Amidoxime resin as well as preparation method and application thereof

By adjusting the resin raw material ratio and hydroxylamine reaction, a three-dimensional network structure is formed, which solves the problem of small adsorption saturation capacity and low efficiency of amidoxime resin during the gallium extraction process, and significantly improves the adsorption and desorption rate of gallium.

CN119080999APending Publication Date: 2024-12-06ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411381795.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the process of gallium extraction, amidoxime resin has problems such as small adsorption saturation capacity, easy damage, and low efficiency in the adsorption-desorption process.

Method used

By adjusting the ratio of the first monomer containing carbon and nitrogen triple bonds, the second monomer containing functional groups, the crosslinking agent and the composite pore-generating agent, a three-dimensional network structure is formed, and the adsorption and desorption effect of the resin is improved, and The adsorption amount and selectivity of the resin are enhanced by the hydroxylamine geminoximetization reaction.

Benefits of technology

The adsorption performance of amidoxime resin is significantly improved, the saturated adsorption amount and desorption rate of gallium are enhanced, and efficient gallium extraction is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080999A_ABST
    Figure CN119080999A_ABST
Patent Text Reader

Abstract

The invention relates to amidoxime resin and a preparation method and application thereof.The amidoxime resin structurally comprises a resin matrix and a functional group, and the resin matrix is prepared from a first monomer containing a carbon-nitrogen triple bond, a second monomer containing the functional group, a cross-linking agent and a composite pore-foaming agent; the first monomer, the second monomer and the cross-linking agent can be subjected to polymerization reaction to form a three-dimensional network structure; the ratio of the weight M1 of the first monomer to the weight M2 of the second monomer to the weight M3 of the cross-linking agent is (50-70): (5-40): (10-30); the ratio of the sum (M1 + M2 + M3) of the weight of the first monomer, the weight of the second monomer and the weight of the cross-linking agent to the weight M4 of the composite pore-foaming agent is 100: (150-400). The amidoxime resin provided by the invention has the structural characteristics of double amidoxime and imide dioxime characteristic functional groups, has a large resin particle mass transfer contact area, and improves the adsorption performance of the resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of adsorption resin preparation, and in particular to an amidoxime resin and a preparation method and application thereof. Background Art

[0002] Gallium (Ga) is widely used in cutting-edge technology fields such as semiconductor materials, photoelectric conversion, magnetic materials, solar cells, pharmaceuticals / radiopharmaceuticals, etc. With the advancement of 5G communications, high-performance components, semiconductors and other technologies, the global demand for gallium continues to increase. At present, the gallium recovery system in the process of producing alumina from bauxite in my country is relatively mature. Almost 90% of gallium is extracted from bauxite, and amidoxime resins have been widely used in gallium extraction.

[0003] At present, amidoxime resins have defects in the gallium extraction process, such as small gallium adsorption saturation capacity, easy breakage, and low efficiency of the adsorption-desorption process. Summary of the invention

[0004] The present application provides an amidoxime resin and a preparation method and application thereof to solve the following technical problem: how to improve the adsorption performance of amidoxime resin.

[0005] In a first aspect, the present application provides an amidoxime resin, wherein the structure of the amidoxime resin comprises a resin matrix and a functional group, wherein the raw materials of the resin matrix comprise: a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent, and a composite porogen, wherein the first monomer, the second monomer, and the crosslinking agent can undergo a polymerization reaction to form a three-dimensional network structure; wherein,

[0006] The weight M of the first monomer containing a carbon-nitrogen triple bond is 1 , the weight M of the second monomer containing a functional group 2 And the weight M of the cross-linking agent 3 Satisfaction relationship:

[0007] M 1 :M 2 :M 3 =(50-70):(5-40):(10-30);

[0008] The weight M of the first monomer containing a carbon-nitrogen triple bond is 1 , the weight M of the second monomer containing a functional group 2 , the weight of the cross-linking agent M 3 And the weight M of the composite porogen 4 Satisfaction relationship:

[0009] (M 1 +M 2 +M 3 ):M4 =100:(150~400).

[0010] Optionally, the first monomer containing a carbon-nitrogen triple bond comprises at least one of the following: acrylonitrile, imino dinitrile, 3,3'-imino dipropionitrile; and / or,

[0011] The second monomer containing a functional group includes at least one of the following: methyl methacrylate, styrene, and ethylene glycol dimethacrylate.

[0012] Optionally, the composite porogen includes at least two of the following: kerosene, liquid paraffin, xylene, cyclohexanone, cyclohexane, and acetophenone.

[0013] Optionally, the cross-linking agent includes at least one of the following: divinylbenzene, isoprene, and triallyl isocyanurate.

[0014] Optionally, the raw materials of the amidoxime resin further include: an initiator and a solvent; wherein,

[0015] The initiator comprises at least one of the following: azobisisobutyronitrile, azobiscyclohexylcarbonitrile, benzoyl peroxide; and / or,

[0016] The solvent is an inorganic salt solution.

[0017] Optionally, the weight M of the first monomer containing a carbon-nitrogen triple bond is 1 , the weight M of the second monomer containing a functional group 2 , the weight of the cross-linking agent M 3 , the weight of the initiator M 5 and the weight M of the solvent 6 Satisfaction relationship: (M 1 +M 2 +M 3 ):M 5 :M 6 =100:(0.5~2):(30~300).

[0018] In a second aspect, the present application provides a method for preparing the amidoxime resin according to any one of the first aspects, the method comprising:

[0019] Mixing a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent, a composite porogen, an initiator and a solvent to obtain a mixed material;

[0020] In a vacuum environment, the mixed material is heat-treated at a first temperature, a second temperature, and a third temperature in sequence to perform a polymerization reaction to obtain a resin matrix;

[0021] The resin matrix is ​​subjected to an amidoximation reaction with hydroxylamine to obtain an amidoxime resin.

