Porous Nb2C / transition metal sulfide heterojunction material and preparation method and application thereof
By using the template method to construct porous Nb2C/transition metal sulfide heterojunction material in sodium ion hybrid capacitors, the problem of insufficient energy density and cycle stability of the negative electrode material in the prior art is solved, and high energy density and long cycle stability are achieved performance of sodium ion hybrid capacitors.
Patent Information
- Application Number
- CN202411349862.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
AI Technical Summary
The existing sodium ion hybrid capacitor negative electrode materials have shortcomings in terms of energy density and cyclic stability, especially the low specific capacity of Nb-based MXene and the poor cyclic stability and rate performance of transition metal sulfides, resulting in poor energy density and cyclic stability. ideal.
The frame structure of porous Nb2C is constructed by the template method, and the transition metal sulfide nanosheets are grown in situ on it to form a porous Nb2C/transition metal sulfide heterojunction material. Through this structural design, electron transport is promoted and multiple reactions are provided. Active sites to improve electrochemical performance.
High energy density and long cycle stability are achieved, porous Nb2C/transition metal sulfide heterojunction material exhibits high specific capacity and excellent cycle stability in sodium ion hybrid capacitors, with specific capacity at 100mAg–1 current density reaching 725.7mAh g–1 and retains an energy density of 89.7% after 20,000 cycles.
Smart Images

Figure CN119069269A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of negative electrode materials for sodium ion hybrid capacitors, and in particular relates to a porous Nb2C / transition metal sulfide heterojunction material and a preparation method and application thereof. Background Art
[0002] With the rapid development of renewable energy and the popularity of electric vehicles, the demand for high-performance energy storage devices is increasing. Supercapacitors have become an important component of future energy storage technology due to their advantages of fast charging, long life and environmental friendliness. However, supercapacitors face the challenge of low energy density. Currently, sodium ion hybrid capacitors have outstanding performance in energy storage devices due to their abundant resources and low cost. Therefore, seeking sodium ion hybrid capacitor negative electrode materials with high energy density and long cycle stability has great application prospects.
[0003] Among the many electrode materials developed, MXene, as a new type of two-dimensional material, has become a hot topic of research due to its excellent conductivity, good mechanical strength and chemical stability. Among them, Nb-based MXene (such as Nb2C, Nb4C3) has a unique layered structure, rich surface chemical properties and high conductivity, which makes Nb-based MXene as a negative electrode material for sodium ion energy storage. It can effectively alleviate the kinetic challenges faced by sodium ions in the energy storage process and achieve faster charge and discharge rates. However, the actual specific capacity contributed by Nb-based MXene in organic systems is low. According to the energy density calculation formula E = 1 / 2CV 2 , specific capacity and energy density are directly proportional, so low specific capacity affects its energy density.
[0004] Transition metal sulfides have high theoretical specific capacity, good conductivity and multiple reactive active sites. They can effectively react with sodium ions to provide high energy density. They are promising negative electrode materials for sodium ion batteries. However, they face the problems of slow sodium ion diffusion kinetics and volume expansion, which lead to unsatisfactory cycle stability and rate performance. Low rate performance will also lead to low energy density at high power density, which will also have an adverse effect on cycle stability.
[0005] Most existing technologies use hydrothermal methods to directly grow transition metal sulfides between MXene sheets, which leads to longer ion transport channels and less utilized reactive surfaces, which in turn affects the electrochemical performance. Summary of the invention
[0006] In view of the deficiencies of the above-mentioned prior art, the purpose of the present invention is to provide a porous Nb2C / transition metal sulfide heterojunction material and its preparation method and application. The present invention constructs a framework structure of porous Nb2C by a template method, and then fully mixes it with a transition metal salt and a sulfur source, and then undergoes a one-step annealing treatment to achieve in-situ growth of transition metal sulfide nanosheets on the porous Nb2C framework to obtain a porous Nb2C / transition metal sulfide heterojunction material. The porous Nb2C / transition metal sulfide heterojunction material prepared by the method of the present invention promotes electron transport and has multiple reactive active sites. The sodium ion hybrid capacitor assembled with the porous Nb2C / transition metal sulfide heterojunction material as the negative electrode material and the negative electrode material and the activated carbon positive electrode has high energy density and long cycle stability.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] A method for preparing a porous Nb2C / transition metal sulfide heterojunction material comprises the following steps:
[0009] Multilayer Nb2C is prepared by corroding Nb2AlC powder, and the multilayer Nb2C is layered using an organic intercalant to obtain few-layer Nb2C.
