Polyimide heat insulation nanofiber with controllable cavity structure as well as preparation method and application of polyimide heat insulation nanofiber
By using coaxial electrospinning technology in polyimide materials, composite nanofibers with core-shell structures are prepared, and a controlled cavity structure is formed through step-by-step heating and calcination, the separation of polyimide materials in extreme environments is solved. The problem of insufficient thermal insulation performance and mechanical performance achieves a combination of efficient heat insulation and excellent mechanical properties.
Patent Information
- Application Number
- CN202411386754.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing polyimide materials have poor thermal insulation and mechanical properties in extreme environments, mainly due to the inability to regulate the shape, size and distribution of the cavity structure.
Coaxial electrospinning technology is used to prepare composite nanofibers with core-shell structures at high voltages, and a controllable cavity structure is formed through step-by-step heating and calcination, and the shape and size of the cavity structure are adjusted to improve thermal insulation performance.
It significantly reduces the thermal conductivity of nanofibers, improves thermal insulation and mechanical properties, is suitable for extreme environments, and has reduced material density and high porosity, and has self-cleaning function.
Smart Images

Figure CN119061510A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new thermal insulation materials, and specifically relates to a polyimide thermal insulation nanofiber with a controllable cavity structure, a preparation method and an application thereof. Background Art
[0002] Thermal insulation materials (which can block heat flow transfer) involve various fields such as energy management and thermal protection of human life and health, and play a vital role. Among them, the composition selection and structural design of thermal insulation materials are the key to determining their thermal insulation performance. Compared with natural thermal insulation materials such as cotton, linen, and silk, synthetic thermal insulation materials such as polyester and polyurethane have the advantages of low cost and stable performance, but it is still difficult to meet the high requirements of thermal protection in extreme environments such as space and deep sea. Although some inorganic thermal insulation materials can achieve thermal protection in extreme environments, their structural brittleness and high density make it difficult for inorganic thermal insulation materials to be widely popularized.
[0003] Polyimide is a type of macromolecular polymer with imide groups in the main chain. Its low thermal conductivity, high mechanical properties and good thermal stability enable it to shine as a thermal insulation material in extreme environments. Existing studies have shown that compared with other polymers, the thermal conductivity of polyimide materials is lower, about 0.25 W·m at room temperature. -1 ·K -1 . However, faced with the challenge of efficient thermal insulation in current extreme environments, simple polyimide and its composite materials are difficult to meet the demand. The existing patent CN106498558B discloses a coaxial electrospun polyimide micro / nano hollow structure material and its preparation method, which has a simple process and safe and controllable conditions. However, the shape, size and distribution of the hollow structure cannot be controlled, resulting in poor thermal insulation and mechanical properties of the obtained polyimide material in extreme environments. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a polyimide nanofiber thermal insulation material with a controllable cavity structure and a preparation method and application thereof, so as to overcome the problem that the shape, size and distribution of the cavity structure of the existing polyimide materials cannot be controlled, resulting in poor thermal insulation and mechanical properties in extreme environments.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions: The invention discloses a method for preparing polyimide heat-insulating nanofibers with a controllable cavity structure, comprising the following steps: 1) dissolving dianhydride and diamine monomers in an organic solvent to prepare an electrospinning shell layer solution; dissolving a template substance in an organic solvent to prepare an electrospinning core layer solution; wherein the template substance is one of polymethyl methacrylate, thermoplastic polyurethane or polyvinyl pyrrolidone; 2) The coaxial electrospinning technology was used to stretch the electrospinning shell solution and the core solution under high voltage to obtain composite nanofibers with a core-shell structure; the spinning voltage was 10-25 kV, the distance between the needle and the receiving platform was 5-15 cm, the pushing rate was 0.05-1..2 mL / h, and the spinning temperature was 20-50 ℃.
[0006] 3) The composite nanofibers with a core-shell structure are calcined in a stepwise manner under an inert gas atmosphere to obtain polyimide thermal insulation nanofibers with a controllable cavity structure.