[0022] Optionally, the first temperature is 50° C. to 70° C.; and / or,

[0023] The second temperature is 75°C to 85°C; and / or,

[0024] The third temperature is 90°C to 98°C.

[0025] Optionally, the pressure of the vacuum environment is 2000Pa to 6000Pa.

[0026] In a third aspect, the present application provides a use of the amidoxime resin described in any one embodiment of the first aspect in gallium extraction.

[0027] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0028] The amidoxime resin provided in the embodiment of the present application has a structure including a resin matrix and a functional group. The raw materials of the matrix resin include: a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent and a composite porogen. The first monomer, the second monomer and the crosslinking agent can undergo a polymerization reaction to form a three-dimensional network structure. The weight M of the first monomer containing a carbon-nitrogen triple bond is 1 , the weight M of the second monomer containing the functional group 2 and the weight of the crosslinking agent M 3 Satisfaction relationship: M 1 :M 2 :M 3 =(50-70):(5-40):(10-30); the weight of the first monomer containing a carbon-nitrogen triple bond M 1 , the weight M of the second monomer containing the functional group 2 , the weight of the crosslinking agent M 3 and the weight of the porogen M 4 Satisfaction relationship: (M 1 +M 2 +M 3 ):M 4 =100:(150~400). The first monomer containing a carbon-nitrogen triple bond and the second monomer containing a functional group coordinately regulate the skeleton structure of the resin matrix and provide more reactive sites; wherein the functional group of the second monomer can improve the physical and chemical properties of the resin matrix, thereby improving the adsorption and desorption effects of the amidoxime resin; the crosslinking agent can polymerize with the two monomers to form a three-dimensional network structure and satisfy M 1 :M 2 :M 3=(50-70):(5-40):(10-30), thereby providing more grafting sites for the subsequent amidoximation reaction of the resin matrix and hydroxylamine, thereby improving the conversion rate, and further improving the adsorption capacity and selectivity of the amidoxime resin; the composite porogen can improve the pore structure of the amidoxime resin, thereby constructing a macroporous, high specific surface area and high-throughput amidoxime resin structure, and satisfying (M 1 +M 2 +M 3 ):M 4 =100:(150-400), thereby increasing the mass transfer contact area of ​​the amidoxime resin particles and improving the adsorption amount and desorption rate of the amidoxime resin. In summary, the adsorption performance of the amidoxime resin is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0031] Figure 1 A molecular structure of an amidoxime resin provided in an embodiment of the present application;

[0032] Figure 2 A schematic flow chart of a method for preparing an amidoxime resin provided in an embodiment of the present application;

[0033] Figure 3 This is an infrared spectrum of an amidoxime resin provided in Example 4 of the present application;

[0034] Figure 4 A morphological characteristic diagram of an amidoxime resin provided in Example 4 of the present application;

[0035] Figure 5 A particle size distribution diagram of an amidoxime resin provided in Example 4 of the present application;

[0036] Figure 6 This is a scanning electron microscope image of an amidoxime resin provided in Example 4 of the present application. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0038] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0039] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0040] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0041] In a first aspect, the present application provides an amidoxime resin, wherein the structure of the amidoxime resin comprises a resin matrix and a functional group, wherein the raw materials of the resin matrix comprise: a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent, and a composite porogen, wherein the first monomer, the second monomer, and the crosslinking agent can undergo a polymerization reaction to form a three-dimensional network structure; wherein,

[0042] The weight M of the first monomer containing a carbon-nitrogen triple bond is 1 , the weight M of the second monomer containing a functional group 2 And the weight M of the cross-linking agent 3 Satisfaction relationship: M 1 :M 2 :M 3 =(50-70):(5-40):(10-30);

[0043] The weight M of the first monomer containing a carbon-nitrogen triple bond is 1 , the weight M of the second monomer containing a functional group 2 , the weight of the cross-linking agent M 3 And the weight M of the composite porogen 4 Satisfaction relationship:

[0044] (M 1 +M 2 +M 3 ):M 4 =100:(150~400).

[0045] In the embodiment of the present application, the first monomer containing a carbon-nitrogen triple bond and the second monomer containing a functional group cooperate to regulate the skeleton structure of the resin matrix and provide more reactive sites; wherein the functional group of the second monomer can improve the physical and chemical properties of the resin matrix, thereby improving the adsorption and desorption effects of the amidoxime resin; the crosslinking agent can polymerize with the two monomers to form a three-dimensional network structure and satisfy M 1 :M 2 :M 3 =(50-70):(5-40):(10-30), thereby providing more grafting sites for the subsequent amidoximation reaction of the resin matrix and hydroxylamine, thereby improving the conversion rate, and further improving the adsorption capacity and selectivity of the amidoxime resin; the composite porogen can improve the pore structure of the amidoxime resin, thereby constructing a macroporous, high specific surface area and high-throughput amidoxime resin structure, and satisfying (M 1 +M 2 +M 3 ):M 4 =100:(150~400), thereby increasing the mass transfer contact area of ​​the amidoxime resin particles and improving the adsorption amount and desorption rate of the amidoxime resin.

[0046] The weight of the first monomer containing a carbon-nitrogen triple bond, the second monomer containing a functional group, the crosslinking agent, and the composite porogen are rationally designed to exert their respective functional effects, thereby facilitating the acquisition of an ideal amidoxime resin molecular structure and pore structure of the amidoxime resin, increasing the mass transfer contact area of ​​the resin particles, and thereby improving the adsorption performance of the amidoxime resin. Figure 1 The molecular structure of an amidoxime resin provided in the embodiment of the present application is shown in Figure 1 , indicating that the structure has the structural characteristics of diamidoximine and imidedioxime characteristic functional groups. Exemplary, M 1 :M 2 :M 3 It can be 50:30:20, 60:30:10, 70:20:10, 65:20:15, 60:10:30, 70:5:25, 50:40:10, etc. (M 1 +M 2 +M 3 ):M 4 It can be 100:150, 100:200, 100:250, 100:300, 100:350, 100:400, etc.

