Copper plasma etching method and method for manufacturing display panel

Through the plasma etching method, the reaction of hydrogen chloride and hydrogen is used to control the base temperature to achieve precise dry etching of copper, solving the problems of wet etching stability and by-product deposition in high-resolution copper line etching, and improving Improve process stability and product quality.

CN109599331BActive Publication Date: 2024-10-25SAMSUNG DISPLAY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811011271.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-09-29
Filing Date
2018-08-31
Publication Date
2024-10-25
Estimated Expiration
2038-08-31

AI Technical Summary

Technical Problem

Typical wet etching processes have difficulty controlling the precise critical dimensions of copper lines, especially at widths of 2 microns or less, resulting in copper plasma etching issues with stability and by-product deposition when forming high-resolution and high-density circuits. .

Method used

Plasma etching method is adopted, using hydrogen chloride and hydrogen as etching gas, forming high-density plasma through electron cyclotron resonance plasma source, controlling the base temperature at about 10°C or lower, and passing Cu+Cl, CuCl, CuCl2 and CuH, The reaction stage of Cu3Cl3 realizes dry etching of copper, avoiding the use of additional energy, and adjusts the process stability through the ratio of hydrogen radicals and chlorine radicals.

Benefits of technology

It achieves copper dry etching at room temperature without additional energy, accurately controls the critical size, improves process stability, avoids by-product deposition and product quality degradation, and enhances the reliability of etching equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109599331B_ABST
    Figure CN109599331B_ABST
Patent Text Reader

Abstract

The present invention relates to a copper plasma etching method and a display panel manufacturing method. The copper plasma etching method according to an exemplary embodiment includes: placing a substrate on a susceptor in a processing chamber of a plasma etching device; supplying an etching gas including hydrogen chloride into the processing chamber; plasma etching a conductive layer containing copper in the substrate; and maintaining the temperature of the susceptor at 10°C or lower during the plasma etching.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2017-0127794 filed on September 29, 2017, in the Korean Intellectual Property Office, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present disclosure relates to a copper plasma etching method, and a method for manufacturing an electronic device such as a display panel by using copper plasma etching. Background Art

[0004] When manufacturing electronic devices such as display devices, semiconductor devices, etc., high-resolution circuits and high-density circuits may be required. In order to form high-resolution circuits and high-density circuits, the wires forming the circuits may need to be narrowed, and therefore, copper with high conductivity may be advantageous. Therefore, an etching process for controlling etching uniformity of copper wires, forming a good profile, having a precise critical dimension (CD), etc. may be required. However, a typical wet etching process may have difficulty in controlling a precise critical dimension when forming a copper wire having a width of, for example, about 2 micrometers (μm) or less.

[0005] The above information disclosed in this Background section is only for enhancement of understanding of the background of the invention and therefore it may contain information that does not form the prior art that is already known in this country to a person of ordinary skill in the art. Summary of the invention

[0006] Embodiments of the present application provide an improved copper plasma etching method and a method for manufacturing an electronic device.

[0007] A copper plasma etching method comprises: placing a substrate including a conductive layer containing copper on a susceptor in a processing chamber of a plasma etching device; supplying an etching gas including hydrogen chloride into the processing chamber; plasma etching the conductive layer containing copper on the substrate; and maintaining the temperature of the susceptor at about 10° C. or less during the plasma etching.

[0008] Plasma etching can include the following reaction stages:

[0009] The first reaction stage: Cu+Cl→CuCl(s)

[0010] The second reaction stage: CuCl+Cl→CuCl 2 (s)

[0011] The third reaction stage: CuCl 2 +3H→CuH(g)+2HCl(g)

[0012] 3CuCl 2 +3H→Cu 3 Cl 3 (g)+3HCl(g)

[0013] 3CuCl 2 +3 / 2H 2 →Cu 3 Cl 3 (g) + 3HCl (g).

[0014] In plasma etching, the number of hydrogen radicals may be greater than or equal to the number of chlorine radicals.

[0015] The etching gas may further include H 2 gas.

[0016] H 2 The flow rate ratio of the gas to the hydrogen chloride may be about 0.5 or less.

[0017] Plasma etching may be performed using plasma formed from an electron cyclotron resonance (ECR) plasma source.

[0018] In plasma etching, reactive ion etching may be applied.

[0019] Plasma etching can be performed in about 10 -2 About 10 -4 The process is carried out under the pressure of the support.

[0020] In plasma etching, a photoresist mask may be used as an etching mask.