[0007] The presence of the above-mentioned cavity structure greatly reduces the heat conduction path inside the nanofiber. Heat conduction is one of the main ways of heat transfer. When there are a large number of cavities in the material, the heat needs to bypass these cavities during the transfer process, thereby increasing the resistance to heat conduction and reducing the efficiency of heat conduction. The air in the cavity structure is a poor conductor of heat, and its thermal conductivity is much lower than that of solid materials. Therefore, by introducing a cavity structure into the nanofiber, it is equivalent to adding a large number of thermal resistance units inside the material. These thermal resistance units can effectively block the transfer of heat, so that the heat is more hindered when passing through the material, thereby improving the thermal insulation performance of the material.
[0008] During the preparation process, the selected template material (polymethyl methacrylate, thermoplastic polyurethane or polyvinyl pyrrolidone) has an important influence on the shape of the final cavity structure. The morphology and properties of different template materials will result in different shapes of cavities produced by decomposition during the calcination process. The shape of the cavity structure directly affects the heat conduction path inside it. Nanofibers with complex-shaped cavities can more effectively block the direct conduction of heat, because heat needs to bypass or pass through these cavities and complex structures during the transfer process, thereby increasing the resistance to heat conduction and reducing the efficiency of heat conduction, thereby improving the thermal insulation performance of the nanofibers.
[0009] In the coaxial electrospinning process, by adjusting the spinning voltage, the distance between the needle and the receiving platform, the pushing rate, and the spinning temperature and other parameters, the drawing speed and morphology of the shell solution and the core solution can be controlled, thereby controlling the size of the cavity structure. The present invention optimizes the size of the cavity structure to 703 nm, and this aperture greatly limits the thermal motion of gas molecules, thereby effectively inhibiting gas phase heat transfer. This nanocavity effect reduces the efficiency of heat transfer directly through the gas by increasing the tortuosity of the heat conduction path, which significantly reduces the thermal conductivity of the material, even lower than the thermal conductivity of static air, and greatly improves the thermal insulation performance of the material.
[0010] Furthermore, in step 1), the mass ratio of dianhydride to diamine monomer is 0.8:1.2, N,N-dimethylformamide.
[0011] Furthermore, in step 1), the dianhydride monomer is one of 4,4′-biphenyl ether dianhydride, 3,3′,4,4′-biphenyltetracarboxylic acid dianhydride or pyromellitic acid anhydride, and the diamine monomer is one of p-phenylenediamine, 4,4′-diaminodiphenyl ether or 1H-benzimidazole-1,2-diamine.
[0012] Furthermore, in step 1), the mass of the organic solvent is 2-4 times the total mass of the monomers, and the organic solvent is one or two of N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylformamide / toluene or N,N-dimethylformamide / tetrahydrofuran.
[0013] Furthermore, in step 1), the mixed solution of dianhydride and diamine monomers and organic solvent is fully reacted in a water bath at 0-10°C for 3-6 hours at a mechanical stirring rate of 200-500 r / min to obtain a light yellow transparent viscous electrospinning shell solution.
[0014] Furthermore, in step 2), the electrospinning shell layer solution and the core layer solution are subjected to vacuum degassing treatment at 20-30° C., respectively, and then the electrospinning shell layer solution and the core layer solution are stretched using coaxial electrospinning technology.
[0015] Furthermore, in step 3), the step-by-step temperature calcination is as follows: in an inert gas atmosphere, the temperature is first increased from 30°C to 150~230°C at a rate of 5~10°C / min and kept for 0.5~2h, then increased to 280~350°C and kept for 0.5~2h, then increased to 400~500°C and kept for 0.5~2h, and finally cooled naturally.
[0016] The present invention also discloses a polyimide thermal insulation nanofiber with a controllable cavity structure prepared by the preparation method of any one of the above-mentioned polyimide thermal insulation nanofibers with a controllable cavity structure. The polyimide thermal insulation nanofiber has a cavity structure inside, and the cavity diameter is 45 nm-703 nm.
[0017] Furthermore, the thermal insulation temperature of imide nanofibers is -196~400°C, and the thermal conductivity is 0.020~0.0261W·m -1 ·K -1 ; Porosity is 97.8~99.2%, and volume density is 0.020~0.035 g / cm 3 , the water contact angle is 140°~145°.
