High-voltage sandwich-structured gel polymer electrolyte, and preparation method and application thereof
By using a combination of polylactic acid and polycaprolactone fibrous membranes and hydroxyapatite dielectric layers in gel electrolytes, the problem of poor electrochemical stability at high voltages is solved, and high energy density and degradability are achieved. Meet environmental protection requirements.
Patent Information
- Application Number
- CN202411289445.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-03
AI Technical Summary
The existing gel electrolytes have poor electrochemical stability at high voltages, and the materials used during the preparation process are non-renewable, resulting in limited carbon emissions and energy density improvements.
Polylactic acid (PLA) and polycaprolactone (PCL) are used as fibrous membrane materials, and porous structure is constructed with N,N'-methylene bisacrylamide crosslinking agent, and hydroxyapatite (HAP) is encapsulated on the outside. The nanoparticles form an ultra-thin dielectric layer, which improves the liquid retention rate and high voltage stability of the electrolyte.
It has achieved the improvement of electrochemical performance at high voltage, enhanced the degradability and environmental protection of gel polymer electrolytes, expanded the application scenarios, conformed to the concept of green environmental protection, and provided support for sustainable development.
Smart Images

Figure CN119069265A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer, gel electrolyte, supercapacitor and electrochemical technology, and specifically relates to a high-voltage "sandwich" structure gel polymer electrolyte, a preparation method and application thereof. Background Art
[0002] Gel polymer electrolytes (GPEs) not only satisfy the advantages of high safety and deformability but also are expected to obtain more superior electrochemical performance, and are a promising alternative to liquid electrolytes in portable and wearable device applications.
[0003] A good gel polymer electrolyte requires that the polymer matrix can store sufficient electrolyte and have excellent liquid retention rate to ensure electrochemical stability under large current and long cycle. Therefore, the selection of polymer materials and the design of electrolyte matrix structure are particularly important.
[0004] Commonly used polymer materials for preparing gel matrix, such as polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene oxide (PEO), and polyacrylonitrile (PAN), are mostly extracted from fossil fuels. As non-renewable resources, their preparation and degradation have caused a lot of carbon emissions. In addition, their low liquid retention rate and low electrochemical stability at high voltage also hinder the effective improvement of the energy density of quasi-solid-state supercapacitors.
[0005] The patent application document with publication number CN114496589A discloses a porous gel electrolyte and its preparation method and application. After adding polylactic acid (PLA) and polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) to dichloromethane (DCM) and N,N-dimethylformamide (DMF) respectively and mixing them evenly, the obtained A solution and B solution are mixed and stirred evenly, and then coated on the PTFE membrane with a scraper, and the solvent is evaporated to form a porous polymer gel electrolyte membrane. However, due to the low voltage window of the gel electrolyte membrane, it is not suitable for supercapacitors under high voltage. The internal electrolyte volatilization is easy to occur in the supercapacitors circulating under high voltage, which affects the stability of the supercapacitor. Summary of the invention
[0006] In order to overcome the deficiencies in the above-mentioned prior art, the purpose of the present invention is to provide a high-voltage "sandwich" structure gel polymer electrolyte, a preparation method and its application, using degradable materials polylactic acid (PLA) and polycaprolactone (PCL) as the internal fibrous membrane, and using N,N'-methylenebisacrylamide (MBA) cross-linking agent to construct a porous structure inside the fibrous membrane, thereby increasing the surface area of the electrolyte fibrous membrane, which is conducive to storing more electrolyte, and using polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) to wrap hydroxyapatite (HAP) nanoparticles to construct an ultra-thin dielectric layer on both sides of the outside, which can not only slow down the volatilization and loss of the electrolyte, but also the presence of the dielectric layer can slow down the polarization degree of the electrolyte under high voltage.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A high voltage "sandwich" structure gel polymer electrolyte includes a fibrous membrane obtained by electrospinning polylactic acid (PLA) and polycaprolactone (PCL), and a dielectric layer structure formed by hydrolyzed inorganic nanomaterial hydroxyapatite (HAP) wrapped by polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) on both sides of the fibrous membrane.
[0009] A method for preparing a high voltage "sandwich" structure gel polymer electrolyte comprises the following steps:
[0010] S1. Hydrolyze and modify the inorganic nanomaterial hydroxyapatite (HAP) by coupling agent KH550 to obtain the inorganic nanomaterial hydroxyapatite (HAP) hydrolyzed and modified by coupling agent KH550, add the inorganic nanomaterial hydroxyapatite (HAP) hydrolyzed and modified by coupling agent KH550 into dichloromethane (DCM), disperse it ultrasonically in a water bath, add polylactic acid (PLA) after being evenly dispersed, stir it magnetically, add polycaprolactone (PCL) after the polylactic acid (PLA) is completely dissolved, stir it magnetically, and finally add N,N-dimethylformamide (DMF) and continue stirring until the solution is evenly mixed to obtain a mixed solution A;
[0011] S2, electrospinning the mixed solution A obtained in step S1 to obtain a sample, and drying the sample in a vacuum oven to obtain a fibrous membrane;
[0012] S3, adding a certain amount of inorganic nanomaterial hydroxyapatite (HAP) modified by coupling agent KH550 hydrolysis to an acetone solution, ultrasonically dispersing in a water bath, adding polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) after uniform dispersion, magnetically stirring, adding appropriate amounts of bisbenzoylphenylphosphine oxide (CIBA) photoinitiator and N,N'-methylenebisacrylamide (MBA) crosslinking agent in a light-proof environment, and continuing to stir, after uniform stirring, a mixed solution B is obtained;
[0013] S4, soaking the fibrous membrane obtained in step S2 in the mixed solution B obtained in step S3, taking it out, and finally drying it to obtain a composite polymer membrane;
[0014] S5, soaking the composite polymer membrane prepared in step S4 in an organic electrolyte, taking it out after soaking for 1-1.5 hours, to obtain a gel polymer electrolyte.
[0015] In the step S1, the total solid content of polylactic acid (PLA) and polycaprolactone (PCL) is 15wt% to 18wt%, and the mass ratio is polylactic acid (PLA): polycaprolactone (PCL) = (2 to 1): 1; the solid content of the inorganic nanomaterial hydroxyapatite (HAP) modified by hydrolysis of the coupling agent KH550 is 1wt% to 3wt%; and the mass ratio is dichloromethane (DCM): N,N-dimethylformamide (DMF) = (4 to 1): 1.