[0047] In some embodiments, the first monomer containing a carbon-nitrogen triple bond comprises at least one of the following: acrylonitrile, imino dinitrile, 3,3'-imino dipropionitrile; and / or,

[0048] The second monomer containing a functional group includes at least one of the following: methyl methacrylate, styrene, and ethylene glycol dimethacrylate.

[0049] In an embodiment of the present application, the first monomer containing a carbon-nitrogen triple bond can be a combination of one or more of acrylonitrile, imino dinitrile, and 3,3'-imino dipropionitrile; the second monomer containing a functional group can be a combination of one or more of methyl methacrylate, styrene, and ethylene glycol dimethacrylate. Methyl methacrylate and ethylene glycol dimethacrylate are hydrophilic, which improve the hydrophilicity of the resin matrix. The improved hydrophilicity is beneficial to increasing the mass transfer rate of the resin, thereby improving the adsorption and desorption effects; styrene has a benzene ring structure, which can provide more reactive sites, increase the mass transfer contact area of ​​the resin particles, and improve the adsorption performance and strength of the resin.

[0050] In some embodiments, the composite porogen includes at least two of the following: kerosene, liquid paraffin, xylene, cyclohexanone, cyclohexane, and acetophenone.

[0051] In the embodiments of the present application, the composite porogen is at least two of kerosene, liquid paraffin, xylene, cyclohexanone, cyclohexane, and acetophenone, which can improve the pore structure of the amidoxime resin, thereby constructing a macroporous, high specific surface area, and high-throughput amidoxime resin structure, increasing the mass transfer contact area of ​​the amidoxime resin particles, and improving the adsorption amount and desorption rate of the amidoxime resin.

[0052] In some embodiments, the cross-linking agent includes at least one of the following: divinylbenzene, isoprene, triallyl isocyanurate.

[0053] In the embodiment of the present application, the crosslinking agent can be a combination of one or more of divinylbenzene, isoprene, and triallyl isocyanurate. These crosslinking agents can promote the polymerization reaction between the two monomers to form a three-dimensional network structure, providing more grafting sites for the subsequent amidoximation reaction of the resin matrix and hydroxylamine, thereby improving the conversion rate, and then improving the adsorption capacity and selectivity of the amidoxime resin.

[0054] In some embodiments, the raw materials of the amidoxime resin further include: an initiator and a solvent; wherein,

[0055] The initiator comprises at least one of the following: azobisisobutyronitrile, azobiscyclohexylcarbonitrile, benzoyl peroxide; and / or,

[0056] The solvent is an inorganic salt solution.

[0057] In the present application embodiment, the initiator can be a combination of one or more of azobisisobutyronitrile, azobiscyclohexylcarbonitrile, and benzoyl peroxide. The cross-linking agent and the initiator can synergistically promote the polymerization reaction between the two monomers, provide more grafting sites for the subsequent amidoximation reaction of the resin matrix and hydroxylamine, thereby improving the conversion rate, and then improving the adsorption capacity and selectivity of the amidoxime resin. The solvent can be an inorganic salt solution, which can be a mixture of one or more of a sodium chloride aqueous solution, a calcium chloride aqueous solution, etc., and the inorganic salt solution can play a certain protective role on the resin, forming a protective film during the resin synthesis process.

[0058] In some embodiments, the weight M of the first monomer containing a carbon-nitrogen triple bond is 1 , the weight M of the second monomer containing a functional group 2 , the weight of the cross-linking agent M 3 , the weight of the initiator M 5 and the weight M of the solvent 6 Satisfaction relationship: (M 1 +M 2 +M 3 ):M 5 :M 6=100:(0.5~2):(30~300).

[0059] In the examples of the present application, the weights of the initiator and the solvent are reasonably designed to facilitate the respective functional effects of the initiator and the solvent. 1 +M 2 +M 3 ):M 5 :M 6 It can be 100:0.5:50, 100:2:200, 100:1:150, 100:2:120, 100:1.5:240, 100:1:250, 100:1:300, 100:0.5:30, etc.

[0060] In a second aspect, the present application provides a method for preparing the amidoxime resin described in any one of the first aspects, Figure 2 A schematic diagram of a process for preparing an amidoxime resin provided in an embodiment of the present application; see Figure 2 , the method comprising:

[0061] S1, mixing a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent, a composite porogen, an initiator and a solvent to obtain a mixed material;

[0062] S2. In a vacuum environment, heat-treating the mixed material at a first temperature, a second temperature, and a third temperature in sequence to perform a polymerization reaction to obtain a resin matrix solution;

[0063] S3, subjecting the resin matrix to an amidoximation reaction with hydroxylamine to obtain an amidoxime resin.

[0064] In some embodiments, the first temperature is 50°C to 70°C; and / or,

[0065] The second temperature is 75°C to 85°C; and / or,

[0066] The third temperature is 90°C to 98°C.

[0067] In the embodiment of the present application, the first temperature stage can realize the control of the intensity of the polymerization reaction; the second temperature stage can realize the control of the reaction process of the resin skeleton formation; the third temperature stage can realize the control of the resin grafting process. Exemplarily, the first temperature can be 50°C, 55°C, 60°C, 65°C, 70°C, etc.; the second temperature can be 75°C, 77°C, 79°C, 82°C, 84°C, etc.; the third temperature can be 90°C, 92°C, 94°C, 96°C, 98°C, etc. In addition, the reaction time corresponding to the first temperature can be 1h~4h, the reaction time corresponding to the second temperature can be 1h~4h, and the reaction time corresponding to the third temperature can be 4h~8h. Furthermore, a dispersant can also be added to the raw materials of the above-mentioned polymerization reaction, and the dispersant can be a combination of one or more of methyl cellulose and gelatin.