[0018] Furthermore, the above-mentioned controllable cavity structure polyimide thermal insulation nanofiber is used in thermal insulation materials.
[0019] Compared with the prior art, the present invention has the following beneficial effects: The invention discloses a method for preparing a polyimide heat-insulating nanofiber with a controllable cavity structure. First, an electrospinning shell solution and a core solution are prepared. The nanofiber is prepared by using a template material (one of polymethyl methacrylate, thermoplastic polyurethane or polyvinyl pyrrolidone), so as to achieve the regulation of the cavity structures of different shapes in the polyimide heat-insulating nanofiber. The nanofiber with a complex cavity shape can more effectively block the direct conduction of heat, because the heat needs to bypass or pass through these cavities and complex structures during the transfer process, thereby increasing the resistance of heat conduction and reducing the heat conduction efficiency, thereby obtaining a nanofiber with low thermal conductivity and improving the heat insulation performance of the nanofiber; secondly, the shell solution and the core solution are synchronously spun by coaxial electrospinning technology to form a composite nanofiber with a core-shell structure. The size of the cavity diameter can be controlled by adjusting the process parameters such as the shell concentration and the core pushing rate, thereby obtaining a polyimide heat-insulating nanofiber with low thermal conductivity. The pore size greatly limits the thermal motion of gas molecules, thereby effectively inhibiting gas phase heat transfer. This nanocavity effect reduces the efficiency of heat transfer directly through the gas by increasing the tortuosity of the heat conduction path, significantly reducing the thermal conductivity of the material, even lower than the thermal conductivity of static air, and greatly improving the thermal insulation performance of the material. Experimental verification shows that the diameter of the cavity structure in the nanofiber prepared by the present invention is 45-703 nm; finally, the aforementioned composite nanofiber is subjected to a step-by-step temperature calcination treatment to achieve the thermal imidization reaction of the composite nanofiber and the removal of the core layer template material, and successfully prepares a polyimide nanofiber with a controllable cavity structure. In summary, by selecting the template material and setting parameters such as the pushing rate, the precise control of nanofibers with cavity structures of different shapes and sizes is achieved, thereby obtaining polyimide nanofibers with low thermal conductivity, thereby achieving high-efficiency thermal insulation performance and excellent mechanical properties of polyimide thermal insulation nanofibers in extreme environments.
[0020] Furthermore, the step-wise temperature rise calcination treatment in the preparation method causes the polyamic acid (PAA) shell layer in the composite nanofiber with a core-shell structure to undergo a thermal imidization reaction and be converted into polyimide (PI), and simultaneously removes the core layer template material to form a cavity structure. Specifically, the step-wise temperature rise is performed at a rate of 5 to 10 °C / min in an inert gas atmosphere.
[0021] (1) The temperature is raised from 30 °C to 150-230 °C and kept at this temperature for 0.5-2 h. The purpose of this stage is to gradually evaporate the solvent in the fiber and prepare for the subsequent thermal imidization reaction.
[0022] (2) The temperature is further raised to 280-350 °C and kept within this temperature range for 0.5-2 h. At this stage, the polyamic acid shell begins to undergo thermal imidization reaction, that is, the amide bond in the molecule undergoes dehydration cyclization to form a stable imide ring structure. This process is a cyclization reaction, in which the nitrogen atom on the amide bond attacks the carbon atom in the carboxylic acid by nucleophilic attack and eliminates the water molecule, thereby forming a stable imide ring structure. This reaction process converts polyamic acid into polyimide, thereby giving the fiber excellent thermal stability and low thermal conductivity.
[0023] (3) After the thermal imidization reaction is completed, continue to heat up to 400~500℃ and keep it warm for 0.5~2h. The purpose of this stage is to completely remove the core layer template material (such as polymethyl methacrylate, thermoplastic polyurethane or polyvinyl pyrrolidone, etc.), thereby forming a cavity structure inside the fiber. This cavity structure helps to improve the thermal insulation and mechanical properties of the fiber.
[0024] During the thermal imidization process, the removal of the template material not only forms a cavity structure, but also leads to a significant shrinkage of the fiber volume. This volume shrinkage effect combined with the formation of the internal cavity greatly reduces the density of the material, reaching an ultra-light level. At the same time, the complete removal of the template material also ensures the high porosity of the material, further enhancing its thermal insulation performance.
