Thin barrier GaN SBD device based on nanochannel array and its preparation method

By introducing a nanochannel array structure into the GaN SBD device, direct contact between the sidewall anode and the 2DEG channel and three-sided depletion of 2DEG are achieved, which solves the problems of high turn-on voltage, large conduction loss and large reverse leakage current of traditional GaN SBD devices. problems and improve the performance and integration of the device.

CN108962976BActive Publication Date: 2024-10-11JIEJIE SEMICON CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201810706771.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-06-29
Publication Date
2024-10-11
Estimated Expiration
2038-06-29

AI Technical Summary

Technical Problem

When improving the performance of traditional GaN SBD devices, there are problems such as high turn-on voltage of low work function Schottky anodes, large reverse leakage current, large conduction loss of high work function Schottky anodes, and anode metal contact etching damage.

Method used

A thin-barrier GaN SBD device based on a nanochannel array is used to form an Al(In, Ga)N/GaN heterostructure, a SiNx charge recovery layer and a nanochannel array structure on the substrate, and combined with LPCVD technology to grow SiNx charges The recovery layer and electron beam evaporation technology deposit the anode metal to achieve direct contact between the sidewall anode metal and the 2DEG channel and deplete 2DEG on three sides.

Benefits of technology

It significantly reduces the turn-on threshold and conduction loss, increases the forward conduction current density, reduces the reverse leakage current, saves the design area, improves the integration level and reduces the process cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108962976B_ABST
    Figure CN108962976B_ABST
Patent Text Reader

Abstract

The present disclosure provides a thin barrier GaN SBD device based on a nanochannel array and a preparation method thereof; the thin barrier GaN SBD device based on a nanochannel array comprises: a substrate; a thin barrier Al(In, Ga)N / GaN heterostructure formed on the substrate; a SiNx charge recovery layer formed on the non-anode region of the thin barrier Al(In, Ga)N / GaN heterostructure; a nanochannel array structure formed on the anode region of the thin barrier Al(In, Ga)N / GaN heterostructure; and a cathode metal formed in the through hole of the SiNx charge recovery layer and an anode metal formed on the nanochannel array structure. The GaN SBD device disclosed in the present disclosure and the preparation method thereof can obtain low turn-on voltage, high forward current density and low reverse leakage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of semiconductor devices, and in particular to a thin barrier GaNSBD device based on a nanochannel array and a preparation method thereof. Background Art

[0002] The research results show that the improvement of the performance of traditional GaN SBD has the following obvious drawbacks: on the one hand, although the low work function Schottky anode can reduce the turn-on voltage, its reverse leakage current is large; on the other hand, although the high work function Schottky anode can reduce the off-state leakage current and increase the reverse withstand voltage, it significantly increases the turn-on voltage and conduction loss. At the same time, the GaN SBD with thick barrier structure needs to thin the barrier layer through anode etching to achieve the requirements of enhancing gate control and reducing leakage, but it increases the etching damage problem of the anode metal contact surface.

[0003] In view of the above disadvantages, it is urgent to provide a GaN SBD device that has low forward loss conduction and effective reverse cutoff. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the above technical problems, the present disclosure provides a thin barrier GaNSBD device based on a nanochannel array and a preparation method thereof, so as to at least partially solve the above technical problems.

[0006] (II) Technical solution

[0007] According to one aspect of the present disclosure, a thin barrier GaNSBD device based on a nanochannel array is provided, comprising:

[0008] substrate;

[0009] A thin barrier Al(In, Ga)N / GaN heterostructure formed on the substrate;

[0010] A SiNx charge recovery layer formed on the non-anode region of the thin barrier Al(In, Ga)N / GaN heterostructure;

[0011] A nanochannel array structure formed on the thin barrier Al(In, Ga)N / GaN heterostructure anode region; and

[0012] A cathode metal is formed in the through hole of the SiNx charge recovery layer and an anode metal is formed on the nanochannel array structure.

[0013] In some embodiments, the thin barrier Al(In, Ga)N / GaN heterostructure includes: a GaN buffer layer formed on the substrate and an Al(In, Ga)N thin barrier layer formed on the GaN buffer layer.