[0010] Using positively charged polystyrene nanospheres as templates, the templates and few-layer Nb2C with negative surface charges are self-assembled by electrostatic adsorption in water, and then subjected to high-temperature annealing in an inert atmosphere to remove the template and form a porous structure. The polystyrene nanospheres are distributed between Nb2C layers by electrostatic adsorption. During the annealing process, the polystyrene nanospheres are removed to form a porous Nb2C framework structure.
[0011] Porous Nb2C, a transition metal salt and a sulfur source are mixed to obtain a precursor, and the precursor is annealed to achieve in-situ growth of transition metal sulfide nanosheets on the porous Nb2C framework to obtain a porous Nb2C / transition metal sulfide heterojunction material.
[0012] Preferably, in order to construct a stable porous MXene framework structure, the mass ratio of polystyrene nanospheres to few-layer Nb2C is 0.1-0.4:1. Too many polystyrene nanospheres cause the porous Nb2C framework structure to collapse, and too few polystyrene nanospheres are insufficient to contribute enough growth sites.
[0013] Preferably, the transition metal salt is selected from Mo-based metal salts, W-based metal salts or V-based metal salts containing multiple active sites.
[0014] Preferably, the mass ratio of porous Nb2C, transition metal salt and sulfur source is 1-2:1-4:1-4. When the ratio is less than 1:4:4, the transition metal sulfide nanosheets grow excessively, resulting in the porous Nb2C being covered, causing the porous Nb2C / transition metal sulfide heterojunction material to have low conductivity and poor cycle stability; when the ratio is greater than 2:1:1, the growth sites of porous Nb2C cannot be effectively utilized, so that fewer transition metal sulfide nanosheets grow on porous Nb2C, resulting in a low specific capacity of the porous Nb2C / transition metal sulfide heterojunction material.
[0015] Preferably, when synthesizing porous Nb2C, the annealing conditions are: treating at 400-500°C for 0.5-2h.
[0016] Preferably, when synthesizing porous Nb2C / transition metal sulfide heterojunction materials, the annealing conditions are: 2-8 hours at 400-600°C. When the temperature is too high, porous Nb2C is prone to derive oxides, reducing the conductivity of the porous Nb2C / transition metal sulfide heterojunction material; when the temperature is too low, it is not conducive to the growth of transition metal sulfide nanosheets. When the time is short, transition metal sulfides do not have time to nucleate and grow; when the time is long, transition metal sulfide nanosheets are prone to agglomeration, resulting in low active site utilization.
[0017] Preferably, the method of Nb2AlC powder is: placing Nb2AlC powder in a fluorine-containing etchant, and then performing a hydrothermal reaction to obtain multilayer Nb2C.
[0018] The fluorine-containing etchant is composed of NH4F and HCl, and the mass ratio of the two is 1:6-10; the hydrothermal reaction conditions are: reacting at 140-220°C for 12-48h.
[0019] The organic intercalant is selected from tetramethylammonium hydroxide, tetrapropylammonium hydroxide or tetrabutylammonium hydroxide.
[0020] Preferably, porous Nb2C, transition metal salt and sulfur source are first mixed in water and then dried to obtain a precursor, which is then mixed in an aqueous solution and dried to achieve uniform mixing of the three. After annealing, transition metal sulfide nanosheets are uniformly grown on the porous Nb2C.
[0021] Preferably, the porous Nb2C / transition metal sulfide heterojunction material obtained after annealing is also subjected to an acid pickling treatment, wherein the treatment method is as follows: the porous Nb2C / transition metal sulfide heterojunction material is placed in a 1 mol / L H2SO4 solution and stirred for 6-12 hours, and the oxide impurities in the porous Nb2C / transition metal sulfide heterojunction material are removed by acid pickling. The oxide impurities occupy the mass of the porous Nb2C / transition metal sulfide heterojunction material, which will make the actual electrochemical performance data measured lower, that is, affect the redox activity.
[0022] The present invention also protects the porous Nb2C / transition metal sulfide heterojunction material prepared by the above preparation method.