[0068] In some embodiments, the pressure of the vacuum environment is 2000Pa to 6000Pa.

[0069] In the embodiment of the present application, the pressure of the vacuum environment can be 2000Pa to 6000Pa, which can regulate the intensity of the above-mentioned polymerization reaction and ensure the purity of the reaction system. Exemplarily, the pressure of the vacuum environment can be 2000Pa, 2500Pa, 3000Pa, 3500Pa, 4000Pa, 4500Pa, 5000Pa, 5500Pa, 6000Pa, etc.

[0070] Furthermore, S2 also includes: washing, extracting, and vacuum drying the resin matrix solution obtained by the polymerization reaction to obtain a resin matrix; wherein the washing includes: washing the resin matrix solution with ethanol and hot water, and then soaking it in ethanol and hot water for 3h to 6h to dissolve unreacted porogens and reagents; the extraction includes: extracting the washed resin matrix with a vacuum pump, and filtering the solution after each rest; the vacuum drying includes: drying the extracted resin matrix with a vacuum drying oven, and the drying temperature can be 40°C to 60°C.

[0071] Further, in S3, the resin matrix and hydroxylamine undergo an amidoximation reaction, specifically including: the amidoximation reaction adopts a hydration method, first dissolving the resin matrix in a 30wt% to 50wt% ethanol / methanol / N,N-dimethylformamide aqueous solution, adding hydroxylamine hydrochloride and a base under stirring using a cyano-ammoniation conversion method, and reacting at a temperature close to reflux of 60°C to 90°C for 5h to 24h. Among them, the base can be a combination of one or more of sodium carbonate, sodium hydroxide, sodium nitrite, and sodium bisulfite. The product obtained by the amidoximation reaction of the resin matrix and hydroxylamine is washed, extracted, and dried to obtain the target amidoxime resin. The washing process includes: washing the product with hot water and cold water, and then soaking it in hot water and cold water for 2 hours to 5 hours to leach out impurities attached to the surface of the resin; the extraction process includes: extracting the washed product with a vacuum pump, and filtering the solution after each static step; the vacuum drying process includes: drying the extracted product with a vacuum drying oven, the drying temperature is 40°C to 60°C, and the drying time is 12 hours.

[0072] The preparation method of the amidoxime resin is realized based on the above-mentioned amidoxime resin. The specific raw materials of the amidoxime resin can refer to the above-mentioned embodiments. Since the preparation method of the amidoxime resin adopts part or all of the technical solutions of the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.

[0073] In a third aspect, the present application provides a use of the amidoxime resin described in any one embodiment of the first aspect in gallium extraction.

[0074] In the embodiment of the present application, the amidoxime resin meets the following indicators: O content is 16% to 30%, specific surface area is 70m 2 / cm 3 ~180m 2 / cm 3 The amidoxime resin has a good application effect in the sodium aluminate solution used by enterprises to produce alumina: when the gallium content is low at 160mg / L to 200mg / L, the saturated adsorption capacity of the resin for gallium is 10mg / g to 15mg / g, and the desorption rate can reach more than 90%, so it can be used to extract gallium.

[0075] The application of the amidoxime resin in gallium extraction is achieved based on the above-mentioned amidoxime resin. The specific raw materials of the amidoxime resin can refer to the above-mentioned embodiments. Since the application of the amidoxime resin in gallium extraction adopts part or all of the technical solutions of the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.

[0076] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0077] Example 1

[0078] An amidoxime resin, the structure of which comprises a resin matrix and a functional group, wherein the raw materials of the resin matrix comprise: a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent, a composite porogen, an initiator and a solvent; wherein the first monomer containing a carbon-nitrogen triple bond is acrylonitrile, the second monomer containing a functional group is styrene, the crosslinking agent is divinylbenzene, the composite porogen comprises cyclohexane and xylene, the initiator is azobisisobutyronitrile, and the solvent is a calcium chloride aqueous solution; the weight M of the first monomer containing a carbon-nitrogen triple bond is 1 , the weight M of the second monomer containing the functional group 2 and the weight of the crosslinking agent M 3 Satisfaction relationship: M 1 :M 2 :M 3 =70:20:10; weight of the first monomer containing a carbon-nitrogen triple bond M 1 , the weight M of the second monomer containing the functional group 2 , the weight of the crosslinking agent M 3 And the weight M of the composite porogen 4 Satisfaction relationship:

[0079] (M 1 +M 2 +M 3 ):M 4 =100:350; the weight of the first monomer containing a carbon-nitrogen triple bond M 1 , the weight M of the second monomer containing the functional group 2 , the weight of the crosslinking agent M 3 , the weight of the initiator M 5 and the weight of the solvent M 6 Satisfaction relationship:

[0080] (M 1 +M 2 +M 3 ):M 5 :M 6 =100:0.5:100.