[0021] A display panel manufacturing method includes: forming a conductive layer containing copper on a substrate; placing the substrate having the conductive layer formed thereon on a susceptor in a processing chamber of a plasma etching device; supplying an etching gas including hydrogen chloride into the processing chamber; plasma etching the conductive layer; and maintaining the temperature of the susceptor at about 10°C or less during the plasma etching.

[0022] The plasma etching of the conductive layer may include forming a gate line and a gate.

[0023] The plasma etching of the conductive layer may include forming a data line, a source electrode, and a drain electrode.

[0024] The substrate may be a plastic substrate.

[0025] Copper can be dry-etched without additionally using energy such as heat energy, light energy, plasma energy, etc. In addition, during etching of copper, deposition of byproducts in etching equipment can be prevented, critical dimensions can be accurately controlled, and process stability can be improved. In addition, there are several beneficial effects that can be understood throughout the specification. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The above and other advantages and features of the present disclosure will become more apparent by describing in more detail exemplary embodiments of the present disclosure with reference to the accompanying drawings.

[0027] Figure 1 is a schematic diagram of a plasma etching apparatus according to an exemplary embodiment.

[0028] Figure 2 is a flow chart of a copper plasma etching method according to an exemplary embodiment.

[0029] Figure 3 is a schematic diagram of a copper plasma etching process according to an exemplary embodiment.

[0030] Figure 4 are photographs showing etching results depending on whether reactive ion etching is applied or not.

[0031] Figure 5 is shown according to the hydrogen chloride and H 2 Photographs of etching results with different gas flow rate ratios.

[0032] Figure 6 It shows that when hydrogen chloride and H 2 Electron microscope photograph of the etching result when the gas flow rate ratio is 47.5:12.5.

[0033] Figure 7 is a graph showing optical emission spectroscopy (OES) intensity according to etching time.

[0034] Figure 8 are photographs showing etching results according to etching time.

[0035] Fig. 9 is a schematic cross-sectional view of an organic light emitting display panel according to an exemplary embodiment.

[0036] Fig.10 is a schematic cross-sectional view of a liquid crystal display panel according to an exemplary embodiment. DETAILED DESCRIPTION

[0037] The present invention will be described more fully hereinafter with reference to the accompanying drawings, in which exemplary embodiments of the present invention are shown. As those skilled in the art will appreciate, the described embodiments may be modified in various different ways, all without departing from the spirit or scope of the present invention.

[0038] The drawings and description are to be regarded as illustrative in nature and not restrictive. Like reference numerals refer to like elements throughout the specification.

[0039] In addition, for better understanding and easy description, the size and thickness of each configuration shown in the drawings are arbitrarily displayed, but the present invention is not limited thereto. In the drawings, for clarity, the thickness of layers, films, plates, regions, etc. are exaggerated. In the drawings, for better understanding and easy description, the thickness of some layers and regions are exaggerated.

[0040] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, it can be directly on the other element or intervening elements may also be present. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements.

[0041] In addition, unless explicitly described to the contrary, the word “comprise” and variations such as “comprises” or “comprising”, will be understood to imply the inclusion of stated elements but not the exclusion of any other elements.

[0042] Furthermore, in this specification, unless explicitly described to the contrary, the phrase “on a plane” means observing a target portion from the top, and the phrase “on a cross section” means observing a cross section formed by vertically cutting the target portion from the side.

[0043] It will be understood that although the terms "first", "second", "third", etc. may be used herein to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, the "first element", "component", "region", "layer" or "part" discussed below may be referred to as a second element, component, region, layer or part without departing from the teachings of this article.

[0044] The terms used herein are only for the purpose of describing specific embodiments and are not intended to be limiting. As used herein, unless the context clearly indicates otherwise, the singular forms "a", "an", and "the" are intended to include plural forms, including "at least one". "At least one" should not be interpreted as limiting "a" or "an". "Or" means "and / or". As used herein, the term "and / or" includes any or all combinations of one or more of the relevant listed items.

[0045] In addition, relative terms such as "lower" or "bottom" and "upper" or "top" may be used herein to describe the relationship of one element to another element, as shown in the figures. It will be understood that relative terms are intended to include different orientations of the device in addition to the orientation depicted in the drawings. For example, if the device in one of the figures is flipped, the element described as being on the "lower" side of the other element will then be positioned on the "upper" side of the other element. Therefore, depending on the specific orientation of the figure, the exemplary term "lower" can include both "lower" and "upper" orientations. Similarly, if the device in one of the figures is flipped, the element described as being "below" or "below" the other element will then be positioned "above" the other element. Therefore, the exemplary terms "below..." or "below..." can include both "upper" and "lower" orientations.