[0025] The present invention also discloses a polyimide thermal insulation nanofiber with a controllable cavity structure. By regulating the shape, size and distribution of the cavity structure inside the fiber, the thermal conductivity of the polyimide nanofiber can be precisely controlled, thereby obtaining a polyimide thermal insulation nanofiber with high-efficiency thermal insulation performance and excellent mechanical properties.
[0026] Furthermore, the polyimide heat-insulating nanofiber of the present invention has a cavity structure constructed inside, and the cavity diameter is controlled to be 45-703 nm, thereby achieving ultra-low thermal conductivity, high-efficiency thermal insulation and excellent mechanical properties of the polyimide nanofiber. On the one hand, the controllable cavity structure constructed inside the polyimide nanofiber, whose nanometer-level pore size greatly limits the thermal motion of gas molecules, thereby effectively inhibiting gas phase heat transfer. This nanocavity effect reduces the efficiency of heat transmission directly through the gas by increasing the tortuosity of the heat conduction path, so that the thermal conductivity of the material is significantly reduced, even lower than the thermal conductivity of static air. On the other hand, the solid / solid interface formed between the fibers, as a scattering center of phonons (quantized particles for heat transfer) during the heat conduction process, effectively reduces the linear propagation of phonons and increases the scattering and reflection of phonons. This phonon scattering mechanism further weakens the heat conduction efficiency, and synergizes with the nanocavity effect to achieve the characteristics of ultra-low thermal conductivity. On the third hand, the cavity structure inside the nanofiber will undergo plastic deformation when subjected to external force. During this plastic deformation process, the growth and reconstruction of the cavity consumes part of the external input energy, thereby slowing down the overall deformation rate of the material. In addition, the presence of the cavity also increases the stress concentration points inside the fiber, promotes the deflection and bifurcation of the crack, improves the fracture toughness of the material, and makes the material have excellent mechanical properties. Experimental measurements show that the temperature tolerance of polyimide thermal insulation nanofibers is -70-300°C, and the thermal conductivity is 0.020~0.0261 W·m -1 ·K -1 , effectively reducing heat transfer and improving thermal insulation effects; its interior has an ultra-high porosity of 97.8~99.2%, and its volume density can be controlled at 0.020~0.035 g / cm 3 The microporous structures not only help reduce the density of the material, but also further improve the thermal insulation effect. The low surface energy characteristics of polyimide fibers come from the hydrophobic groups in their molecular structure. These hydrophobic groups form a protective layer on the fiber surface, making it difficult for water molecules to adhere to and spread on its surface. When a water droplet contacts the fiber surface, due to the effect of surface tension, the water droplet will present a high contact angle (WCA=140°~145°), so that it will quickly roll off and carry away the pollutants on the surface, and it is not easily wetted by water or liquid, thus achieving a self-cleaning function. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a scanned image of the polyimide heat-insulating nanofiber with a controllable cavity structure of the present invention; Figure 2 This is a transmission image of the controllable cavity structure polyimide heat insulation nanofiber of the present invention, in which the internal cavity structure is in the shape of a mesopore; Figure 3 This is a transmission image of the bamboo-like internal cavity structure of the polyimide heat-insulating nanofiber with controllable cavity structure of the present invention; Figure 4 This is a transmission image of the controllable cavity structure polyimide thermal insulation nanofiber of the present invention, in which the internal cavity structure is mesoporous; Figure 5 This is the water contact angle image of the polyimide heat insulation nanofiber with controllable cavity structure of the present invention; Figure 6 This is a comparison chart of thermal conductivity of intrinsic polyimide, solid polyimide nanofiber, and polyimide heat-insulating nanofiber with controlled cavity structure of the present invention; Figure 7 This is an infrared thermal imaging image of the polyimide heat-insulating nanofiber with a controllable cavity structure of the present invention; Figure 8 This is an infrared thermal imaging image of the polyimide heat-insulating nanofiber with controllable cavity structure of the present invention. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0029] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0030] The present invention is described in further detail below in conjunction with embodiments: Example 1 Step 1): First, 18.4 g of 4,4'-diaminodiphenyl ether was dissolved in N,N-dimethylformamide solution with a mass of 4 times the total mass of the monomers, argon was introduced, and the mixture was stirred in a water bath at 0 °C under mechanical stirring at 300 r / min until completely dissolved. 20.2 g of pyromellitic anhydride was added in batches in 6 times, keeping the molar ratio of dianhydride to diamine at 1, with an interval of 20 min each time. After the addition was completed, stirring was continued for 5 h to obtain a light yellow transparent viscous electrospinning shell solution with a solid content of 20%, which was refrigerated for later use; then 15 g of polymethyl methacrylate was dissolved in 35 g of N,N-dimethylformamide at room temperature to obtain an electrospinning core solution, which was refrigerated for later use.