[0081] A method for preparing amidoxime resin comprises: step 1: using a vacuum back suction method, first connecting a device, then mixing gelatin with a mass fraction of 0.1% and 100g of calcium chloride aqueous solution, adding them into a pear-shaped bottle, heating them in a water bath to 50°C, dissolving the dispersant; then introducing nitrogen protection, and the ventilation time is 0.5h; mixing an oil phase and an initiator, and gradually sucking them into the pear-shaped bottle by a vacuum back suction method for reaction: weighing styrene with a mass fraction of 20%, acrylonitrile with a mass fraction of 70%, and divinylbenzene with a mass fraction of 10%, and cycloadding the mixture; Hexane and xylene are used as porogens, and the total weight is 350% of the total weight of the monomer and the crosslinking agent. Finally, 0.5% of azobisisobutyronitrile by mass is added and mixed evenly. The vacuum pressure range is adjusted to 3500Pa, and the ventilation valve is controlled to suck the oil phase into the pear-shaped bottle at a uniform speed for reaction; the speed of the rotary evaporator is adjusted to 120-240 rpm, and the reaction is kept at 60°C for 1 hour; then the temperature is raised to 75°C and the reaction is kept for 2 hours; the temperature is raised to 95°C and the reaction is kept for 8 hours;

[0082] Step 2: After the polymerization reaction is completed, the copolymer beads are transferred to a sand core funnel and washed with anhydrous ethanol and hot water. After the porogen is extracted, the copolymer beads are filtered and vacuum dried to obtain copolymer beads.

[0083] Step 3: Using the hydration method, nitrogen is introduced, and 1.2-1.8 times the volume of the beads is added with stirring. A 1M sodium hydroxide aqueous solution is added to 20 times the mass fraction of 30% ethanol, 30% N,N-dimethylformamide and 40% water to adjust the pH value to 8. The dried copolymer beads are added to the mixed solution, stirred and swollen at 50°C for 60 minutes, and then heated to 90°C for 5 hours;

[0084] Step 4: After the reaction in step 3 is completed, the resin is transferred to a sand core funnel, the solution is filtered out, and then washed with hot water and cold water, filtered and vacuum dried to obtain amidoxime resin. The O content of the resin is 23.2%, and the specific surface area is 130m 2 / cm 3 ; The adsorption amount of gallium in sodium aluminate is 12.0 mg / g, and the desorption rate is 92.4%.

[0085] Example 2

[0086] An amidoxime resin, the structure of which comprises a resin matrix and a functional group, wherein the raw materials of the resin matrix comprise: a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent, a composite porogen, an initiator and a solvent; wherein the first monomer containing a carbon-nitrogen triple bond is acrylonitrile, the second monomer containing a functional group is styrene, the crosslinking agent is isoprene, the composite porogen comprises liquid paraffin and cyclohexanone, the initiator comprises azobisisobutyronitrile and azobiscyclohexylcarbonitrile, and the solvent is a sodium chloride aqueous solution; the weight M of the first monomer containing a carbon-nitrogen triple bond is 1 , the weight M of the second monomer containing the functional group 2 and the weight of the crosslinking agent M 3 Satisfaction relationship: M 1 :M 2 :M 3 =60:10:30; the weight of the first monomer containing a carbon-nitrogen triple bond M 1 , the weight M of the second monomer containing the functional group 2 , the weight of the crosslinking agent M 3 And the weight M of the composite porogen 4 Satisfaction relationship: (M 1 +M 2 +M 3 ):M 4 =100:250; the weight of the first monomer containing a carbon-nitrogen triple bond M 1 , the weight M of the second monomer containing the functional group 2 , the weight of the crosslinking agent M 3 , the weight of the initiator M 5 and the weight of the solvent M 6 Satisfaction relationship: (M 1 +M 2 +M 3 ):M 5 :M 6 =100:0.5:160.

[0087] A method for preparing amidoxime resin comprises: step 1: using a vacuum back suction method, first connecting a device, then mixing 0.5% by mass of methyl cellulose, 0.5% of gelatin and 160g of sodium chloride aqueous solution, adding the mixture into a pear-shaped bottle, heating the mixture in a water bath to 60°C, dissolving the dispersant; then introducing nitrogen for protection, with a ventilation time of 1 hour; mixing an oil phase and an initiator, and gradually sucking the mixture into the pear-shaped bottle for reaction by using a vacuum back suction method: weighing 10% by mass of styrene, 60% by mass of acrylonitrile, 30% by mass of isoprene, and liquid stone; Wax and cyclohexanone are added as porogens at a mass ratio of 4:1, and the total weight is 250% of the total weight of the monomer and the crosslinking agent. Finally, 0.4% of azobisisobutyronitrile and 0.1% of azobiscyclohexylcarbonitrile are added and mixed evenly. The vacuum pressure range is adjusted to 3000Pa, and the ventilation valve is controlled to suck the oil phase into the pear-shaped bottle at a uniform speed for reaction; the speed of the rotary evaporator is adjusted to 80-150 rpm, and the reaction is kept at 70°C for 2h; then the temperature is raised to 80°C and the reaction is kept for 3h; the temperature is raised to 90°C and the reaction is kept for 6h;

[0088] Step 2: After the polymerization reaction is completed, the copolymer beads are transferred to a sand core funnel and washed with acetone, anhydrous ethanol and hot water. After the porogen is extracted, the copolymer beads are filtered and vacuum dried to obtain copolymer beads.

[0089] Step 3: Using the hydration method, nitrogen is introduced, and 1.5-2.0 times the volume of the beads is added with stirring. In 10 times the mass fraction of 40% N,N-dimethylformamide and 60% water, a 1M sodium hydroxide aqueous solution is added to adjust the pH value to 9, and the dried copolymer beads are added to the mixed solution. Stir and swell at 50°C for 60 minutes, and then heat to 70°C for 9 hours;

[0090] Step 4: After the reaction in step 3 is completed, the resin is transferred to a sand core funnel, the solution is filtered out, and then washed with hot water and cold water, filtered and vacuum dried to obtain amidoxime resin. The resin has an O content of 25.3% and a specific surface area of ​​145m 2 / cm 3 The adsorption amount of gallium in sodium aluminate was 13.4 mg / g, and the desorption rate was 94.5%.