[0046] As used herein, "about" or "approximately" is inclusive of the stated value and means within an acceptable range of deviation of the particular value as determined by one of ordinary skill in the art, taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations, or within ±20%, 10%, or 5% of the stated value.

[0047] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs. It will be further understood that terms such as those defined in common dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant art and in the present disclosure, and will not be interpreted as an idealized or overly formal meaning unless explicitly defined as such herein.

[0048] Exemplary embodiments are described herein with reference to cross-sectional illustrations that are schematic illustrations of ideal embodiments. As such, variations in the shapes of the illustrations due to, for example, manufacturing techniques and / or tolerances are contemplated. Therefore, the embodiments described herein should not be construed as being limited to the specific shapes of the regions as illustrated herein, but rather include deviations in shape that are caused, for example, by manufacturing. For example, a region illustrated or described as flat may typically have rough and / or nonlinear features. In addition, illustrated sharp angles may be rounded. Therefore, the regions illustrated in the accompanying drawings are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions, and are not intended to limit the scope of the claims of the present invention.

[0049] In dry etching of copper (Cu), a halogen gas including fluorine (F) or chlorine (Cl) may be desirable, and a mixed gas containing hydrogen (H), nitrogen (N), helium (He), argon (Ar), etc. may be used as necessary. When a mixed gas containing chlorine is used, chlorine ions and radicals are formed by using plasma and then react with copper, thereby forming copper (I) chloride (CuCl) or copper (II) chloride (CuCl 2 ) reactants. Under typical conditions, the reactants can remain in a liquid phase or a solid phase, so copper can be etched by evaporation by applying additional energy (e.g., thermal energy, light energy, plasma energy, etc.).

[0050] CuCl or CuCl 2 The evaporation point is about 1000°C at normal pressure and about 10 -2 Up to 10 -4 The temperature of the plasma source is about 150°C in a vacuum of 1000 torr (which may be a typical pressure of an etching apparatus using a plasma source). Therefore, when a thermal method is used, CuCl or CuCl 2 Heat to about 200°C or higher to completely etch CuCl or CuCl 2 , so that no residue remains. When using optical methods, the etching equipment can be used to etch CuCl or CuCl by using a UV source 2 A radiation beam having an energy of about 2.2 electron volts (eV) or more is irradiated to vaporize copper. However, when the energy is exhausted, due to the vaporized CuCl or CuCl 2 When being discharged to the outside of the chamber, the vaporized solid CuCl or CuCl comes into contact with the inner surface of the chamber. 2 It may be redeposited on the inner surface of the substrate or chamber. When redeposition continues, the exhaust conditions for maintaining the vacuum state may change, and when redeposition increases significantly, the pipeline may be blocked and the plasma cannot be maintained. In addition, the etching byproducts redeposited into the chamber may form particles, thereby interrupting etching. In addition, the etching byproducts may contaminate the substrate, thereby reducing product quality or reducing yield.

[0051] In order to solve such a problem, according to an exemplary embodiment, a method for effectively converting CuCl or CuCl as a chlorine reactant is provided. 2 Converted to CuH and Cu which can be vaporized at room temperature 3 Cl 3 For example, the temperature of a susceptor (also referred to as a susceptor electrode or a lower electrode) on which the substrate is placed is maintained lower than the temperature of other constituent elements of the etching apparatus, thereby etching copper without causing the above-mentioned problems.

[0052] According to an exemplary embodiment, an apparatus and method for dry etching copper without using an additional energy source for vaporizing etching byproducts are provided. High-density plasma is formed as an electron cyclotron resonance (ECR) plasma source, and chlorine (Cl) and hydrogen (H) are continuously supplied at the same ratio by using hydrogen chloride as an etching gas to generate CuH and Cu in a gas phase at room temperature. 3 Cl 3 Optionally, H is added to the etching gas. 2 The gas is used to increase the density of hydrogen (H) radicals, thereby improving process stability and accelerating the generation of CuH and Cu 3 Cl 3 The reaction speed. 2 The flow rate ratio of gas to hydrogen chloride (H 2 / HCl) may be, for example, 1 or less or 0.2 or less.

[0053] Figure 1 is a schematic diagram of a plasma etching apparatus according to an exemplary embodiment, Figure 2 is a flow chart of a copper plasma etching method according to an exemplary embodiment, and Figure 3 is a schematic diagram of a copper plasma etching process according to an exemplary embodiment.