[0031] Step 2): The shell layer solution and the core layer solution obtained in step 1) were subjected to vacuum degassing treatment at 25 °C, and then connected to the 17 / 22G coaxial spinning needle of the electrospinning machine using a hose and spun continuously for 8 h to form composite nanofibers with a core-shell structure. The spinning voltage was 16 kV, the distance between the needle and the receiving platform was 8 cm, the shell layer push rate was 0.23 mL / h, the core layer push rate was 0.45 mL / h, and the spinning temperature was 30 °C.
[0032] Step 3): The core-shell composite nanofiber obtained in step 2) was placed in a 120 °C vacuum oven to remove organic solvents and moisture, and then heated from 30 °C to 200 °C at a rate of 5 °C / min for 1 h in an argon atmosphere, and then heated to 320 °C for 1 h to achieve thermal imidization, and then heated to 450 °C for 1 h to remove the core layer polymethyl methacrylate template, and finally cooled naturally to obtain a polyimide thermal insulation nanofiber with a hollow structure, a cavity diameter of 562 nm, and a thermal conductivity of 0.0206 W·m -1 ·K -1 .
[0033] Example 2 Step 1): First, 10.8 g of p-phenylenediamine was dissolved in a N, N-dimethylacetamide solution with a mass three times the total mass of the monomers, argon was introduced, and the mixture was stirred in a water bath at 10 °C under mechanical stirring at 250 r / min until completely dissolved. 38.7 g of 4, 4′-biphenyl ether dianhydride was added in batches in 6 times, keeping the molar ratio of dianhydride to diamine at 0.8, with an interval of 15 min each time. After the addition was completed, stirring was continued for 6 h to obtain a transparent viscous electrospinning shell solution with a solid content of 20%, which was refrigerated for later use; then 10 g of thermoplastic polyurethane was dissolved in 20 g of N, N-dimethylformamide and 20 g of tetrahydrofuran at room temperature to obtain an electrospinning core solution, which was refrigerated for later use.
[0034] Step 2): The shell layer solution and the core layer solution obtained in step 1) were subjected to vacuum degassing treatment at 25 °C, and then connected to the 18 / 25G coaxial spinning needle of the electrospinning machine using a hose and spun continuously for 8 h to form composite nanofibers with a core-shell structure. The spinning voltage was 10 kV, the distance between the needle and the receiving platform was 10 cm, the shell layer push rate was 0.18 mL / h, the core layer push rate was 0.42 mL / h, and the spinning temperature was 25 °C.
[0035] Step 3): The core-shell composite nanofibers obtained in step 2) were placed in a 120 °C vacuum oven to remove the remaining organic solvent and moisture, and then heated from 30 °C to 230 °C at a rate of 5 °C / min in an argon atmosphere for 0.5 h, and then heated to 340 °C for 1 h to achieve thermal imidization, and then heated to 500 °C for 0.5 h to remove the core layer thermoplastic polyurethane template, and finally cooled naturally to obtain a bamboo-shaped polyimide thermal insulation nanofiber with a cavity diameter of 423 nm and a thermal conductivity of 0.0213 W·m -1 ·K -1 .