[0023] The present invention also protects the use of the above-mentioned porous Nb2C / transition metal sulfide heterojunction material in the preparation of negative electrode materials for sodium ion hybrid capacitors.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention provides a method for preparing a porous Nb2C / transition metal sulfide heterojunction material, which comprises the following steps: Nb2AlC powder is corroded by a fluorine-containing etchant, and then a layering treatment is performed by an organic intercalation agent to obtain a few-layer Nb2C; polystyrene nanospheres are used as a template, and the template and the few-layer Nb2C are subjected to electrostatic adsorption self-assembly, and then an annealing treatment is performed to remove the template and construct a framework structure of the porous Nb2C, wherein the porous Nb2C is recorded as P-Nb2C; porous Nb2C, a transition metal salt and a sulfur source are fully mixed, and then a one-step annealing treatment is performed to realize the in-situ growth of transition metal sulfide nanosheets on the porous Nb2C framework structure, thereby obtaining a porous Nb2C / transition metal sulfide heterojunction material.
[0026] Compared with the prior art, most of the prior art uses a hydrothermal method to directly grow transition metal sulfides between MXene sheets, resulting in longer ion transmission channels and reactive surfaces with low utilization rates. The present invention designs the structure of the porous Nb2C / transition metal sulfide heterojunction material, firstly uses a template method to obtain a framework structure of the porous Nb2C, the design of the framework structure of the porous Nb2C provides abundant growth sites for transition metal sulfide nanosheets, shortens the ion diffusion path, and is conducive to efficient ion diffusion; then, in situ growth of transition metal sulfide nanosheets is performed on the framework structure of the porous Nb2C, and the transition metal sulfide nanosheets provide a high specific capacity with multiple reactive activities. In addition, the porous Nb2C / transition metal sulfide heterojunction material obtained by the preparation method of the present invention is a heterojunction structure. The construction of the heterojunction structure provides multiple reaction active sites, which is conducive to the occurrence of multiple redox reactions, contributes to pseudocapacitance, and enhances the electrochemical activity of the porous Nb2C / transition metal sulfide heterojunction material; the heterojunction interface effect also provides a charge transfer channel, promotes electron transport, and the heterojunction interface effectively enhances the electrochemical reaction kinetics of the porous Nb2C / transition metal sulfide heterojunction material, thereby meeting the research on sodium ion hybrid capacitors with high energy density and long cycle stability, which has important scientific significance and application prospects and will further promote the development of the field of hybrid capacitors.
[0027] 2. The porous Nb2C / transition metal sulfide heterojunction material of the present invention has multiple reactive active sites and fast electrochemical reaction kinetics in the sodium ion half-cell. –1 At a current density of 1.3 200 mAh g, the specific capacity of the porous Nb2C / MoS2 heterojunction material reached 725.7 mAh g –1 The sodium ion hybrid capacitor with porous Nb2C / MoS2 heterojunction material as negative electrode material and activated carbon positive electrode has a high energy density (250.6Wh kg –1 ) and excellent long-term cycling stability (89.7% retention after 20,000 cycles). BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the SEM image of P-Nb2C prepared in Example 1 of the present invention.
[0029] Figure 2 This is the SEM image of the P-Nb2C / MoS2 heterojunction material prepared in Example 1 of the present invention.
[0030] Figure 3 CV curves of the P-Nb2C / MoS2 heterojunction material and P-Nb2C at 100mV / s in Example 1 of the present invention.
[0031] Figure 4 CV curves of the P-Nb2C / MoS2 heterojunction material of Example 1 of the present invention at different scan rates.
[0032] Figure 5 This is a schematic diagram of the structure of a P-Nb2C / MoS2 / / AC sodium ion hybrid capacitor assembled using P-Nb2C / MoS2 of Example 1 of the present invention.
[0033] Figure 6 This is the cyclic stability diagram of the P-Nb2C / MoS2 / / AC sodium ion hybrid capacitor assembled with P-Nb2C / MoS2 according to Example 1 of the present invention.
[0034] Figure 7 This is the SEM image of the P-Nb2C / WS2 heterojunction material of Example 2 of the present invention.
[0035] Figure 8 CV curves of the P-Nb2C / WS2 heterojunction material of Example 2 of the present invention at different scan rates.
[0036] Fig. 9 2 is the GCD curve of the P-Nb2C / WS2 heterojunction material of Example 2 of the present invention at different scanning rates. DETAILED DESCRIPTION
[0037] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention. The experimental methods described in the embodiments of the present invention are conventional methods unless otherwise specified.