[0091] Example 3

[0092] A amidoxime resin, the structure of which comprises a resin matrix and a functional group, wherein the raw materials of the resin matrix comprise: a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent, a composite porogen, an initiator and a solvent; wherein the first monomer containing a carbon-nitrogen triple bond is 3,3'-iminobispropionitrile, the second monomer containing a functional group is methyl methacrylate, the crosslinking agent is isoprene, the composite porogen comprises acetophenone, xylene and cyclohexane, the initiator is azobisisobutyronitrile and benzoyl peroxide, and the solvent is a sodium chloride solution; the weight M of the first monomer containing a carbon-nitrogen triple bond is 1000 g / cm2 ... 1 , the weight M of the second monomer containing the functional group 2 and the weight of the crosslinking agent M 3 Satisfaction relationship: M 1 :M 2 :M 3 =50:40:10; the weight of the first monomer containing a carbon-nitrogen triple bond M 1 , the weight M of the second monomer containing the functional group 2 , the weight of the crosslinking agent M 3 And the weight M of the composite porogen 4 Satisfaction relationship: (M 1 +M 2 +M 3 ):M 4 =100:300; the weight of the first monomer containing a carbon-nitrogen triple bond M 1 , the weight M of the second monomer containing the functional group 2 , the weight of the crosslinking agent M 3 , the weight of the initiator M 5 and the weight of the solvent M 6 Satisfaction relationship: (M 1 +M 2 +M 3 ):M 5 :M 6 =100:1.5:200.

[0093] A preparation method of amidoxime resin comprises: step 1: using a vacuum back suction method, first connecting a device, then mixing 2% polyvinyl alcohol by mass, 1% gelatin and 200g of sodium chloride aqueous solution, adding them into a pear-shaped bottle, heating them in a water bath to 40°C to dissolve the dispersant; then introducing nitrogen for protection, and the ventilation time is 1h; mixing an oil phase and an initiator, and gradually sucking them into the pear-shaped bottle by a vacuum back suction method for reaction: weighing 40% methyl methacrylate by mass, 50% 3,3'-iminobispropionitrile by mass, 10% isoprene by mass, benzene Ethyl ketone, xylene and cyclohexane are used as porogens, and the mass ratio of 3:3:4 is 300% of the total weight of the monomer and the crosslinking agent. Finally, 1% by mass of azobisisobutyronitrile and 0.5% by mass of benzoyl peroxide are added and mixed evenly. The vacuum pressure range is adjusted to 4000Pa, and the ventilation valve is controlled to suck the oil phase into the pear-shaped bottle at a uniform speed for reaction; the speed of the rotary evaporator is adjusted to 140-280 rpm, and the reaction is kept at 55°C for 3 hours; then the temperature is raised to 78°C and the reaction is kept at 3 hours; the temperature is raised to 98°C and the reaction is kept at 4 hours;

[0094] Step 2: After the polymerization reaction is completed, the copolymer beads are transferred to a sand core funnel and washed with anhydrous ethanol and hot water. After the porogen is extracted, the copolymer beads are filtered and vacuum dried to obtain copolymer beads.

[0095] Step 3: Using the hydration method, nitrogen is introduced, and 1.8-2.5 times the volume of the beads is added with stirring. A 1M sodium hydroxide aqueous solution is added to 15 times the mass fraction of 30% methanol and 70% water to adjust the pH value to 6.5. The dried copolymer beads are added to the mixed solution, stirred and swollen at 40°C for 120 minutes, and then heated to 80°C for 12 hours;

[0096] Step 4: After the reaction in step 3 is completed, the resin is transferred to a sand core funnel, the solution is filtered out, and then washed with hot water and cold water, filtered and vacuum dried to obtain amidoxime resin. The O content of the resin is 20.5%, and the specific surface area is 84m 2 / cm 3 The adsorption amount of gallium in sodium aluminate was 11.9 mg / g, and the desorption rate was 90.3%.

[0097] Example 4

[0098] An amidoxime resin, the structure of which comprises a resin matrix and a functional group, wherein the raw materials of the resin matrix comprise: a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent, a composite porogen, an initiator and a solvent; wherein the first monomer containing a carbon-nitrogen triple bond is acrylonitrile, the second monomer containing a functional group is methyl methacrylate, the crosslinking agent is triallyl isocyanurate, the composite porogen comprises xylene and kerosene, the initiator is benzoyl peroxide and azobiscyclohexylcarbonitrile, and the solvent is a sodium chloride solution; the weight M of the first monomer containing a carbon-nitrogen triple bond is 1 , the weight M of the second monomer containing the functional group 2 and the weight of the crosslinking agent M 3 Satisfaction relationship: M 1 :M 2 :M 3 =50:30:20; the weight of the first monomer containing a carbon-nitrogen triple bond M 1 , the weight M of the second monomer containing the functional group 2 , the weight of the crosslinking agent M 3 And the weight M of the composite porogen 4 Satisfaction relationship: (M 1 +M 2 +M 3 ):M 4 =100:150; the weight of the first monomer containing a carbon-nitrogen triple bond M 1 , the weight M of the second monomer containing the functional group 2 , the weight of the crosslinking agent M 3 , the weight of the initiator M 5 and the weight of the solvent M 6 Satisfaction relationship: (M 1 +M 2 +M 3 ):M 5 :M 6 =100:1.5:240.