[0014] In some embodiments, a two-dimensional electron gas (2DEG) is generated between the Al(In, Ga)N thin barrier layer and the GaN buffer layer of the thin-barrier Al(In, Ga)N / GaN heterostructure.

[0015] In some embodiments, the nanochannel duty cycle is less than 50%, the nanochannel groove bottom depth is greater than the 2DEG channel depth, and the depth difference between the two is more than 30nm, and the anode metal is in direct contact with the 2DEG channel.

[0016] In some embodiments, the long side extension direction of the nanochannel recess is parallel to the connection direction of the anode and the cathode of the thin barrier GaN SBD device.

[0017] In some embodiments, a SiNx charge recovery layer is grown on top of the Al(In, Ga)N thin barrier layer using LPCVD technology, the thickness of the LPCVD-SiNx charge recovery layer is less than 20 nm, and the stress is between 1 GPa and 5 GPa.

[0018] In some embodiments, the thin barrier Al(In, Ga)N / GaN heterostructure is formed by regrowth using MOCVD, MBE or HVPE methods, the barrier layer thickness in the thin barrier Al(In, Ga)N / GaN heterostructure is between 3nm and 6nm, and the Al component is not higher than 25%; the cathode metal is Ti / Al / Ni / Au ohmic contact cathode metal, and the anode metal is Ti / Au Schottky contact anode metal.

[0019] According to another aspect of the present disclosure, a method for preparing a thin barrier GaN SBD device based on a nanochannel array is provided, comprising:

[0020] Forming a thin barrier Al(In,Ga)N / GaN heterostructure;

[0021] forming a SiNx charge recovery layer on the thin barrier Al(In, Ga)N / GaN heterostructure;

[0022] Removing part of the SiNx charge recovery layer on the non-anode region of the thin barrier Al(In, Ga)N / GaN heterostructure to form a through hole;

[0023] preparing an ohmic contact type cathode metal in the through hole of the SiNx charge recovery layer;

[0024] Removing the SiNx charge recovery layer on the anode region of the thin barrier Al(In, Ga)N / GaN heterostructure;

[0025] forming a nanochannel array structure on the thin barrier Al(In, Ga)N / GaN heterostructure anode region; and

[0026] A Schottky contact type anode metal is prepared on the anode region and the nanochannel array structure.

[0027] In some embodiments, the long side of the nanochannel groove extends in parallel to the connection direction of the diode anode and cathode, and the nanochannel duty cycle is less than 50%, the bottom depth of the nanochannel groove is greater than the 2DEG channel depth, and the depth difference between the two is more than 30nm.

[0028] In some embodiments, a SiNx charge recovery layer is grown on top of the Al(In, Ga)N thin barrier layer using LPCVD technology; the thickness of the LPCVD-SiNx charge recovery layer is less than 20 nm, and the stress is between 1 GPa and 5 GPa.

[0029] (III) Beneficial effects

[0030] It can be seen from the above technical solutions that the thin barrier GaN SBD device based on nanochannel array and the preparation method thereof disclosed in the present invention have at least one of the following beneficial effects:

[0031] (1) Compared with the traditional planar GaN SBD structure, the present invention introduces direct contact between the sidewall anode metal and the 2DEG channel while retaining the top Schottky contact. Since the sidewall anode metal is in direct contact with the 2DEG, the sidewall diode has a lower barrier height, and the current is preferentially conducted at the sidewall, which significantly reduces the diode's turn-on threshold and conduction loss, and increases the forward conduction current density.

[0032] (2) Compared with the traditional groove-type GaN SBD structure, the groove direction of the nanochannel disclosed in the present invention is parallel (not perpendicular) to the connection line between the anode and the cathode, which can avoid completely cutting off the 2DEG channel between the anode and the cathode, thereby improving the conduction current density; and does not occupy the space between the anode and the cathode, which can effectively save the design area and improve the integration.

[0033] (3) The 2DEG concentration in the GaN heterojunction structure of the thin barrier structure is low, and it can be raised to a normal level through the SiNx charge recovery layer. When the charge recovery layer is removed from the anode region of the thin barrier structure, the 2DEG in the channel will be greatly reduced. In addition, the introduction of a nanochannel array structure in the anode region can further deplete the 2DEG in the channel from both side walls, thereby significantly reducing the reverse leakage current of the device.