[0038] Taking into account the technical problem of low specific capacity of Nb-based MXene materials in the prior art, and the technical defects of poor cycle stability and rate performance of transition metal sulfides, the present invention composites Nb-based MXene with transition metal sulfides to obtain P-Nb2C / transition metal sulfide heterojunction materials. In the P-Nb2C / transition metal sulfide heterojunction material, the specific capacity is improved by transition metal sulfides, the diffusion kinetics and volume expansion problems of sodium ions in the energy storage process are alleviated by Nb-based MXene materials, and the rate performance and structural stability of the heterojunction material are improved by Nb-based MXene materials, thereby obtaining a P-Nb2C / transition metal sulfide heterojunction material with high energy density and long cycle stability, overcoming the technical defects of low specific capacity of Nb-based MXene materials, and overcoming the problems of unsatisfactory cycle stability and rate performance of transition metal sulfides, and being able to use P-Nb2C / transition metal sulfide heterojunction materials as negative electrode materials and apply them to sodium ion hybrid capacitors.
[0039] The technical solution of the present invention is explained below using embodiments, which are specifically as follows:
[0040] Example 1
[0041] A method for preparing a P-Nb2C / MoS2 heterojunction material comprises the following steps:
[0042] (1) 1 g of Nb2AlC powder was slowly added to the fluorine-containing etchant and stirred for 30 min. Then, it was transferred into a 50 mL polytetrafluoroethylene hydrothermal reactor and hydrothermally reacted at 180 °C for 24 h. The product was collected and centrifuged at 5000 rpm for 5 min. It was washed with deionized water several times until the pH was neutral. The precipitate was collected and re-ultrasonicated in ethanol for 15 min. The multilayer Nb2C was collected after centrifugal drying.
[0043] The fluorine-containing etchant is composed of 1 g of NH4F and 20 mL of 12 mol / L HCl.
[0044] 1 g of multilayer Nb2C was uniformly dispersed in 20 mL of tetramethylammonium hydroxide (TMAOH, 10% w / w) aqueous solution and stirred for 24 h, then centrifuged at 10000 rpm for 1 h and washed with deionized water 3 times. The precipitate was collected and added back into deionized water, and ultrasonicated in an ice-water bath under argon atmosphere for 1 h to obtain a few-layer Nb2C aqueous dispersion.
[0045] (2) 60 mL of 2 mg / mL of a few-layer Nb2C aqueous dispersion was slowly poured into 30 mL of a 1 mg / mL polystyrene aqueous solution, stirred for 1 h, dried at 60 °C for 12 h, and then annealed at 450 °C in an argon atmosphere in a tube furnace for 0.5 h to obtain porous Nb2C, namely P-Nb2C.
[0046] (3) 0.2 g of (NH4)6Mo7O 24 ·4H2O was added to 50mL of 2mg / mL P-Nb2C dispersion and stirred for 0.5h, then 0.2g of thiourea was added and stirring was continued for 2h, the precipitate was collected by centrifugation, and vacuum dried at 60℃ for 12h to obtain a precursor, the precursor was annealed at 450℃ for 3h under argon atmosphere, the powder was collected, and stirred in 1mol / L H2SO4 solution for 12h, and then centrifuged and washed several times to obtain P-Nb2C / MoS2 heterojunction material.
[0047] Example 2
[0048] A method for preparing a P-Nb2C / WS2 heterojunction material, which has the same preparation steps as those in Example 1, except that (NH4)6Mo7O 24 4H2O is replaced by an equal amount of (NH4)6W7O 24 6H2O, including the following steps:
[0049] (1) 1 g of Nb2AlC powder was slowly added to the fluorine-containing etchant and stirred for 30 min. Then, it was transferred into a 50 mL polytetrafluoroethylene hydrothermal reactor and hydrothermally reacted at 180 °C for 24 h. The product was collected and centrifuged at 5000 rpm for 5 min. It was washed with deionized water several times until the pH was neutral. The precipitate was collected and re-ultrasonicated in ethanol for 15 min. The multilayer Nb2C was collected after centrifugal drying.
[0050] The fluorine-containing etchant is composed of 1 g of NH4F and 20 mL of 12 mol / L HCl.