[0016] In the step S1, the water bath temperature is 0-10°C, the ultrasonic dispersion treatment is performed for 15-30 minutes, and the speed of the magnetic stirring treatment is 300-400 rpm.
[0017] In step S2, the temperature of the vacuum oven is 60-80° C., and the drying time is 12-15 hours.
[0018] In the step S2, the voltage of the electrospinning is 15-20 kV, the distance between the spinning needle and the receiving drum is 15-18 cm, the rotation speed of the receiving drum is 900-1300 r / min, the time is 6-10 h, and the pushing speed is 0.5-1 mL / h.
[0019] In the step S3, by mass ratio: the solid content of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) is 2.5wt% to 10wt%; the content of the inorganic nanomaterial hydroxyapatite (HAP) modified by hydrolysis of the coupling agent KH550 is 5% to 10% of the mass of the polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP); the photoinitiator CIBA and the cross-linking agent MBA are both 10% to 20% of the mass of the inorganic nanomaterial hydroxyapatite (HAP) modified by hydrolysis of the coupling agent KH550.
[0020] In step S3, the water bath temperature is 0-10° C., the ultrasonic dispersion is performed for 15-30 min, and the speed of the magnetic stirring treatment is 300-400 rpm.
[0021] The step S4 is specifically as follows:
[0022] The fibrous membrane obtained in step S2 is soaked in the mixed solution B obtained in step S3 for 3 to 5 seconds, then taken out and UV-cured for cross-linking. The light curing time is 2 to 3 minutes, and the light power is 50 to 75%. Finally, it is placed in a vacuum oven at 60 to 80° C. for 12 to 15 hours to volatilize the residual acetone solution to obtain a composite polymer membrane.
[0023] The organic electrolyte of step 5 includes but is not limited to acetonitrile (AN)-based, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC) or ethyl methyl carbonate (EMC)-based.
[0024] An application of a high-voltage "sandwich" structure gel polymer electrolyte is used to assemble a supercapacitor with the gel polymer electrolyte prepared above. The supercapacitor includes a button type, a cylindrical type or a soft package type.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The gel polymer electrolyte prepared by the present invention is mostly made of degradable materials. Materials such as polylactic acid (PLA) and polycaprolactone (PCL) have good biocompatibility and degradability, and can be degraded into harmless substances after use, meeting environmental protection requirements. In addition, the addition of inorganic nanomaterial hydroxyapatite (HAP) modified by coupling agent KH550 hydrolysis as a regenerated material enhances the electrochemical performance of the gel polymer electrolyte at high voltage. At the same time, the construction of the dielectric layer increases the specific capacitance, so the energy density is also improved. These characteristics not only expand the application scenarios of the gel polymer electrolyte, but also comply with the green environmental protection concept advocated by the country, and contribute to sustainable development.
[0027] (2) In the present invention, the hydrolyzed HAP coated with polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) is used as a dielectric modification layer, which can achieve the stable existence of polylactic acid (PLA) and polycaprolactone (PCL) based electrolytes in high voltage acetonitrile (AN) based electrolytes.
[0028] (3) The PLA of the present invention has good filament forming properties, is suitable for electrospinning, and has shape memory function. PCL, as one of the commonly used linear aliphatic semi-crystalline polyesters, has a low melting temperature and phase transition temperature. It also shows great potential in suppressing the crystallinity of the polymer matrix and manufacturing shape memory electrolytes under mild stimulation, and can achieve perfect fit with electrodes under different bending conditions. The fibrous structure obtained by electrospinning is conducive to the migration of electrolytes under electric fields, and the nanomaterial hydroxyapatite (HAP) treated with coupling agent 3-aminopropyltriethoxysilane (KH550) has better dispersibility. It is evenly dispersed in the PVDF-HFP solution. The dielectric layer constructed on both sides of the fibrous membrane can not only improve the stability of the electrolyte membrane under high voltage, but also the polarization effect of the high dielectric dielectric layer can improve the specific capacitance, thereby improving the energy density of the supercapacitor.
[0029] (4) The present invention uses commercially available renewable polymers polylactic acid (PLA) and polycaprolactone (PCL) that can be used for large-scale production to produce a polymer matrix through electrospinning. The polymer matrix is not only environmentally friendly and has shape memory characteristics, but also has lower crystallinity and wider electrochemical window of polycaprolactone (PCL) and better film-forming property and higher thermal stability of polylactic acid (PLA), which can ensure the excellent electrochemical performance of the gel polymer electrolyte at high voltage.
[0030] (5) The gel polymer electrolyte prepared by the traditional casting method has a low liquid retention rate. At the same time, its large interface impedance significantly reduces the rate performance of the supercapacitor. The sandwich structure polymer matrix designed by the present invention can effectively alleviate the above problems. It uses degradable materials polylactic acid (PLA) and polycaprolactone (PCL) as the internal fiber skeleton, which can absorb sufficient electrolyte. At the same time, polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) is used to wrap hydroxyapatite (HAP) nanoparticles on both sides of the outside to construct ultra-thin dielectric layers on both sides. The outer ultra-thin dielectric polymer film can slow down the volatilization and loss of the electrolyte and improve the liquid retention rate. In addition, the ultra-thin dielectric layer can slow down the polarization of the electrolyte at high voltage and the failure phenomenon of inorganic salts, improve the stability of the gel polymer electrolyte at high voltage, and the assembled supercapacitor can show excellent electrochemical performance at high voltage.
[0031] (6) The main materials used in the present invention, polylactic acid (PLA) and polycaprolactone (PCL), are both biodegradable materials that can be degraded into harmless substances after use, meeting environmental protection requirements. Secondly, the internal skeleton adopts electrostatic spinning to obtain a fibrous structure with a large porosity, which is beneficial to the rate performance of the supercapacitor; at the same time, adding ultra-thin dielectric layers on both sides of the internal skeleton can not only enable the supercapacitor to work normally under high voltage, but also slow down the volatilization of the electrolyte inside the gel electrolyte, thereby improving the stability of the supercapacitor under high voltage.
[0032] In summary, the present invention has a simple design, a pollution-free preparation process, no high temperature is required, and the process is safe. The use of environmentally friendly materials achieves high electrolyte absorption and high voltage stability and a bendable electrolyte, which provides feasibility for the widespread application of quasi-solid-state supercapacitors, complies with the country's advocacy of green environmental protection concepts, and contributes to sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is the infrared spectrum result of the composite polymer film of Example 1 of the present invention.