[0034] (4) Compared with the hybrid anode GaN SBD, the present invention reduces the anode ohmic contact electrode, further reduces the device size, improves the integration, and reduces the process cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The above and other purposes, features and advantages of the present disclosure will become more apparent through the accompanying drawings. The same reference numerals in all the drawings indicate the same parts, and the drawings are not intentionally scaled to the actual size, but the focus is on illustrating the subject matter of the present disclosure.

[0036] Figure 1 Schematic diagram of the structure of a thin barrier GaN SBD device based on a nanochannel array according to an embodiment of the present disclosure.

[0037] Figure 2-7 It is a schematic diagram of the preparation process of a thin barrier GaN SBD device based on a nanochannel array according to an embodiment of the present disclosure.

[0038] Figure 8-9 FIG. 1 is a schematic diagram of the structure of a nanochannel array according to an embodiment of the present disclosure (W trench is the channel groove width, W fin H is the width of the protrusion on the side of the channel groove, fin is the protrusion / channel groove depth).

[0039] Fig.10 The present invention is a flow chart of a method for preparing a thin barrier GaN SBD device based on a nanochannel array according to an embodiment of the present disclosure.

[0040] Fig.11 FIG. 1 is a schematic diagram of the Schottky barrier height between the anode metal and the AlGaN material according to an embodiment of the present disclosure.

[0041] Fig.12 The figure is a curve diagram of the forward turn-on voltage and forward operating voltage of the SBD device according to the embodiment of the present disclosure.

[0042] <Description of symbols>

[0043] 1-substrate, 2-GaN buffer layer, 3-Al(In, Ga)N thin barrier layer, 4-SiNx charge recovery layer, 5-nanochannel array structure, 6-cathode metal, 7-anode metal, 8-two-dimensional electron gas. DETAILED DESCRIPTION

[0044] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0045] It should be noted that in the drawings or descriptions, similar or identical parts use the same figure numbers. The implementation methods not shown or described in the drawings are forms known to those of ordinary skill in the art. In addition, although demonstrations of parameters containing specific values ​​may be provided herein, it should be understood that the parameters do not need to be exactly equal to the corresponding values, but can be approximated to the corresponding values ​​within an acceptable error tolerance or design constraint. The directional terms mentioned in the embodiments, such as "up", "down", "front", "back", "left", "right", etc., are only reference directions of the drawings. Therefore, the directional terms used are used to illustrate and are not used to limit the scope of protection of the present disclosure.

[0046] In response to the above problems, the present disclosure proposes a thin-barrier GaN SBD device based on a nanochannel array and a preparation method thereof. The thin-barrier structure effectively improves the gate control capability, and the nanochannel array can deplete the 2DEG channel from three sides. At the same time, the low-barrier Schottky contact on the sidewall increases the low-loss current channel, thereby obtaining a GaN SBD with low off-state leakage current, low turn-on voltage and high forward conduction current density.

[0047] like Figure 1 As shown, the present invention discloses a thin barrier GaN SBD device based on a nanochannel array, comprising:

[0048] substrate;

[0049] A thin barrier Al(In, Ga)N / GaN heterostructure formed on the substrate;

[0050] A SiNx charge recovery layer formed on the non-anode region of the thin barrier Al(In, Ga)N / GaN heterostructure;

[0051] A nanochannel array structure formed on the thin barrier Al(In, Ga)N / GaN heterostructure anode region; and

[0052] A cathode metal is formed in the through hole of the SiNx charge recovery layer and an anode metal is formed on the nanochannel array structure.

[0053] The thin barrier Al(In, Ga)N / GaN heterostructure comprises: a GaN buffer layer formed on the substrate and an Al(In, Ga)N thin barrier layer formed on the GaN buffer layer.

[0054] The thin barrier Al(In, Ga)N / GaN heterostructure can be regrown by MOCVD, MBE or HVPE, but the present disclosure is not limited thereto. Preferably, the barrier layer thickness in the thin barrier Al(In, Ga)N / GaN heterostructure is between 3nm and 6nm, and the Al component is not higher than 25%.