[0051] 1 g of multilayer Nb2C was uniformly dispersed in 20 mL of tetramethylammonium hydroxide (TMAOH, 10% w / w) aqueous solution and stirred for 24 h, then centrifuged at 10000 rpm for 1 h and washed with deionized water 3 times. The precipitate was collected and added back into deionized water, and ultrasonicated in an ice-water bath under argon atmosphere for 1 h to obtain a few-layer Nb2C aqueous dispersion.
[0052] (2) 60 mL of 2 mg / mL of a few-layer Nb2C aqueous dispersion was slowly poured into 30 mL of a 1 mg / mL polystyrene aqueous solution, stirred for 1 h, dried at 60 °C for 12 h, and then annealed at 450 °C in an argon atmosphere in a tube furnace for 0.5 h to obtain porous Nb2C, namely P-Nb2C.
[0053] (3) 0.2 g of (NH4)6W7O 24·6H2O was added to 50mL of 2mg / mL P-Nb2C dispersion and stirred for 0.5h, then 0.2g of thiourea was added and stirring was continued for 2h, the precipitate was collected by centrifugation, and vacuum dried at 60℃ for 12h to obtain a precursor, which was annealed at 450℃ for 3h under argon atmosphere, the obtained powder was collected, and stirred in 1mol / L H2SO4 solution for 12h, and then centrifuged and washed several times to obtain P-Nb2C / WS2 heterojunction material.
[0054] Example 3
[0055] A method for preparing a P-Nb2C / VS2 heterojunction material, which has the same preparation steps as those in Example 1, except that (NH4)6Mo7O 24 4H2O is replaced by an equal amount of (NH4)2V6O 16 5H2O, including the following steps:
[0056] (1) 1 g of Nb2AlC powder was slowly added to the fluorine-containing etchant and stirred for 30 min. Then, it was transferred into a 50 mL polytetrafluoroethylene hydrothermal reactor and hydrothermally reacted at 180 °C for 24 h. The product was collected and centrifuged at 5000 rpm for 5 min. It was washed with deionized water several times until the pH was neutral. The precipitate was collected and re-ultrasonicated in ethanol for 15 min. The multilayer Nb2C was collected after centrifugal drying.
[0057] The fluorine-containing etchant is composed of 1 g of NH4F and 20 mL of 12 mol / L HCl.
[0058] 1 g of multilayer Nb2C was uniformly dispersed in 20 mL of tetramethylammonium hydroxide (TMAOH, 10% w / w) aqueous solution and stirred for 24 h, then centrifuged at 10000 rpm for 1 h and washed with deionized water 3 times. The precipitate was collected and added back into deionized water, and ultrasonicated in an ice-water bath under argon atmosphere for 1 h to obtain a few-layer Nb2C aqueous dispersion.
[0059] (2) 60 mL of 2 mg / mL of a few-layer Nb2C aqueous dispersion was slowly poured into 30 mL of a 1 mg / mL polystyrene aqueous solution, stirred for 1 h, dried at 60 °C for 12 h, and then annealed at 450 °C in an argon atmosphere in a tube furnace for 0.5 h to obtain porous Nb2C, namely P-Nb2C.
[0060] (3) 0.2 g of (NH4)2V6O 16·5H2O was added to 50mL of 2mg / mL P-Nb2C dispersion and stirred for 0.5h, then 0.2g of thiourea was added and stirring was continued for 2h, the precipitate was collected by centrifugation, and vacuum dried at 60℃ for 12h to obtain a precursor, the precursor was annealed at 450℃ for 3h under argon atmosphere, the obtained powder was collected, and stirred in 1mol / L H2SO4 solution for 12h, and then centrifuged and washed several times to obtain P-Nb2C / VS2 heterojunction material.
[0061] Example 4
[0062] A method for preparing a P-Nb2C / MoS2 heterojunction material comprises the following steps:
[0063] (1) 1 g of Nb2AlC powder was slowly added to the fluorine-containing etchant and stirred for 30 min. Then, it was transferred into a 50 mL polytetrafluoroethylene hydrothermal reactor and hydrothermally reacted at 140 °C for 48 h. The product was collected and centrifuged at 5000 rpm for 5 min. It was washed with deionized water several times until the pH was neutral. The precipitate was collected and re-ultrasonicated in ethanol for 15 min. The multilayer Nb2C was collected after centrifugal drying.
