating aerogel composite material as well as preparation method and application thereof
CN120736873A
Ceramic nanofiber aerogel with high compression strength and low thermal conductivity and preparation method thereof
CN121021173A