[0055] A two-dimensional electron gas 2DEG is generated between the Al(In, Ga)N thin barrier layer and the GaN buffer layer of the thin barrier Al(In, Ga)N / GaN heterostructure. The nanochannel duty cycle is less than 50%; the bottom depth of the nanochannel groove is greater than the 2DEG channel depth, and the depth difference between the two is more than 30nm; the anode metal is in direct contact with the 2DEG channel (please combine Figure 7 and 9 As shown, the anode metal in the nanochannel is in direct contact with the 2DEG channel). The extending direction of the long side of the groove of the nanochannel array structure (the groove may be a rectangular groove, corresponding to the long side of the rectangular groove) is parallel to the connection direction of the anode and cathode of the thin barrier GaN SBD device.

[0056] Specifically, the SiNx charge recovery layer is grown on the Al(In, Ga)N thin barrier layer using LPCVD technology, the thickness of the LPCVD-SiNx charge recovery layer is less than 20 nm, and the stress is between 1 GPa and 5 GPa.

[0057] The cathode metal is Ti / Al / Ni / Au ohmic contact cathode metal, and the anode metal is Ni / Au Schottky contact anode metal. The Schottky contact metal must cover the anode region without SiNx (x is between 1.1 and 1.5) dielectric part and the groove part of the nanochannel.

[0058] Please refer to Figure 2-10 As shown, the method for preparing a thin barrier GaN SBD device based on a nanochannel array disclosed in the present invention mainly includes the following steps:

[0059] S1, forming a thin barrier Al(In, Ga)N / GaN heterostructure. Specifically, the step S1 includes the following sub-steps:

[0060] S11, providing a substrate 1; wherein the substrate includes but is not limited to silicon, silicon carbide, and sapphire substrate.

[0061] S12, forming a GaN buffer layer 2 on the substrate; specifically, the GaN buffer layer may be formed by using a MOCVD process.

[0062] S13, forming an Al(In, Ga)N thin barrier layer 3 on the GaN buffer layer, wherein the Al(In, Ga)N thin barrier layer and the GaN buffer layer form a thin barrier Al(In, Ga)N / GaN heterostructure; specifically, the Al(In, Ga)N thin barrier layer can be formed on the GaN buffer layer by metal organic compound chemical vapor deposition, molecular beam epitaxy or hydride vapor phase epitaxy.

[0063] Preferably, the thickness of the thin barrier layer is 3nm to 6nm, and the Al component is not higher than 25%. A two-dimensional electron gas 8 (longitudinal naturally depleted heterojunction 2DEG (2D Electron Gas, 2DEG)) is generated between the Al(In, Ga)N thin barrier layer and the GaN buffer layer of the thin barrier Al(In, Ga)N / GaN heterostructure, which is generated by spontaneous polarization and piezoelectric polarization effects. The thin barrier energy band and electric field distribution suppress the source of 2DEG electrons in the channel, forming a two-dimensional electron gas.

[0064] S2, growing a SiNx charge recovery layer 4. Specifically, growing a LPCVD-SiNx charge recovery layer on the Al(In, Ga)N thin barrier layer of the thin barrier Al(In, Ga)N / GaN heterostructure, and growing a SiNx charge recovery layer on the Al(In, Ga)N thin barrier layer using LPCVD technology. More specifically, the thickness of the LPCVD-SiNx charge recovery layer is less than 20 nm, and the stress is between 1 GPa and 5 GPa.

[0065] Among them, the charge recovery layer LPCVD-SiNx can restore the heterojunction 2DEG, and the 2DEG concentration is significantly increased.

[0066] S3, removing the SiNx charge recovery layer on the non-anode area and preparing the cathode metal. Specifically, the step S3 includes the following sub-steps:

[0067] S31, removing part of the SiNx charge recovery layer on the non-anode area of ​​the thin barrier Al(In, Ga)N / GaN heterostructure to form a through hole; specifically, etching can be performed by combining dry and wet etching to remove part of the SiNx charge recovery layer on the non-anode area to form a through hole on the SiNx charge recovery layer.

[0068] S32, preparing an ohmic contact type cathode metal (Ti / Al / Ni / Au) 6 in the through hole of the SiNx charge recovery layer; specifically, the ohmic contact cathode metal (Ti / Al / Ni / Au) can be prepared by evaporating the metal and then forming a high temperature alloy.