[0034] Figure 2 This is a graph showing the thermogravimetric results of the composite polymer film of Example 1 of the present invention.
[0035] Figure 3 This is a scanning electron microscope image (SEM image) of the composite polymer film of Example 1 of the present invention; wherein, Figure 3 (a) is the sample plane diagram, Figure 3 (b) is the cross-sectional view of the sample.
[0036] Figure 4 This is an electrochemical impedance spectroscopy (EIS) diagram of the gel polymer electrolyte in Example 1 of the present invention in a button-type supercapacitor.
[0037] Figure 5 This is a charge and discharge curve diagram of the gel polymer electrolyte in Example 1 of the present invention in a button-type supercapacitor.
[0038] Figure 6 This is a rate performance diagram of the gel polymer electrolyte in a button-type supercapacitor according to Example 1 of the present invention.
[0039] Figure 7 This is a graph showing the cycling performance of the gel polymer electrolyte in a button-type supercapacitor according to Example 1 of the present invention.
[0040] Figure 8 This is an optical display diagram of the sample in Example 1 of the present invention. DETAILED DESCRIPTION
[0041] The technical solution adopted by the present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0042] The present invention proposes a design concept of the above-mentioned gel polymer electrolyte, wherein the hydroxyapatite (HAP) nanoparticles modified by hydrolysis of the coupling agent 3-aminopropyltriethoxysilane (KH550) coated with polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) are evenly distributed on both sides of the polylactic acid (PLA) / polycaprolactone (PCL) fiber skeleton as a dielectric layer to form a "sandwich" structure. The dielectric layer, as an important component of the surface layer of the gel polymer electrolyte, bears the functions of insulation and separation of electrodes, slowing down the polarization of electrolyte solvents and inorganic salts at high voltages and the failure of inorganic salt molecules, and improving the stability of the electrolyte at high voltages. Through reasonable material selection and structural design, this gel polymer electrolyte can provide a good ion transmission channel while improving the high voltage resistance of the electrolyte through the dielectric layer, thereby ensuring the stable operation of the supercapacitor under high voltage conditions.
[0043] The gel polymer electrolyte can exist stably in acetonitrile-based electrolytes, and can be assembled into button-type and flexible quasi-solid-state supercapacitors, which exhibit stable electrochemical properties under high voltage.
[0044] The present invention provides a high-voltage "sandwich" structure gel polymer electrolyte, comprising a fibrous membrane obtained by electrospinning polylactic acid (PLA) and polycaprolactone (PCL), and a dielectric layer structure formed by polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) wrapping hydrolyzed inorganic nanomaterial hydroxyapatite (HAP) on both sides of the fibrous membrane. The polarization phenomenon of the dielectric layer under high voltage can protect the internal electrolyte, prevent the electrolyte from volatilizing and slow down the occurrence of side reactions.
[0045] A method for preparing a high-voltage "sandwich" structure gel polymer electrolyte, wherein the composite "sandwich" structure gel polymer electrolyte with ultra-thin dielectric layers on both sides can operate stably under high voltage, and the ultra-thin dielectric layer can slow down the polarization of the electrolyte under high voltage, comprising the following steps:
[0046] S1. Hydrolyze and modify the inorganic nanomaterial hydroxyapatite (HAP) by coupling agent KH550 to obtain the inorganic nanomaterial hydroxyapatite (HAP) hydrolyzed and modified by coupling agent KH550. Add the inorganic nanomaterial hydroxyapatite (HAP) hydrolyzed and modified by coupling agent KH550 into dichloromethane (DCM), and ultrasonically disperse it in a water bath at 0-10°C for 15-30 minutes. After being evenly dispersed, add polylactic acid (PLA) and stir it magnetically at a speed of 300-400rpm. After the polylactic acid (PLA) is completely dissolved, add polycaprolactone (PCL) and stir it magnetically at a speed of 300-400rpm. Finally, add N,N-dimethylformamide (DMF) and continue stirring until the solution is evenly mixed to obtain a mixed solution A.
[0047] In the step S1, the total solid content of polylactic acid (PLA) and polycaprolactone (PCL) is 15wt% to 18wt%, and the mass ratio of polylactic acid (PLA): polycaprolactone (PCL) is 1:1; the solid content of the inorganic nanomaterial hydroxyapatite (HAP) hydrolyzed and modified by coupling agent KH550 is 1wt% to 3wt%; and the mass ratio of dichloromethane (DCM): N,N-dimethylformamide (DMF) is 2:1;
[0048] The present invention uses renewable materials PLA and PCL as electrolyte matrices or diaphragms. PCL has a wide electrochemical window, and both are widely available, green and environmentally friendly, and have been commercialized at a low price.
[0049] S2. The mixed solution A obtained in step S1 is subjected to electrospinning for 6-10 h. The electrospinning voltage is 15-20 kV, the distance between the spinning needle and the receiving drum is 15-18 cm, the rotation speed of the receiving drum is 900-1300 r / min, the pushing speed is 0.5-1 mL / h, and the obtained sample is dried in a vacuum oven at 60-80°C for 12-15 h to obtain a fibrous membrane.
[0050] S3, adding a certain amount of inorganic nanomaterial hydroxyapatite (HAP) modified by coupling agent KH550 hydrolysis to an acetone solution, ultrasonically dispersing in a water bath at 0-10°C for 15-30 minutes, adding polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and magnetically stirring after uniform dispersion, the speed of magnetic stirring treatment is 300-400rpm, adding appropriate amount of bisbenzoylphenylphosphine oxide (CIBA) photoinitiator and N,N'-methylenebisacrylamide (MBA) crosslinking agent in a light-proof environment, and continuing to stir, after uniform stirring, a mixed solution B is obtained;
[0051] In the step S3, by mass ratio: the solid content of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) is 2.5wt% to 10wt%; the content of inorganic nanomaterial hydroxyapatite (HAP) modified by hydrolysis of coupling agent KH550 is 5% to 10% of the mass of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP); the photoinitiator CIBA and the crosslinking agent MBA are both 10% to 20% of the mass of inorganic nanomaterial hydroxyapatite (HAP) modified by hydrolysis of coupling agent KH550;
[0052] The polymer PVDF-HFP has good film-forming property, can wrap HAP on the surface of the cellulose skeleton to form an ultra-thin dielectric layer with uniform HAP distribution, and can slow down the volatilization of electrolyte inside the fiber skeleton.