[0036] Example 3 Step 1): First, 14.8 g of 1H-benzimidazole-1,2-diamine was dissolved in a mixed solution of N,N-dimethylformamide / toluene with a mass twice the total mass of the monomers, argon was introduced, and the mixture was stirred in a water bath at 5 °C under mechanical stirring at 400 r / min until completely dissolved. 24.4 g of 3,3',4,4'-biphenyltetracarboxylic anhydride was added in batches in 5 times, keeping the molar ratio of anhydride to diamine at 1.2, with an interval of 20 min each time. After the addition was completed, stirring was continued for 4 h to obtain a transparent and viscous electrospinning shell solution with a solid content of 20%, which was refrigerated for standby use; then 33.2 g of polyvinyl pyrrolidone was dissolved in 76.9 g of N,N-dimethylformamide at room temperature to obtain an electrospinning core solution, which was refrigerated for standby use.
[0037] Step 2): The shell solution and the core solution obtained in step 1) were mixed in equal mass to form a blended spinning solution, vacuum degassing was performed at 20 °C, and then a hose was used to connect the 21G spinning needle of the electrospinning machine and continuously spun for 8 h to form a composite nanofiber with a core-shell structure. The spinning voltage was 18 kV, the distance between the needle and the receiving platform was 15 cm, the pushing rate was 0.25 mL / h, and the spinning temperature was 40 °C.
[0038] Step 3): The core-shell composite nanofibers obtained in step 2) are placed in a 120 °C vacuum oven to remove the remaining organic solvent and moisture, and then heated from 30 °C to 150 °C at a rate of 10 °C / min for 2 hours in an argon atmosphere, and then heated to 350 °C for 2 hours to achieve thermal imidization, and then heated to 400 °C for 0.5 hours to remove the core layer polyvinyl pyrrolidone template, and finally cooled naturally to obtain a polyimide thermal insulation nanofiber with a mesoporous cavity structure and a cavity diameter of 45 nm. The mesoporous structure achieves higher thermal insulation efficiency through dense small channels, and has better mechanical properties and a wider range of applications. The mesoporous structure has a higher porosity, which means more air and less solid material, thereby reducing the overall thermal conductivity, and the thermal conductivity coefficient is 0.0261 W·m -1 ·K -1 .
[0039] Example 4 Step 1): First, 14.8 g of 1H-benzimidazole-1,2-diamine was dissolved in N,N-dimethylformamide / tetrahydrofuran solution with a mass of 3 times the total mass of the monomers, argon was introduced, and the mixture was stirred in a water bath at 0 ° C under mechanical stirring at 200 r / min until completely dissolved. 31.2 g of 4,4′-biphenyl ether dianhydride was added in batches in 5 times to keep the molar ratio of dianhydride to diamine at 1, with an interval of 10 min each time. After the addition was completed, stirring was continued for 3 h to obtain a transparent viscous electrospinning shell solution with a solid content of 18%, which was refrigerated for standby use; then 12 g of polymethyl methacrylate was dissolved in 28 g of N,N-dimethylformamide at room temperature to obtain an electrospinning core solution, which was refrigerated for standby use.
[0040] Step 2): The shell layer solution and the core layer solution obtained in step 1) were subjected to vacuum degassing at 30 °C, and then connected to the 18 / 25G coaxial spinning needle of the electrospinning machine using a hose and spun continuously for 8 h to form composite nanofibers with a core-shell structure. The spinning voltage was 25 kV, the distance between the needle and the receiving platform was 5 cm, the shell layer push rate was 0.33 mL / h, the core layer push rate was 0.75 mL / h, and the spinning temperature was 50 °C.
[0041] Step 3): The core-shell composite nanofiber obtained in step 2) was placed in a 120 °C vacuum oven to remove the remaining organic solvent and moisture, and then heated from 30 °C to 200 °C at a rate of 10 °C / min in an argon atmosphere for 1 h, and then heated to 280 °C for 0.5 h to achieve thermal imidization, and then heated to 450 °C for 2 h to remove the core layer polymethyl methacrylate template, and finally cooled naturally to obtain a polyimide thermal insulation nanofiber with a hollow structure, a cavity diameter of 703 nm, and a thermal conductivity of 0.0239 W·m -1 ·K -1 .