[0069] S4, removing the SiNx charge recovery layer on the anode region, forming a nanochannel array structure 5, and preparing an anode metal 7. Specifically, the step S4 includes the following sub-steps:

[0070] S41, removing the SiNx charge recovery layer on the anode region of the thin barrier Al(In, Ga)N / GaN heterostructure;

[0071] S42, forming a nanochannel array structure on the thin barrier Al(In, Ga)N / GaN heterostructure anode region. Etching of the nanochannel array structure: using a Cl-based gas dry etching process to etch the nanochannel array in the dielectric opening region of the anode, the long side extension direction of the nanochannel groove is parallel to the connection direction of the diode anode and cathode, thereby avoiding completely cutting off the 2DEG channel, thereby increasing the conduction current density; and not occupying the space between the anode and the cathode, which can effectively save the design area and improve the integration. The nanochannel duty cycle (width / period) is less than 50%, H fin -H AlGaN >30nm, the depth of the nanochannel groove must be at least 30nm below the 2DEG distribution layer. Figure 8-9 shown.

[0072] S43, depositing Schottky contact anode metal (Ni / Au) on the anode region and the nanochannel array structure by electron beam evaporation technology. The Schottky contact metal covers the dielectric opening portion of the anode region and the groove portion of the nanochannel.

[0073] In the thin barrier GaN SBD device based on nanochannel array, the 2DEG in the anode region is depleted in three directions by the top anode and the sidewall anode, and the 2DEG concentration is extremely low. The 2DEG in the anode outer region is regulated by the LPCVD-SiNx charge recovery layer, and the 2DEG concentration is relatively high.

[0074] Fig.11 The Schottky barrier height between the anode metal of the SBD disclosed in the present invention and the AlGaN material (here AlGaN is used as an example for explanation) is shown. As can be seen from the figure, the top Schottky barrier height is higher, and the side wall Schottky barrier height is lower. When the current is turned on in the forward direction, the side wall is preferentially conducted.

[0075] Fig.12 V(I=1mA / mm) is the forward turn-on voltage, and V(I=100mA / mm) is the forward operating voltage. Comparison of the two curves shows that the SBD disclosed in the present invention has a lower turn-on voltage of 0.66V, a lower operating voltage of 1.26V, a lower reverse leakage current of 2.4e-16mA / mm, and a significantly improved forward conduction current.

[0076] The present invention discloses a new device structure and its preparation method proposed for the shortcomings of the traditional planar GaN Schottky barrier diode (SBD) such as high turn-on voltage, low forward current density and large reverse leakage. The device structure introduces a nanochannel array structure parallel to the anode and cathode connection line in the thin barrier GaN SBD anode region, and increases the direct contact between the sidewall anode and the 2DEG channel while the top anode Schottky contact exists. The nanochannel array structure can effectively deplete the 2DEG in the channel from three directions, and combined with the characteristics of the thin barrier structure with very low 2DEG concentration, significantly reduces the reverse leakage current of the diode; at the same time, compared with the Schottky barrier height at the top, the sidewall anode and 2DEG direct contact have a lower barrier, significantly reducing the conduction voltage and loss of the diode, thereby increasing the forward conduction current density; the nanochannel array structure design parallel to the anode and cathode connection line effectively avoids the disadvantage of completely cutting off the 2DEG channel, improves the forward conduction capability, and reduces the device size to improve the integration.

[0077] So far, the embodiments of the present disclosure have been described in detail in conjunction with the accompanying drawings. Based on the above description, those skilled in the art should have a clear understanding of the present disclosure.

[0078] It should be noted that the implementation methods not shown or described in the drawings or the text of the specification are all forms known to ordinary technicians in the relevant technical field and are not described in detail. In addition, the above definitions of each element are not limited to the various specific structures, shapes or methods mentioned in the embodiments, and ordinary technicians in the field can simply change or replace them.

[0079] Similarly, it should be understood that in order to streamline the present disclosure and aid in understanding one or more of the various disclosed aspects, in the above description of the exemplary embodiments of the present disclosure, the various features of the present disclosure are sometimes grouped together into a single embodiment, figure, or description thereof. However, this disclosed method should not be interpreted as reflecting the following intention: the claimed disclosure requires more features than the features explicitly recited in each claim. More specifically, as reflected in the claims below, the disclosed aspects are less than all the features of the single embodiment disclosed above. Therefore, the claims that follow the specific embodiment are hereby expressly incorporated into the specific embodiment, with each claim itself serving as a separate embodiment of the present disclosure.