[0053] S4, taking out the fibrous membrane obtained in step S2, soaking it in the mixed solution B obtained in step S3 for 3-5 seconds, taking it out, and performing UV curing and cross-linking, the light curing time is 2-3 minutes, the light power is 50-75%, and finally standing in a vacuum oven at 60-80°C for 12-15 hours to volatilize the residual acetone solution, to obtain a composite polymer membrane;
[0054] The invention adds nano-HAP to enhance the toughness of the fiber skeleton formed by spinning. The HAP nanoparticles are grafted on the electrolyte surface as a stabilizer and catalyst under the action of ultraviolet light to form an ultrathin dielectric layer to improve the stability of GEP under high voltage. MBA is used as a cross-linking agent to participate in constructing the porous structure on the fiber skeleton surface, which can increase the specific surface area of the polymer matrix and absorb more electrolyte.
[0055] S5, soaking the composite polymer membrane prepared in step S4 in an acetonitrile (AN)-based organic electrolyte, taking it out after soaking for 1-1.5 hours, to obtain a gel polymer electrolyte.
[0056] An application of a high-voltage "sandwich" structure gel polymer electrolyte is used to assemble a supercapacitor with the gel polymer electrolyte prepared above. The supercapacitor includes a button type, a cylindrical type or a soft package type, and the soft package can be flexible and bendable.
[0057] The present invention proposes a supercapacitor having the above-mentioned gel polymer electrolyte. The high electrolyte absorption rate and liquid retention rate of the gel polymer electrolyte and the protection of the dielectric layer ensure that the supercapacitor using the electrolyte has excellent electrochemical performance at high voltage.
[0058] The polylactic acid (PLA) and polycaprolactone (PCL) of the present invention are both biodegradable materials. At the same time, PLA is easy to filament and suitable for electrostatic spinning. PCL has a wide electrochemical window and has poor mechanical properties when used alone, but can show good mechanical properties when used in combination with PLA. Therefore, a mixed solution of the two is selected for electrostatic spinning. In order to achieve better spinning effect, the total solid content of the two in the solution should not be too high or too low. If the content is too low, the filaments are too thin, and if it is too high, it is not easy to filament. Therefore, the solid content is preferably 15wt% to 18wt%, and the ratio of the two is 1:1 to achieve the best effect; hydroxyapatite (HAP) has a higher dielectric constant, lower dielectric loss and high biocompatibility, so adding a small amount of HAP during the spinning process can achieve the effect of increasing the mechanical properties and dielectric properties of the spinning membrane, but the content should not be too high and cannot affect the spinning effect. It is best to select 1% to 3% of the sum of the mass of all solutes and the solution; polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) wraps HAP as a dielectric layer, and the thickness of the dielectric layer will affect the electrolysis The migration of ions in the liquid affects the rate performance of the supercapacitor and thus affects the power density. Therefore, if the dielectric layer is to be ultra-thin, the PVDF-HFP content must not be too high. The solid content is preferably selected between 5wt% and 10wt%. If the content is too low, it is not easy to form a film. If the content is too high, the dielectric layer will be thicker. The HAP content as the dielectric layer structure will also affect its rate performance. It is best to be 5% to 10% of PVDF-HFP. If the content is too low, the dielectric constant of the dielectric layer will be lower. If the content is too high, the dispersibility will be affected, and the rate performance of the supercapacitor will be reduced. The content of the photoinitiator CIBA and the cross-linking agent MBA is 10% to 20% of the hydroxyapatite (HAP). If the content is too low, the cross-linking is insufficient. If the content is too high, the electrolyte membrane will become brittle and the mechanical properties will be affected.
[0059] Example 1
[0060] A high-voltage "sandwich" structure gel polymer electrolyte includes a fibrous membrane obtained by electrospinning polylactic acid (PLA) and polycaprolactone (PCL), and a dielectric layer structure formed by polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) wrapping hydrolyzed inorganic nanomaterial hydroxyapatite (HAP) on both sides of the fibrous membrane. The polarization phenomenon of the dielectric layer under high voltage can protect the internal electrolyte, prevent the volatilization of the electrolyte and slow down the occurrence of side reactions.
[0061] A method for preparing a high voltage "sandwich" structure gel polymer electrolyte comprises the following steps:
[0062] S1. Weigh 0.1g of inorganic nanomaterial hydroxyapatite (HAP) modified by coupling agent KH550 hydrolysis, add it to 4.275mL of dichloromethane (DCM) and carry out ultrasonic treatment in a 0℃ water bath for 30min. After being evenly dispersed, add 0.75g of polylactic acid (PLA) and stir magnetically at 400rpm for 1h. After the polylactic acid (PLA) is completely dissolved, add 0.75g of polycaprolactone (PCL) and stir magnetically at 400rpm for 60min. Stir evenly. Finally, add 2.99mL of N,N-dimethylformamide (DMF) and continue to stir magnetically at 400rpm for 1h until the solution is evenly mixed to obtain a mixed solution A.
[0063] S2, pouring the mixed solution A obtained in step S1 into the injection needle tube for electrospinning for 7.5 hours, the voltage of electrospinning is 20 kV, the straight-line distance between the spinning needle and the collection drum is 15 cm, the rotation speed of the collection drum is 1200 r / min, and the pushing speed of the injection needle tube during the process is 1 mL / h. The sample obtained after spinning is placed in a 60°C vacuum oven for drying for 12 hours to volatilize the residual dichloromethane (DCM) and N,N-dimethylformamide (DMF) solvents to obtain a fibrous membrane;
[0064] S3, add 0.005g of the inorganic nanomaterial hydroxyapatite (HAP) treated by hydrolysis of coupling agent 3-aminopropyltriethoxysilane (KH550) to 1.561mL of acetone solution, and ultrasonically disperse it in a water bath at 0°C for 30min, add 0.1g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) after uniform dispersion, and magnetically stir it at 400rmp for 30min. After stirring evenly, add 0.001g of bisbenzoylphenylphosphine oxide (CIBA) photoinitiator and 0.001g of N,N'-methylenebisacrylamide (MBA) crosslinking agent in a light-proof environment, and continue stirring at 400rmp for 30min to obtain a mixed solution B;
[0065] S4, cutting a piece of the fibrous membrane obtained in step S2 into a size of 4×4 cm, lightly immersing it in the mixed solution B obtained in step S3 for 3 seconds in a dark environment, then photocuring it under ultraviolet light for 3 minutes with a light power of 50%, and finally standing it in a vacuum oven at 60° C. for 12 hours to volatilize the residual acetone solution, thereby obtaining a composite polymer membrane;
[0066] S5. The composite polymer membrane obtained in step 4 is named PP@7.5PV-5HA. The prepared composite polymer membrane is punched into a circular electrolyte with a diameter of 14 μm, and is soaked in an acetonitrile (AN)-based organic electrolyte for 1 hour and then taken out to obtain a gel polymer electrolyte.