[0099] A preparation method of amidoxime resin comprises: step 1: using a vacuum back suction method, first connecting a device, then mixing 1% polyvinyl alcohol by mass, 0.5% methyl cellulose and 240g of sodium chloride aqueous solution, adding them into a pear-shaped bottle, heating them in a water bath to 50°C to dissolve the dispersant; then introducing nitrogen for protection, and the ventilation time is 1h; mixing an oil phase and an initiator, and gradually sucking them into the pear-shaped bottle by a vacuum back suction method for reaction: weighing 30% methyl methacrylate by mass, 50% acrylonitrile, and 20% triallyl isocyanurate by mass Acid esters, xylene and kerosene are used as porogens, and the mass ratio is 8:2, and the total weight is 150% of the total weight of the monomer and the crosslinking agent. Finally, 0.5% of benzoyl peroxide and 1% of azobiscyclohexylcarbonitrile are added and mixed evenly. The vacuum pressure range is adjusted to 2000Pa, and the ventilation valve is controlled to suck the oil phase into the pear-shaped bottle at a uniform speed for reaction; the speed of the rotary evaporator is adjusted to 100-200 rpm, and the reaction is kept at 50℃ for 4h; then the temperature is raised to 75℃ and the reaction is kept at this temperature for 2h; the temperature is raised to 90℃ and the reaction is kept at this temperature for 8h;

[0100] Step 2: After the polymerization reaction is completed, the copolymer beads are transferred to a sand core funnel and washed with anhydrous ethanol and hot water. After the porogen is extracted, the copolymer beads are filtered and vacuum dried to obtain copolymer beads.

[0101] Step 3: Using the hydration method, nitrogen is introduced, and 1.1-1.8 times the volume of the beads are added with stirring. A 1M sodium hydroxide aqueous solution is added to 8 times the mass fraction of 20% N,N-dimethylformamide, 30% anhydrous ethanol and 50% water to adjust the pH value to 7.5. The dried copolymer beads are added to the mixed solution, stirred and swollen at 50°C for 60 minutes, and then heated to 70°C for 24 hours;

[0102] Step 4: After the reaction in step 3 is completed, the resin is transferred to a sand core funnel, the solution is filtered out, and then washed with hot water and cold water, filtered and vacuum dried to obtain amidoxime resin. The O content of the resin is 28.4%, and the specific surface area is 155m 2 / cm 3 The adsorption amount of gallium in sodium aluminate was 14.3 mg / g, and the desorption rate was 96.2%.

[0103] Comparative Example 1

[0104] Based on the disclosure of Example 4, the difference between Comparative Example 1 and Example 4 is that: 1 :M 3 =70:30; no second monomer.

[0105] The resin has an O content of 8.5% and a specific surface area of ​​38.7 m 2 / cm3 The adsorption amount of gallium in sodium aluminate was 5.4 mg / g, and the desorption rate was 76.5%.

[0106] Comparative Example 2

[0107] Based on the disclosure of Example 4, the difference between Comparative Example 2 and Example 4 is that the total weight of the porogen is 130% of the total weight of the monomer and the cross-linking agent.

[0108] The resin has an O content of 13.6% and a specific surface area of ​​26.4 m 2 / cm 3 The adsorption amount of gallium in sodium aluminate was 7.2 mg / g, and the desorption rate was 67.2%.

[0109] Comparative Example 3

[0110] Based on the disclosure of Example 4, the difference between Comparative Example 3 and Example 4 is that: 1 :M 2 :M 3 =75:3:22.

[0111] The resin has an O content of 14.2% and a specific surface area of ​​49.5 m 2 / cm 3 The adsorption amount of gallium in sodium aluminate is 6.3 mg / g, and the desorption rate is 78.5%.

[0112] Comparative Example 4

[0113] Based on the disclosure of Example 4, the difference between Comparative Example 4 and Example 4 is that the total weight of the porogen is 450% of the total weight of the monomer and the cross-linking agent.

[0114] The resin has an O content of 33.6% and a specific surface area of ​​202.5 m 2 / cm 3 The adsorption amount of gallium in sodium aluminate was 7.8 mg / g, and the desorption rate was 96.4%.

[0115] Comparative Example 5

[0116] Based on the disclosure of Example 4, the difference between Comparative Example 5 and Example 4 is that the vacuum pressure range is adjusted to 8800 Pa.

[0117] The resin has an O content of 5.1% and a specific surface area of ​​140.8 m 2 / cm 3 The adsorption amount of gallium in sodium aluminate was 4.2 mg / g, and the desorption rate was 45.6%.

[0118] In summary, the amidoxime resin provided in the embodiment of the present application satisfies the following conditions: the O content is 16% to 30%, the specific surface area is 70 m 2 / cm 3 ~180m 2 / cm 3 . The amidoxime resin is used to extract gallium, and the saturated adsorption amount of gallium is between 10mg / g and 15mg / g, and the desorption rate can reach more than 90%. In Comparative Example 1, no second monomer is added, resulting in a decrease in grafting sites and a decrease in adsorption; in Comparative Example 2, the total weight of the porogen is low, resulting in fewer resin pores, slower mass transfer, less contact area, fewer effective functional groups, and a decrease in gallium adsorption; in Comparative Example 3, the second monomer is low and the first monomer is high, resulting in fewer resin grafting sites and a decrease in resin adsorption; in Comparative Example 4, the total weight of the porogen is high, resulting in more resin pores and a large specific surface area. Too many pores can easily cause the resin structure to collapse, affecting the stability of the resin; in Comparative Example 5, the vacuum pressure is high, resulting in an increase in side reactions, a decrease in the quality of the resin product, and a low resin adsorption amount.