[0080] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.

Claims

1. A thin barrier GaN SBD device based on a nanochannel array, comprising: substrate; A thin barrier Al(In,Ga)N / GaN heterostructure formed on the substrate; A SiNx charge recovery layer formed on the non-anode region of the thin barrier Al(In,Ga)N / GaN heterostructure; A nanochannel array structure formed on the anode region of the thin barrier Al(In,Ga)N / GaN heterostructure; as well as A cathode metal is formed in the through hole of the SiNx charge recovery layer and an anode metal is formed on the nanochannel array structure.

2. The nanochannel array-based thin barrier GaN SBD device according to claim 1, wherein: The thin barrier Al(In, Ga)N / GaN heterostructure includes: a GaN buffer layer formed on the substrate and an Al(In, Ga)N thin barrier layer formed on the GaN buffer layer.

3. The nanochannel array-based thin barrier GaN SBD device according to claim 2, wherein: A two-dimensional electron gas (2DEG) is generated between the Al(In,Ga)N thin barrier layer and the GaN buffer layer of the thin-barrier Al(In,Ga)N / GaN heterostructure.

4. The nanochannel array-based thin barrier GaN SBD device according to claim 3, wherein: The duty cycle of the nanochannel is less than 50%, the bottom depth of the nanochannel groove is greater than the depth of the 2DEG channel, and the depth difference between the two is more than 30nm, and the anode metal is in direct contact with the 2DEG channel.

5. The nanochannel array-based thin barrier GaN SBD device according to claim 1, wherein: The extending direction of the long side of the nanochannel recess is parallel to the connecting direction of the anode and the cathode of the thin barrier GaN SBD device.

6. The nanochannel array-based thin barrier GaN SBD device according to claim 1, wherein: The SiNx charge recovery layer is grown on the Al(In,Ga)N thin barrier layer using LPCVD technology. The thickness of the LPCVD-SiNx charge recovery layer is <20nm, and the stress is between 1 GPa and 5 GPa.

7. The nanochannel array-based thin barrier GaN SBD device according to claim 1, wherein: The thin barrier Al(In,Ga)N / GaN heterostructure is formed by regrowth using MOCVD, MBE or HVPE methods. The thickness of the barrier layer in the thin barrier Al(In,Ga)N / GaN heterostructure is between 3nm and 6nm, and the Al component is not higher than 25%; the cathode metal is Ti / Al / Ni / Au ohmic contact cathode metal, and the anode metal is Ti / Au Schottky contact anode metal.

8. A method for preparing a thin barrier GaN SBD device based on a nanochannel array, comprising: Formation of thin barrier Al(In,Ga)N / GaN heterostructure; forming a SiNx charge recovery layer on the thin barrier Al(In,Ga)N / GaN heterostructure; Removing part of the SiNx charge recovery layer on the non-anode region of the thin barrier Al(In,Ga)N / GaN heterostructure to form a through hole; preparing an ohmic contact type cathode metal in the through hole of the SiNx charge recovery layer; Removing the SiNx charge recovery layer on the anode region of the thin barrier Al(In,Ga)N / GaN heterostructure; forming a nanochannel array structure on the thin barrier Al(In,Ga)N / GaN heterostructure anode region; as well as A Schottky contact type anode metal is prepared on the anode region and the nanochannel array structure.

9. The method for preparing a thin barrier GaN SBD device based on a nanochannel array according to claim 8, wherein: The long side extension direction of the nanochannel groove is parallel to the connection direction of the diode anode and cathode, and the nanochannel duty cycle is less than 50%, the bottom depth of the nanochannel groove is greater than the 2DEG channel depth, and the depth difference between the two is more than 30nm.

10. The method for preparing a thin barrier GaN SBD device based on a nanochannel array according to claim 8, wherein: The SiNx charge recovery layer is grown on the Al(In,Ga)N thin barrier layer using LPCVD technology; the thickness of the LPCVD-SiNx charge recovery layer is <20 nm, and the stress is between 1 GPa and 5 GPa.