[0067] An application of a high voltage "sandwich" structure gel polymer electrolyte is used to assemble the gel polymer electrolyte prepared above into a supercapacitor, including button type, cylindrical or soft package type. The soft package type supercapacitor has flexibility and bendability, and the bending shape of the soft package is fixed.
[0068] The electrolyte on the surface of the obtained gel polymer electrolyte was wiped dry and assembled into a button-type quasi-solid-state supercapacitor, and the electrochemical performance was tested.
[0069] Example 2
[0070] A high-voltage "sandwich" structure gel polymer electrolyte includes a fibrous membrane obtained by electrospinning polylactic acid (PLA) and polycaprolactone (PCL), and a dielectric layer structure formed by polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) wrapping hydrolyzed inorganic nanomaterial hydroxyapatite (HAP) on both sides of the fibrous membrane. The polarization phenomenon of the dielectric layer under high voltage can protect the internal electrolyte, prevent the volatilization of the electrolyte and slow down the occurrence of side reactions.
[0071] A method for preparing a high voltage "sandwich" structure gel polymer electrolyte comprises the following steps:
[0072] S1. Weigh 0.1g of inorganic nanomaterial hydroxyapatite (HAP) modified by coupling agent KH550 hydrolysis, add it to 4.275mL of dichloromethane (DCM) and carry out ultrasonic treatment in a 5℃ water bath for 30min. After being evenly dispersed, add 0.75g of polylactic acid (PLA) and stir magnetically at 400rpm for 30min. After the polylactic acid (PLA) is completely dissolved, add 0.75g of polycaprolactone (PCL) and stir magnetically at 400rpm for 1h. Stir evenly. Finally, add 2.99mL of N,N-dimethylformamide (DMF) and continue to stir magnetically at 400rpm for 45min until the solution is evenly mixed to obtain a mixed solution A.
[0073] S2, pouring the mixed solution A obtained in step S1 into an injection needle tube for electrospinning for 8 hours, the voltage of electrospinning is 18 kV, the straight-line distance between the spinning needle and the collection drum is 18 cm, the rotation speed of the collection drum is 1300 r / min, and the pushing speed of the injection needle tube during the process is 1 mL / h; placing the sample obtained after spinning in a 60°C vacuum oven for drying for 15 hours to volatilize the residual dichloromethane (DCM) and N,N-dimethylformamide (DMF) solvents to obtain a fibrous membrane;
[0074] S3, adding 0.005g of the inorganic nanomaterial hydroxyapatite (HAP) treated by hydrolysis of coupling agent 3-aminopropyltriethoxysilane (KH550) to 2.405mL of acetone solution, ultrasonically dispersing in a water bath at 0°C for 20min, adding 0.1g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) after uniform dispersion, magnetically stirring at 400rpm for 40min, adding 0.001g of bisbenzoylphenylphosphine oxide (CIBA) photoinitiator and 0.001g of N,N'-methylenebisacrylamide (MBA) crosslinking agent in a light-proof environment, continuing to stir at 400rpm for 35min to obtain a mixed solution B;
[0075] S4, cutting a piece of the fibrous membrane obtained in step S2 into a size of 4×4 cm, lightly immersing it in the mixed solution B obtained in step S3 for 3 seconds in a dark environment, then photocuring it under ultraviolet light for 3 minutes with a light power of 55%, and finally standing it in a vacuum oven at 60° C. for 12 hours to volatilize the residual acetone solution, thereby obtaining a composite polymer membrane;
[0076] S5. The composite polymer membrane obtained in step 4 is named PP@5PV-5HA. The prepared composite polymer membrane is punched into a circular electrolyte with a diameter of 14 μm, and is taken out after being immersed in an acetonitrile (AN)-based organic electrolyte for 1 hour to obtain a gel polymer electrolyte.
[0077] An application of a high voltage "sandwich" structure gel polymer electrolyte is used to assemble the gel polymer electrolyte prepared above into a supercapacitor, including button type, cylindrical or soft package type. The soft package type supercapacitor has flexibility and bendability, and the bending shape of the soft package is fixed.
[0078] The electrolyte on the surface of the obtained gel polymer electrolyte was wiped dry and assembled into a button-type quasi-solid-state supercapacitor, and the electrochemical performance was tested.
[0079] Example 3
[0080] A high-voltage "sandwich" structure gel polymer electrolyte includes a fibrous membrane obtained by electrospinning polylactic acid (PLA) and polycaprolactone (PCL), and a dielectric layer structure formed by polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) wrapping hydrolyzed inorganic nanomaterial hydroxyapatite (HAP) on both sides of the fibrous membrane. The polarization phenomenon of the dielectric layer under high voltage can protect the internal electrolyte, prevent the volatilization of the electrolyte and slow down the occurrence of side reactions.
[0081] A method for preparing a high voltage "sandwich" structure gel polymer electrolyte comprises the following steps:
[0082] S1. Weigh 0.1g of inorganic nanomaterial hydroxyapatite (HAP) modified by coupling agent KH550 hydrolysis, add it to 5.13mL of dichloromethane (DCM) and carry out ultrasonic treatment in a 0℃ water bath for 20min. After being evenly dispersed, add 1g of polylactic acid (PLA) and stir magnetically at 400rpm for 40min. After the polylactic acid (PLA) is completely dissolved, add 0.5g of polycaprolactone (PCL) and stir magnetically at 400rpm for 1h. Stir evenly. Finally, add 1.79mL of N,N-dimethylformamide (DMF) and continue to stir magnetically at 400rpm for 45min until the solution is evenly mixed to obtain a mixed solution A.