[0119] Experimental testing

[0120] The amidoxime resin obtained in Example 4 was structurally characterized. For details, please refer to the following analysis:

[0121] Figure 3 This is an infrared spectrum of an amidoxime resin provided in Example 4 of the present application; see Figure 3 By analyzing the infrared spectrum formed, the functional groups and chemical structure of the resin can be inferred. From the test results, the infrared spectra at 940, 1380, 1658, and 1750 cm -1 The characteristic absorption peaks of NO, CN, C=N, and C=O appear at 3446cm -1 The broad absorption peaks on the left and right are due to -OH, -NH and -NH 2 The band where the stretching vibration appears. According to the test results, the amidoxime groups in the resin = NOH, -NH, -NH 2 The spectrum was confirmed. Figure 4 This is a morphological characteristic diagram of an amidoxime resin provided in Example 4 of the present application; see Figure 4 , optically characterize the resin, the uniformity of the resin, the uniform size of the resin, and the good spheroidization. Figure 5 This is a particle size distribution diagram of an amidoxime resin provided in Example 4 of the present application; see Figure 5 In order to further determine the particle size distribution of the resin as a whole, the resin was subjected to a Malvern particle size test. The limit particle size of 50% is 449.36μm, the limit particle size of 90% is 608.75μm, and the effective particle size can reach 100%. Through this test, it was found that the resin particle size distribution is narrow and the overall particle size of the resin is uniform. Figure 6 This is a scanning electron microscope image of an amidoxime resin provided in Example 4 of the present application; see Figure 6 To further determine the microstructure of the resin, the resin was observed by scanning electron microscopy. Figure 6 It can be seen that the resin particle size is about 300 μm, the resin surface is relatively smooth, and there are some concave or convex objects on the surface, which provides more contact area for the resin. Table 1 is the element content analysis results of the amidoxime resin provided in Example 4. The characteristic elements of the resin can be quantitatively analyzed by elemental analysis. From the test results, it can be seen that the N and O contents on the resin surface are relatively high, which also indicates that the effective functional groups grafted with the resin are more.

[0122] Table 1 Elemental content analysis results of amidoxime resin provided in Example 4

[0123] Sample No. N(%) C(%) H(%) O(%) Example 4 21.195 42.592 6.615 28.426

[0124] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:

[0125] (1) The amidoxime resin provided in the embodiments of the present application has the structural characteristics of bisamidoximate and imidodioxime, which improves the selectivity and saturated adsorption capacity of the resin for adsorbing gallium;

[0126] (2) The resin particle morphology was optimized to increase the mass transfer contact area of ​​the resin particles and improve the adsorption and desorption effects of the resin;

[0127] (3) The preparation method of the amidoxime resin provided in the embodiments of the present application has high yield, short process and low cost;

[0128] (4) The amidoxime resin provided in the embodiments of the present application can target and recover gallium from sodium aluminate solution. The resin has high selectivity, high adsorption efficiency, high desorption rate, and is more environmentally friendly. The preparation process does not require the addition of toxic and harmful chemical reagents such as chloromethyl ether, and the operation is simple and the production process is short.

[0129] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. An amidoxime resin, characterized in that: The structure of the amidoxime resin includes a resin matrix and a functional group. The raw materials of the resin matrix include: a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent and a composite porogen. The first monomer, the second monomer and the crosslinking agent can undergo a polymerization reaction to form a three-dimensional network structure; wherein, The weight M1 of the first monomer containing a carbon-nitrogen triple bond, the weight M2 of the second monomer containing a functional group, and the weight M3 of the cross-linking agent satisfy the relationship: M1:M2:M3=(50~70):(5~40):(10~30); The weight M1 of the first monomer containing a carbon-nitrogen triple bond, the weight M2 of the second monomer containing a functional group, the weight M3 of the cross-linking agent, and the weight M4 of the composite porogen satisfy the relationship: (M1+M2+M3):M4=100:(150~400).

2. The method according to claim 1, characterized in that The first monomer containing a carbon-nitrogen triple bond comprises at least one of the following: acrylonitrile, imino dinitrile, 3,3'-imino dipropionitrile; and / or, The second monomer containing a functional group includes at least one of the following: methyl methacrylate, styrene, and ethylene glycol dimethacrylate.

3. The method according to claim 1, characterized in that: The composite porogen includes at least two of the following: kerosene, liquid paraffin, xylene, cyclohexanone, cyclohexane, and acetophenone.

4. The method according to claim 1, characterized in that: The cross-linking agent includes at least one of the following: divinylbenzene, isoprene, and triallyl isocyanurate.

5. The method according to claim 1, characterized in that: The raw materials of the amidoxime resin also include: an initiator and a solvent; wherein, The initiator comprises at least one of the following: azobisisobutyronitrile, azobiscyclohexylcarbonitrile, benzoyl peroxide; and / or, The solvent is an inorganic salt solution.

6. The method according to claim 5, characterized in that The weight M1 of the first monomer containing a carbon-nitrogen triple bond, the weight M2 of the second monomer containing a functional group, the weight M3 of the cross-linking agent, the weight M5 of the initiator, and the weight M6 of the solvent satisfy the relationship: (M1+M2+M3):M5:M6=100:(0.5~2):(30~300).

7. A method for preparing the amidoxime resin according to any one of claims 1 to 6, characterized in that: The method comprises: Mixing a first monomer containing a carbon-nitrogen triple bond, a second monomer containing a functional group, a crosslinking agent, a composite porogen, an initiator and a solvent to obtain a mixed material; In a vacuum environment, the mixed material is heat-treated at a first temperature, a second temperature, and a third temperature in sequence to perform a polymerization reaction to obtain a resin matrix; The resin matrix is ​​subjected to an amidoximation reaction with hydroxylamine to obtain an amidoxime resin.

8. The method according to claim 7, characterized in that The first temperature is 50°C to 70°C; and / or the second temperature is 75°C to 85°C; and / or the third temperature is 90°C to 98°C.

9. The method according to claim 7, characterized in that: The pressure of the vacuum environment is 2000Pa-6000Pa.

10. Use of the amidoxime resin according to any one of claims 1 to 6 in the extraction of gallium.

Citation Information

Cited By

  • Method for selectively separating and extracting gallium

    CN120060672A

  • A method for selectively separating and extracting gallium

    CN120060672B