[0042] Example 5 Step 1): First, 14.8 g of 1H-benzimidazole-1,2-diamine was dissolved in N,N-dimethylformamide solution with a mass three times the total mass of the monomers, argon was introduced, and the mixture was stirred in a water bath at 0 °C under mechanical stirring at 500 r / min until completely dissolved. 31.2 g of 4,4′-biphenyl ether dianhydride was added in batches in 5 times to keep the molar ratio of dianhydride to diamine at 1, with an interval of 10 min each time. After the addition was completed, stirring was continued for 3 h to obtain a transparent viscous electrospinning shell solution with a solid content of 18%, which was refrigerated for later use; then 12 g of polymethyl methacrylate was dissolved in 28 g of N,N-dimethylformamide at room temperature to obtain an electrospinning core solution, which was refrigerated for later use.
[0043] Step 2): The shell solution and core solution obtained in step 1) were subjected to vacuum degassing at 30 °C, and then connected to the 18 / 25G coaxial spinning needle of the electrospinning machine using a hose and spun continuously for 8 h to form composite nanofibers with a core-shell structure. The spinning voltage was 25 kV, the distance between the needle and the receiving platform was 5 cm, the shell layer push rate was 0.05 mL / h, the core layer push rate was 1.2 mL / h, and the spinning temperature was 20 °C.
[0044] Step 3): The core-shell composite nanofiber obtained in step 2) was placed in a 120 °C vacuum oven to remove the remaining organic solvent and moisture, and then heated from 30 °C to 200 °C at a rate of 10 °C / min in an argon atmosphere for 1 h, and then heated to 280 °C for 0.5 h to achieve thermal imidization, and then heated to 450 °C for 2 h to remove the core layer polymethyl methacrylate template, and finally cooled naturally to obtain a polyimide thermal insulation nanofiber with a hollow structure, a cavity diameter of 385 nm, and a thermal conductivity of 0.0238 W·m -1 ·K -1 .
[0045] The scanning image of the polyimide heat insulation nanofiber with controllable cavity structure obtained by the preparation method of the present invention is as follows: Figure 1 As shown, the fiber morphology is very uniform with an ultra-high aspect ratio, and after random stacking, a nanofiber network fully filled with air is formed between the fibers.
[0046] Figures 2 to 4 This is a transmission image of multiple cavity-structured polyimide nanofibers, which confirms the existence of the cavity structure inside the polyimide nanofibers and the scalability of this strategy. The maximum cavity diameter can reach about 703 nm. Figure 2 The hollow-shaped polyimide nanofiber is prepared. Figure 3 The polyimide nanofiber with bamboo-like cavity structure is prepared. Figure 4 The prepared nanofibers have a mesoporous cavity structure.
[0047] Figure 5 The contact angle image of the polyimide thermal insulation nanofiber with controllable cavity structure is shown. The water contact angle can reach 141°, and the material has certain hydrophobic properties. Figure 6 It can be seen that compared with the intrinsic thermal conductivity of polyimide, the design of nanofibers and controllable cavity structure gives the sample prepared by the present invention an ultra-low thermal conductivity of 0.020~0.025 W·m lower than static air. -1 ·K -1 , with excellent thermal insulation performance. Figure 7 and Figure 8 The thermal insulation performance of the polyimide thermal insulation nanofiber with controllable cavity structure is more intuitively demonstrated. The infrared thermal imaging photos show that there is an obvious color difference between the upper surface of the polyimide nanofiber and the heat source. Figure 7 The infrared thermal imaging image shows that the thermal insulation temperature of the nanofiber is as low as 156 degrees at 300 degrees, indicating that polyimide nanofiber still has excellent high-temperature thermal insulation effect under extreme temperatures; Figure 8 This is an infrared thermal imaging image of the nanofibers with a thermal insulation temperature of 7.2 degrees at -70 degrees, indicating that polyimide nanofibers still have excellent low-temperature thermal insulation effects at extreme temperatures.