[0083] S2, pouring the mixed solution A obtained in step S1 into an injection needle tube for electrospinning for 7 hours, the voltage of electrospinning is 20 kV, the straight-line distance between the spinning needle and the collection drum is 15 cm, the rotation speed of the collection drum is 1000 r / min, and the pushing speed of the injection needle tube during the process is 0.8 mL / h; placing the sample obtained after spinning in a 60° C. vacuum oven for drying for 15 hours to volatilize the residual dichloromethane (DCM) and N,N-dimethylformamide (DMF) solvents to obtain a fibrous membrane;
[0084] S3, adding 0.005g of the inorganic nanomaterial hydroxyapatite (HAP) treated by hydrolysis of coupling agent 3-aminopropyltriethoxysilane (KH550) to 4.937mL of acetone solution, ultrasonically dispersing in a water bath at 0°C for 25min, adding 0.1g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) after uniform dispersion, magnetically stirring at 400rpm for 1h, stirring evenly, adding 0.001g of bisbenzoylphenylphosphine oxide (CIBA) photoinitiator and 0.001g of N,N'-methylenebisacrylamide (MBA) crosslinking agent in a light-proof environment, continuing to stir at 400rpm for 30min to obtain a mixed solution B;
[0085] S4, cutting a piece of the fibrous membrane obtained in step S2 into a size of 4×4 cm, lightly immersing it in the mixed solution B obtained in step S3 for 4 seconds in a dark environment, then photocuring it under ultraviolet light for 3 minutes with a light power of 50%, and finally standing it in a vacuum oven at 60° C. for 12 hours to volatilize the residual acetone solution, thereby obtaining a composite polymer membrane;
[0086] S5. The composite polymer membrane obtained in step 4 is named PP@2.5PV-5HA. The prepared composite polymer membrane is punched into a circular electrolyte with a diameter of 14 μm, and is soaked in an acetonitrile (AN)-based organic electrolyte for 1 hour and then taken out to obtain a gel polymer electrolyte.
[0087] An application of a high voltage "sandwich" structure gel polymer electrolyte is used to assemble the gel polymer electrolyte prepared above into a supercapacitor, including button type, cylindrical or soft package type. The soft package type supercapacitor has flexibility and bendability, and the bending shape of the soft package is fixed.
[0088] The electrolyte on the surface of the obtained gel polymer electrolyte was wiped dry and assembled into a button-type quasi-solid-state supercapacitor, and the electrochemical performance was tested.
[0089] Example 4
[0090] A high-voltage "sandwich" structure gel polymer electrolyte includes a fibrous membrane obtained by electrospinning polylactic acid (PLA) and polycaprolactone (PCL), and a dielectric layer structure formed by polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) wrapping hydrolyzed inorganic nanomaterial hydroxyapatite (HAP) on both sides of the fibrous membrane. The polarization phenomenon of the dielectric layer under high voltage can protect the internal electrolyte, prevent the volatilization of the electrolyte and slow down the occurrence of side reactions.
[0091] A method for preparing a high voltage "sandwich" structure gel polymer electrolyte comprises the following steps:
[0092] S1. Weigh 0.1g of inorganic nanomaterial hydroxyapatite (HAP) modified by coupling agent KH550 hydrolysis, add it to 2.58mL of dichloromethane (DCM) and carry out ultrasonic treatment in a 0℃ water bath for 30min. After being evenly dispersed, add 1g of polylactic acid (PLA) and stir magnetically at 400rpm for 1h. After the polylactic acid (PLA) is completely dissolved, add 0.5g of polycaprolactone (PCL) and stir magnetically at 400rpm for 1h. Stir evenly. Finally, add 3.6mL of N,N-dimethylformamide (DMF) and continue to stir magnetically at 400rpm for 1h until the solution is evenly mixed to obtain a mixed solution A.
[0093] S2, pouring the mixed solution A obtained in step S1 into the injection needle tube for electrospinning for 6.5 hours, the voltage of the electrospinning is 20 kV, the straight-line distance between the spinning needle and the collection drum is 15 cm, the rotation speed of the collection drum is 1100 r / min, and the pushing speed of the injection needle tube during the process is 1 mL / h; placing the sample obtained after spinning in a 60° C. vacuum oven for drying for 12 hours to volatilize the residual dichloromethane (DCM) and N,N-dimethylformamide (DMF) solvents to obtain a fibrous membrane;
[0094] S3, adding 0.0075g of the inorganic nanomaterial hydroxyapatite (HAP) treated by hydrolysis of coupling agent 3-aminopropyltriethoxysilane (KH550) to 1.561mL of acetone solution, ultrasonically dispersing in a water bath at 0°C for 30min, adding 0.1g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) after uniform dispersion, magnetically stirring at 400rpm for 30min, adding 0.0015g of bisbenzoylphenylphosphine oxide (CIBA) photoinitiator and 0.0015g of N,N'-methylenebisacrylamide (MBA) crosslinking agent in a light-proof environment, continuing to stir at 400rpm for 30min to obtain a mixed solution B;
[0095] S4, cutting a piece of the fibrous membrane obtained in step S2 into a size of 4×4 cm, lightly immersing it in the mixed solution B obtained in step S3 for 3 seconds in a dark environment, then photocuring it under ultraviolet light for 3 minutes with a light power of 70%, and finally standing it in a vacuum oven at 60° C. for 12 hours to volatilize the residual acetone solution, thereby obtaining a composite polymer membrane;
[0096] S5. The composite polymer membrane obtained in step 4 is named PP@7.5PV-7.5HA. The prepared composite polymer membrane is punched into a circular electrolyte with a diameter of 14 μm, and is taken out after being immersed in an acetonitrile (AN)-based organic electrolyte for 1 hour to obtain a gel polymer electrolyte.
[0097] An application of a high voltage "sandwich" structure gel polymer electrolyte is used to assemble the gel polymer electrolyte prepared above into a supercapacitor, including button type, cylindrical or soft package type. The soft package type supercapacitor has flexibility and bendability, and the bending shape of the soft package is fixed.
[0098] The electrolyte on the surface of the obtained gel polymer electrolyte was wiped dry and assembled into a button-type quasi-solid-state supercapacitor, and the electrochemical performance was tested.