[0064] The fluorine-containing etchant is composed of 1 g of NH4F and 20 mL of 15 mol / L HCl.
[0065] 1 g of multilayer Nb2C was uniformly dispersed in 20 mL of tetramethylammonium hydroxide (TMAOH, 10% w / w) aqueous solution and stirred for 24 h, then centrifuged at 10000 rpm for 1 h and washed with deionized water 3 times. The precipitate was collected and added back into deionized water, and ultrasonicated in an ice-water bath under argon atmosphere for 1 h to obtain a few-layer Nb2C aqueous dispersion.
[0066] (2) 60 mL of 2 mg / mL of a few-layer Nb2C aqueous dispersion was slowly poured into 12 mL of a 1 mg / mL polystyrene aqueous solution, stirred for 1 h, dried at 60 °C for 12 h, and then annealed at 500 °C in an argon atmosphere in a tube furnace for 1 h to obtain porous Nb2C, namely P-Nb2C.
[0067] (3) 0.4 g of (NH4)6Mo7O 24 ·4H2O was added to 50mL of 2mg / mL P-Nb2C dispersion and stirred for 0.5h, then 0.4g of thiourea was added and stirring was continued for 2h, the precipitate was collected by centrifugation, and vacuum dried at 60℃ for 12h to obtain a precursor, which was annealed at 400℃ for 8h under argon atmosphere, the obtained powder was collected, and stirred in 1mol / L H2SO4 solution for 8h, and then centrifuged and washed several times to obtain P-Nb2C / MoS2 heterojunction material.
[0068] Example 5
[0069] A method for preparing a P-Nb2C / MoS2 heterojunction material comprises the following steps:
[0070] (1) 1 g of Nb2AlC powder was slowly added to a fluorine-containing etchant and stirred for 30 min. The mixture was then transferred into a 50 mL polytetrafluoroethylene hydrothermal reactor and subjected to a hydrothermal reaction at 220 °C for 12 h. The product was collected and centrifuged at 5000 rpm for 5 min. The product was washed with deionized water several times until the pH value was neutral. The precipitate was collected and re-dispersed in ethanol by ultrasonication for 15 min. The multilayer Nb2C was collected after centrifugal drying.
[0071] The fluorine-containing etchant is composed of 1 g of NH4F and 20 mL of 9 mol / L HCl.
[0072] 1 g of multilayer Nb2C was uniformly dispersed in 20 mL of tetramethylammonium hydroxide (TMAOH, 10% w / w) aqueous solution and stirred for 24 h, then centrifuged at 10000 rpm for 1 h and washed with deionized water 3 times. The precipitate was collected and added back into deionized water, and ultrasonicated in an ice-water bath under argon atmosphere for 1 h to obtain a few-layer Nb2C aqueous dispersion.
[0073] (2) 60 mL of 2 mg / mL of a few-layer Nb2C aqueous dispersion was slowly poured into 48 mL of a 1 mg / mL polystyrene aqueous solution, stirred for 1 h, dried at 60 °C for 12 h, and then annealed at 400 °C in an argon atmosphere in a tube furnace for 2 h to obtain porous Nb2C, namely P-Nb2C.
[0074] (3) 0.1 g of (NH4)6Mo7O 24 ·4H2O was added to 50mL, 4mg / mL P-Nb2C dispersion and stirred for 0.5h, then 0.1g thiourea was added and stirring was continued for 2h, the precipitate was collected by centrifugation, and vacuum dried at 60℃ for 12h to obtain a precursor, the precursor was annealed at 600℃ for 2h under argon atmosphere, the obtained powder was collected, and stirred in 1mol / L H2SO4 solution for 6h, and then centrifuged and washed several times to obtain P-Nb2C / MoS2 heterojunction material.
[0075] Examples 1-5 of the present invention all produce P-Nb2C / transition metal sulfide heterojunction materials with high energy density and excellent cycle performance. The following is a study using the P-Nb2C / transition metal sulfide heterojunction material of Example 1 as an example. The specific research method and results are as follows:
[0076] Figure 1 This is the SEM image of P-Nb2C prepared in Example 1 of the present invention. As can be seen from the image, the framework structure of P-Nb2C is obtained using PS balls as templates.