[0048] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing polyimide heat-insulating nanofibers with controllable cavity structure, characterized in that: The following steps are involved: 1) dissolving dianhydride and diamine monomers in an organic solvent to prepare an electrospinning shell layer solution; dissolving a template substance in an organic solvent to prepare an electrospinning core layer solution; wherein the template substance is one of polymethyl methacrylate, thermoplastic polyurethane or polyvinyl pyrrolidone; 2) Using coaxial electrospinning technology, the electrospinning shell solution and the core solution are stretched under high voltage to obtain composite nanofibers with a core-shell structure; wherein the spinning voltage is 10-25 kV, the distance between the needle and the receiving platform is 5-15 cm, the pushing rate is 0.05-1.2 mL / h, and the spinning temperature is 20-50°C; 3) The composite nanofibers with a core-shell structure are calcined in a stepwise manner under an inert gas atmosphere to obtain polyimide thermal insulation nanofibers with a controllable cavity structure.
2. The method for preparing the polyimide heat-insulating nanofiber with controllable cavity structure according to claim 1, characterized in that: In step 1), the molar ratio of dianhydride to diamine monomer is 0.8-1.
2.
3. The method for preparing the polyimide heat-insulating nanofiber with controllable cavity structure according to claim 1, characterized in that: In step 1), the dianhydride monomer is one of 4,4'-biphenyl ether dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride or pyromellitic acid anhydride, and the diamine monomer is one of p-phenylenediamine, 4,4'-diaminodiphenyl ether or 1H-benzimidazole-1,2-diamine.
4. The method for preparing the polyimide heat-insulating nanofiber with controllable cavity structure according to claim 1, characterized in that: In step 1), the mass of the organic solvent is 2-4 times the total mass of the monomers, and the organic solvent is one or two of N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylformamide / toluene or N,N-dimethylformamide / tetrahydrofuran.
5. The method for preparing the polyimide heat-insulating nanofiber with controllable cavity structure according to claim 1, characterized in that: In step 1), the mixed solution of dianhydride and diamine monomers and organic solvent is fully reacted in a water bath at 0-10°C for 3-6 hours at a mechanical stirring rate of 200-500 r / min to obtain a light yellow transparent viscous electrospinning shell solution.
6. The method for preparing the polyimide heat-insulating nanofiber with controllable cavity structure according to claim 1, characterized in that: In step 2), the electrospinning shell layer solution and the core layer solution are subjected to vacuum degassing treatment at 20-30°C, and then the electrospinning shell layer solution and the core layer solution are stretched by coaxial electrospinning technology.
7. The method for preparing the polyimide heat-insulating nanofiber with controllable cavity structure according to claim 1, characterized in that: In step 3), the step-by-step temperature calcination is as follows: in an inert gas atmosphere, the temperature is first increased from 30°C to 150~230°C at a rate of 5~10°C / min and kept for 0.5~2h, then increased to 280~350°C and kept for 0.5~2h, then increased to 400~500°C and kept for 0.5~2h, and finally cooled naturally.
8. The polyimide heat-insulating nanofiber with a controlled cavity structure obtained by the method for preparing the polyimide heat-insulating nanofiber with a controlled cavity structure according to any one of claims 1 to 7, characterized in that: The polyimide thermal insulation nanofiber has a cavity structure inside, and the cavity diameter is 45nm-703nm.
9. The polyimide heat-insulating nanofiber with controllable cavity structure according to claim 8, characterized in that: The thermal insulation and heat preservation polyimide nanofibers have a temperature tolerance of -70~300°C and a thermal conductivity of 0.020~0.0261 W·m -1 ·K -1 ; Porosity is 97.8~99.2%, and volume density is 0.020~0.035 g / cm 3 , the water contact angle is 140°~145°.
10. Use of the polyimide thermal insulation nanofiber with controlled cavity structure as claimed in any one of claims 8 to 9 in thermal insulation materials.
Citation Information
Patent Citations
A coaxial electrospun polyimide micro / nano hollow structure material and its preparation method
CN106498558B
Method for preparing SiOC ceramic fiber with hollow porous structure through coaxial electrospinning
CN105256406A
Coaxial electrospun polyimide micro / nano hollow structure material and preparation method thereof
CN106498558A
Preparation method of hollow polyimide fiber
CN109972227A
Preparation method of polyimide micro / nano ribbon-like fiber
CN110004518A
Cited By
Polyetherimide / polyurethane fiber sponge as well as preparation method and application thereof
CN119900107A