[0099] Example 5
[0100] A high-voltage "sandwich" structure gel polymer electrolyte includes a fibrous membrane obtained by electrospinning polylactic acid (PLA) and polycaprolactone (PCL), and a dielectric layer structure formed by polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) wrapping hydrolyzed inorganic nanomaterial hydroxyapatite (HAP) on both sides of the fibrous membrane. The polarization phenomenon of the dielectric layer under high voltage can protect the internal electrolyte, prevent the volatilization of the electrolyte and slow down the occurrence of side reactions.
[0101] A method for preparing a high voltage "sandwich" structure gel polymer electrolyte comprises the following steps:
[0102] S1. Weigh 0.101g of inorganic nanomaterial hydroxyapatite (HAP) modified by coupling agent KH550 hydrolysis, add it to 4.275mL of dichloromethane (DCM) and carry out ultrasonic treatment in a 0℃ water bath for 30min. After being evenly dispersed, add 0.81g of polylactic acid (PLA) and stir magnetically at 400rpm for 1h. After the polylactic acid (PLA) is completely dissolved, add 0.81g of polycaprolactone (PCL) and stir magnetically at 400rpm for 1h. Stir evenly. Finally, add 2.9925mL of N,N-dimethylformamide (DMF) and continue to stir magnetically at 400rpm for 40min until the solution is evenly mixed to obtain a mixed solution A.
[0103] S2, pouring the mixed solution A obtained in step S1 into the injection needle tube for electrospinning for 6 hours, the voltage of electrospinning is 18 kV, the straight-line distance between the spinning needle and the collection drum is 16 cm, the rotation speed of the collection drum is 1300 r / min, and the pushing speed of the injection needle tube during the process is 1 mL / h; placing the sample obtained after spinning in a 60°C vacuum oven for drying for 12 hours to volatilize the residual dichloromethane (DCM) and N,N-dimethylformamide (DMF) solvents to obtain a fibrous membrane;
[0104] S3, adding 0.01g of the inorganic nanomaterial hydroxyapatite (HAP) treated by hydrolysis of coupling agent 3-aminopropyltriethoxysilane (KH550) to 1.561mL of acetone solution, ultrasonically dispersing in a water bath at 10°C for 30min, adding 0.1g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) after uniform dispersion, magnetically stirring at 400rpm for 30min, adding 0.002g of bisbenzoylphenylphosphine oxide (CIBA) photoinitiator and 0.002g of N,N'-methylenebisacrylamide (MBA) crosslinking agent in a light-proof environment, continuing to stir at 400rpm for 30min to obtain a mixed solution B;
[0105] S4, cutting a piece of the fibrous membrane obtained in step S2 into a size of 4×4 cm, lightly immersing it in the mixed solution B obtained in step S3 in a dark environment for 3 seconds, then photocuring it under ultraviolet light for 2 minutes with a light power of 75%, and finally standing it in a vacuum oven at 60° C. for 12 hours to volatilize the residual acetone solution, thereby obtaining a composite polymer membrane;
[0106] S5. The composite polymer membrane obtained in step 4 is named PP@7.5PV-10HA. The prepared composite polymer membrane is punched into a circular electrolyte with a diameter of 14 μm, and is soaked in an acetonitrile (AN)-based organic electrolyte for 1 hour and then taken out to obtain a gel polymer electrolyte.
[0107] An application of a high voltage "sandwich" structure gel polymer electrolyte is used to assemble the gel polymer electrolyte prepared above into a supercapacitor, including button type, cylindrical or soft package type. The soft package type supercapacitor has flexibility and bendability, and the bending shape of the soft package is fixed.
[0108] The electrolyte on the surface of the obtained gel polymer electrolyte was wiped dry and assembled into a button-type quasi-solid-state supercapacitor, and the electrochemical performance was tested.
[0109] Experimental analysis
[0110] The composite material obtained in Example 1 includes PLA, PCL, PVDF-HFP and HAP. Figure 1 Infrared spectroscopy proves the physical compounding of the above materials and the chemical changes after light curing. Figure 1 It can be seen that the consistency of the positions of the characteristic peaks of various key chemical bonds reflects the physical combination, while the displacement of the characteristic peaks and the change of the peak intensity reflect the chemical changes.
[0111] The thermal stability of the composite material obtained in Example 1 is greatly improved after curing, and the degree of decomposition at high temperature is slowed down. Figure 2 Thermogravimetric testing was demonstrated. Figure 2 It can be seen that the decomposition temperature of the PP@7.5PV-5HA sample is 350°C, while that of the PPH sample is 300°C. Moreover, after 600°C, the PPH sample has been completely decomposed, while there is still some residue in the PP@7.5PV-5HA sample, indicating that the thermal stability of the gel electrolyte membrane with the added dielectric layer is improved.
[0112] The optical photograph of the composite material obtained in Example 1 is as follows Figure 3 As shown in the figure, the surface and interface of the composite membrane were observed by SEM, and it was observed that the electrolyte membrane had a good porous structure, and the surface HAP in the PP@7.5PV-0.5HA sample was evenly dispersed. Figure 3 (a) It can be seen that HAP nanoparticles are distributed on the surface fibers of the sample. Figure 3 (b) It can be seen that due to the fluidity of PVDF-HFP solution, an ultra-thin PVDF-HFP film has been distributed on the outside of the fiber.
[0113] The PP@7.5PV-5HA electrolyte in Example 1 was used to assemble a button-type supercapacitor, and the electrochemical impedance spectroscopy (EIS) results were as follows: Figure 4 As shown, the photocured electrolyte membrane optimizes the ion transport resistance at the interface caused by swelling, and can maintain the same interfacial impedance as the current commercial cellulose separator even with the addition of dielectric layers on both sides.
[0114] The PP@7.5PV-5HA electrolyte in Example 1 was used to assemble a button-type supercapacitor, and the charge-discharge curves measured at a high voltage of 3.5 V were as follows: Figure 5 As shown, the electrolyte membrane in the experimental group can present a standard triangle wave at high voltage, proving the stability of charging and discharging at high voltage.
[0115] The PP@7.5PV-5HA electrolyte in Example 1 was used to assemble a button-type supercapacitor, and the rate performance results measured at a high voltage of 3.5V were as follows: Figure 6 As shown, the electrolyte membrane is 25Ag -1 It can still maintain a high capacitance value at a high current density.