[0077] Figure 2 This is the SEM image of the P-Nb2C / MoS2 heterojunction material prepared in Example 1 of the present invention. It can be seen from the figure that P-Nb2C provides abundant growth sites for MoS2 nanosheets. MoS2 nanosheets grow on P-Nb2C by the heterogeneous interface effect, providing a large accessible specific surface area and a shorter ion migration path for electrolyte ions, which is conducive to efficient ion diffusion.
[0078] The present invention uses a CR2032 button cell to test the behavior of the P-Nb2C / transition metal sulfide heterojunction material in a sodium ion half-cell. The sodium ion half-cell is assembled in an argon-filled glove box, using a sodium metal sheet as a counter electrode, a glass microfiber filter membrane (Whatman, GF / D) as a diaphragm, and a 1 mol / L NaPF6 solution as an electrolyte, wherein the electrolyte is obtained by dissolving NaPF6 in diethylene glycol dimethyl ether (DEGDME).
[0079] Figure 3 The sodium ion half-cell assembled with the P-Nb2C and P-Nb2C / MoS2 heterojunction materials prepared in Example 1 of the present invention has a voltage of 1 mVs -1 From the CV curves at the scan rate, it is observed that the P-Nb2C / MoS2 heterojunction material has abundant redox active sites and can provide a higher specific capacity as a negative electrode material for sodium ion storage. –1 At a current density of 1.34 W, the specific capacity of the P-Nb2C / MoS2 heterojunction material reached 725.7 mAh g –1 , which is much better than the specific capacity of P-Nb2C (174.2mAhg –1 ).
[0080] Figure 4 The CV curves of the sodium ion half-cell assembled with the P-Nb2C / MoS2 heterojunction material prepared in Example 1 of the present invention at different scan rates are shown. The P-Nb2C / MoS2 heterojunction material has fast electrochemical reaction kinetics, and the heterointerface between P-Nb2C and MoS2 can promote charge transfer and enhance the electrochemical reaction kinetics of the P-Nb2C / MoS2 heterojunction material.
[0081] Figure 5This is a structural schematic diagram of a P-Nb2C / MoS2 / / AC sodium ion hybrid capacitor assembled with the P-Nb2C / MoS2 heterojunction material prepared in Example 1 of the present invention and an activated carbon positive electrode. The assembling method is: using the P-Nb2C / MoS2 heterojunction material as the negative electrode, activated carbon as the positive electrode, a glass microfiber filter membrane (Whatman, GF / D) as the diaphragm, and a 1 mol / L NaPF6 solution as the electrolyte to assemble the P-Nb2C / MoS2 / AC hybrid sodium ion capacitor.
[0082] Figure 6 This is the cycling stability diagram of the P-Nb2C / MoS2 / / AC sodium ion hybrid capacitor. The energy density of the P-Nb2C / MoS2 / / AC sodium ion hybrid capacitor can reach 250.6Whkg –1 It can also be seen from the figure that the P-Nb2C / MoS2 / / AC sodium ion hybrid capacitor has excellent long-cycle stability and still has a capacity retention rate of 89.7% after 20,000 cycles.
[0083] Figure 7 This is the SEM image of the P-Nb2C / WS2 heterojunction material prepared in Example 2 of the present invention. It can be seen from the figure that P-Nb2C provides abundant growth sites for WS2 nanosheets. WS2 nanosheets grow on P-Nb2C by the heterogeneous interface effect, providing a large accessible specific surface area and a shorter ion migration path for electrolyte ions, which is conducive to efficient ion diffusion.
[0084] Figure 8 The CV curves of the sodium ion half-cell assembled with the P-Nb2C / WS2 heterojunction material prepared in Example 2 of the present invention at different scan rates are the same as the method of assembling a sodium ion half-cell using the P-Nb2C / MoS2 heterojunction material. The P-Nb2C / WS2 heterojunction material has fast electrochemical reaction kinetics, and the heterointerface between P-Nb2C and WS2 can promote charge transfer and enhance the electrochemical reaction kinetics of the P-Nb2C / WS2 heterojunction material.
[0085] Fig. 9 The GCD curves of the sodium ion half-cell assembled with the P-Nb2C / WS2 heterojunction material prepared in Example 2 of the present invention at different scan rates are shown in Figure 2. The P-Nb2C / WS2 heterojunction material has multiple electrochemical reaction platforms, which are attributed to the multiple redox active sites provided by WS2. The P-Nb2C / WS2 heterojunction material is used as a negative electrode material for sodium ion storage. –1 At a current density of 1.5 200 mAh g, its specific capacity reached 610.0 mAh g –1 , which is much better than the specific capacity of P-Nb2C (174.2mAhg –1 ).