[0116] The PP@7.5PV-5HA electrolyte in Example 1 was used to assemble a button-type supercapacitor, and the cycle charge and discharge performance results measured at a high voltage of 3.5V were as follows: Figure 7 As shown, the electrolyte membrane in the experimental group is 1Ag -1 The band content remained at 85.82% after 10,000 cycles at a current density of 2.547 W, demonstrating the stability of the electrochemical performance of the electrolyte.
[0117] like Figure 8 The optical display diagram of the sample in Example 1 is shown. It shows the state of the gel electrolyte membrane after being bent and deformed to the shape in 80°C hot water, kept for 1 minute, taken out and cooled. After the membrane is deformed, its shape is not affected by external forces at room temperature, showing its shape memory function.
[0118] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A high voltage "sandwich" structure gel polymer electrolyte, characterized in that: The invention comprises a fibrous membrane obtained by electrospinning polylactic acid (PLA) and polycaprolactone (PCL), and a dielectric layer structure formed by wrapping hydrolyzed inorganic nanomaterial hydroxyapatite (HAP) with polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) on both sides of the fibrous membrane.
2. A method for preparing a high voltage "sandwich" structure gel polymer electrolyte, characterized in that: The following steps are involved: S1. Hydrolyze and modify the inorganic nanomaterial hydroxyapatite (HAP) by coupling agent KH550 to obtain the inorganic nanomaterial hydroxyapatite (HAP) hydrolyzed and modified by coupling agent KH550, add the inorganic nanomaterial hydroxyapatite (HAP) hydrolyzed and modified by coupling agent KH550 into dichloromethane (DCM), disperse it ultrasonically in a water bath, add polylactic acid (PLA) after being evenly dispersed, stir it magnetically, add polycaprolactone (PCL) after the polylactic acid (PLA) is completely dissolved, stir it magnetically, and finally add N,N-dimethylformamide (DMF) and continue stirring until the solution is evenly mixed to obtain a mixed solution A; S2, electrospinning the mixed solution A obtained in step S1 to obtain a sample, and drying the sample in a vacuum oven to obtain a fibrous membrane; S3, adding a certain amount of inorganic nanomaterial hydroxyapatite (HAP) modified by coupling agent KH550 hydrolysis to an acetone solution, ultrasonically dispersing in a water bath, adding polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) after uniform dispersion, magnetically stirring, adding appropriate amounts of bisbenzoylphenylphosphine oxide (CIBA) photoinitiator and N,N'-methylenebisacrylamide (MBA) crosslinking agent in a light-proof environment, and continuing to stir, after uniform stirring, a mixed solution B is obtained; S4, soaking the fibrous membrane obtained in step S2 in the mixed solution B obtained in step S3, taking it out, and finally drying it to obtain a composite polymer membrane; S5, soaking the composite polymer membrane prepared in step S4 in an organic electrolyte, taking it out after soaking for 1-1.5 hours, to obtain a gel polymer electrolyte.
3. The method for preparing a high voltage "sandwich" structure gel polymer electrolyte according to claim 2, characterized in that: In the step S1, the total solid content of polylactic acid (PLA) and polycaprolactone (PCL) is 15wt% to 18wt%, and the mass ratio is polylactic acid (PLA): polycaprolactone (PCL) = (2 to 1): 1; the solid content of the inorganic nanomaterial hydroxyapatite (HAP) modified by hydrolysis of the coupling agent KH550 is 1wt% to 3wt%; and the mass ratio is dichloromethane (DCM): N,N-dimethylformamide (DMF) = (4 to 1):
1.
4. The method for preparing a high voltage "sandwich" structure gel polymer electrolyte according to claim 2, characterized in that: In the step S1, the water bath temperature is 0-10°C, the ultrasonic dispersion treatment is performed for 15-30 minutes, and the speed of the magnetic stirring treatment is 300-400 rpm.
5. The method for preparing a high voltage "sandwich" structure gel polymer electrolyte according to claim 2, characterized in that: In step S2, the vacuum oven temperature is 60-80°C and the drying time is 12-15h; In the step S2, the voltage of the electrospinning is 15-20 kV, the distance between the spinning needle and the receiving drum is 15-18 cm, the rotation speed of the receiving drum is 900-1300 r / min, the time is 6-10 h, and the pushing speed is 0.5-1 mL / h.
6. The method for preparing a high voltage "sandwich" structure gel polymer electrolyte according to claim 2, characterized in that: In the step S3, by mass ratio: the solid content of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) is 2.5wt% to 10wt%; the content of the inorganic nanomaterial hydroxyapatite (HAP) modified by hydrolysis of the coupling agent KH550 is 5% to 10% of the mass of the polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP); the photoinitiator CIBA and the cross-linking agent MBA are both 10% to 20% of the mass of the inorganic nanomaterial hydroxyapatite (HAP) modified by hydrolysis of the coupling agent KH550.
7. The method for preparing a high voltage "sandwich" structure gel polymer electrolyte according to claim 2, characterized in that: In step S3, the water bath temperature is 0-10° C., the ultrasonic dispersion is performed for 15-30 min, and the speed of the magnetic stirring treatment is 300-400 rpm.
8. The method for preparing a high voltage "sandwich" structure gel polymer electrolyte according to claim 2, characterized in that: The step S4 is specifically as follows: The fibrous membrane obtained in step S2 is soaked in the mixed solution B obtained in step S3 for 3 to 5 seconds, then taken out and UV-cured for cross-linking. The light curing time is 2 to 3 minutes, and the light power is 50 to 75%. Finally, it is placed in a vacuum oven at 60 to 80° C. for 12 to 15 hours to volatilize the residual acetone solution to obtain a composite polymer membrane.
9. The method for preparing a high voltage "sandwich" structure gel polymer electrolyte according to claim 2, characterized in that: The organic electrolyte of step 5 includes but is not limited to acetonitrile (AN)-based, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC) or ethyl methyl carbonate (EMC)-based.
10. Application of a high voltage "sandwich" structure gel polymer electrolyte, characterized in that: The gel polymer electrolyte prepared according to any one of claims 1 to 9 is used to assemble a supercapacitor, wherein the supercapacitor includes a button type, a cylindrical type or a soft package type.
Citation Information
Patent Citations
Porous gel electrolyte and preparation method and application thereof
CN114496589A
Cited By
Polyethylene oxide-based solid electrolyte as well as preparation method and application thereof
CN120581685A
Polyethylene oxide-based solid electrolyte, preparation method and application thereof
CN120581685B