[0086] In summary, the synthesized P-Nb2C / MoS2 heterojunction material has a significant porous structure, which is conducive to efficient ion diffusion. At the same time, the heterojunction interface provides a convenient transmission channel for charge transfer, ensuring the fast electrochemical reaction kinetics of the P-Nb2C / MoS2 heterojunction in sodium ion storage. The multiple reactive active sites and high electrochemical activity in the P-Nb2C / MoS2 heterojunction material give it a high specific capacity in sodium ion storage. At 100mAg –1 At a current density of 1.34 W, the specific capacity of P-Nb2C / MoS2 reached 725.7 mAh g –1 The P-Nb2C / MoS2 heterojunction material as the negative electrode material and the P-Nb2C / MoS2 / / AC sodium ion hybrid capacitor assembled with the activated carbon positive electrode have a high energy density (250.6Whkg –1 ) and excellent long-cycle stability (89.7% retention after 20,000 cycles), sodium-ion hybrid capacitors have very broad prospects in applications that require high energy and long-cycle stability of supercapacitors.
[0087] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalent technologies, the present invention is also intended to include these changes and variations. The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and their protection scope is not limited thereto. Equivalent substitutions or changes made by those skilled in the art on the basis of the present invention are all within the protection scope of the present invention, and the protection scope of the present invention shall be subject to the claims.
Claims
1. A method for preparing a porous Nb2C / transition metal sulfide heterojunction material, characterized in that: The steps include: Nb2AlC powder is corroded to prepare multilayer Nb2C, and the multilayer Nb2C is layered with an organic intercalation agent to obtain few-layer Nb2C. Using positively charged polystyrene nanospheres as templates, the templates and few-layer Nb2C with negative surface charges are electrostatically adsorbed and self-assembled in water, and then annealed in an inert atmosphere to remove the templates and form a porous structure on the few-layer Nb2C to obtain porous Nb2C. Porous Nb2C, a transition metal salt and a sulfur source are mixed to obtain a precursor, and the precursor is annealed in an inert atmosphere to achieve in-situ growth of transition metal sulfide nanosheets on the porous Nb2C to obtain a porous Nb2C / transition metal sulfide heterojunction material.
2. The method for preparing a porous Nb2C / transition metal sulfide heterojunction material according to claim 1, characterized in that: The mass ratio of polystyrene nanospheres to few-layer Nb2C is 0.1-0.4:
1.
3. The method for preparing a porous Nb2C / transition metal sulfide heterojunction material according to claim 1, characterized in that: When porous Nb2C is synthesized, the annealing conditions are: 400-500°C for 0.5-2h.
4. The method for preparing a porous Nb2C / transition metal sulfide heterojunction material according to claim 1, characterized in that: The transition metal salt is selected from Mo-based metal salts, W-based metal salts or V-based metal salts.
5. The method for preparing a porous Nb2C / transition metal sulfide heterojunction material according to claim 1, characterized in that: The mass ratio of porous Nb2C, transition metal salt and sulfur source is 1-2:1-4:1-4.
6. The method for preparing a porous Nb2C / transition metal sulfide heterojunction material according to claim 1, characterized in that: Porous Nb2C, transition metal salt and sulfur source are first mixed in water and then dried to obtain a precursor.
7. The method for preparing a porous Nb2C / transition metal sulfide heterojunction material according to claim 1, characterized in that: When synthesizing porous Nb2C / transition metal sulfide heterojunction materials, the annealing conditions are: treating at 400-600°C for 2-8h.
8. The method for preparing a porous Nb2C / transition metal sulfide heterojunction material according to claim 1, characterized in that: The porous Nb2C / transition metal sulfide heterojunction material obtained after the annealing treatment is also subjected to an acid pickling treatment. The treatment method is: placing the porous Nb2C / transition metal sulfide heterojunction material in a 1 mol / L H2SO4 solution and stirring for 6-12 hours.
9. A porous Nb2C / transition metal sulfide heterojunction material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the porous Nb2C / transition metal sulfide heterojunction material according to claim 9 in preparing a negative electrode material for a sodium ion hybrid capacitor.