[0054] refer to Figure 1 , the plasma etching apparatus 10 includes a processing chamber 101, a microwave generator 102 for generating microwaves, and a magnetic field generator 103 including a magnetic coil for generating a magnetic field. In addition, the plasma etching apparatus 10 includes a susceptor 104 on which the substrate S is placed, a cooling device 106, and a radio frequency (RF) generator 107 in the processing chamber 101. Although not shown, the plasma etching apparatus 10 includes a gas injection device for injecting gas into the processing chamber 101 and an exhaust device that can exhaust gas (i.e., gas generated during etching) from the processing chamber 101 and control the pressure in the processing chamber 101. The plasma etching apparatus 10 may include several devices for control and operation, or may be connected to such devices. The exemplary plasma etching apparatus 10 may be modified in various ways, as can be determined by those skilled in the art.

[0055] The plasma etching device 10 uses both electric and magnetic fields to form a high-density plasma with a high plasma electron temperature, and can be referred to as an ECR etching device or an ECR plasma generator. When the microwaves generated using the microwave generator 102 have a frequency that matches the electron cyclotron frequency of the magnetic field generated using the magnetic field generator 103, electron cyclotron resonance occurs in the magnetic field in the processing chamber 101. When a gas is injected into such an ECR region, the gas is ionized so that a plasma is formed and the electrons in the plasma are accelerated due to the resonance when passing through the region, so that high energy can be obtained (e.g., achieved), and because the diffusion loss due to the magnetic field is reduced, the gas ionization rate is increased, so that a high-density plasma with a high plasma electron temperature can be generated.

[0056] Figure 2 Show use as Figure 1 The plasma etching apparatus 10 is shown in the process of etching copper.

[0057] refer to Figure 1 and Figure 2 , prepare a substrate S to be etched (S10). The substrate S can be any substrate suitable for being etched, for example, a silicon substrate, such as a wafer, a display substrate, a solar substrate, etc. A copper layer is formed in the substrate S (on which a circuit or electrode including a wire, an electrode, etc. will be formed by etching), and a mask can be formed or placed on the copper layer. The mask can define the portion to be etched in the copper layer. The mask can be a hard mask formed of silicon oxide, etc., or can be formed of a photoresist. In addition to the copper layer, one or more layers to be patterned or not patterned can also be included in the substrate S. The at least one layer can be any layer suitable for a specific device. The prepared substrate S is placed on a pedestal 104 in the processing chamber 101.

[0058] After the substrate S is placed on the susceptor 104 in the process chamber 101, hydrogen chloride or hydrogen chloride and H are supplied into the process chamber 101. 2 Gas (S20). Hydrogen chloride or hydrogen chloride and H 2 The gas is used as a process gas or etching gas for etching copper. Next, chlorine plasma and hydrogen plasma are formed from the process gas by using an ECR plasma source (S30). The ECR plasma source can be supplied using a microwave generator 102 and a magnetic field generator 103.

[0059] The copper layer of the substrate S is etched corresponding to the pattern of the mask using chlorine (Cl) plasma and hydrogen (H) plasma (S40). The etching may be performed through the following three-stage reaction.

[0060] The first reaction stage: Cu+Cl→CuCl(s)

[0061] The second reaction stage: CuCl+Cl→CuCl 2 (s)

[0062] The third reaction stage: CuCl 2 +3H→CuH(g)+2HCl(g)

[0063] 3CuCl 2 +3H→Cu 3 Cl 3 (g)+3HCl(g)

[0064] 3CuCl 2 +3 / 2H 2 →Cu 3 Cl 3 (g) + 3HCl (g).

[0065] The CuCl and CuCl produced in the first and second reaction stages 2 It is non-volatile at room temperature and -2 Up to 10 -4 When heat of about 150° C. or more is applied at 100° C. (which may be the process pressure of the plasma apparatus 10), the copper ions are vaporized. However, since CuCl and CuCl are generated by the reaction between copper and chlorine, 2 Heat is generated, and the energy from the plasma increases the internal temperature of the processing chamber 101, so CuCl and CuCl 2 Can be partially vaporized without additional heat supply. Therefore, when copper is etched, it may be necessary to suppress CuCl and CuCl 2 vaporizes so that CuCl and CuCl are redeposited in the process chamber 101 when copper is etched. 2 The temperature increase of the substrate S may be suppressed, and the temperature of the substrate S may be controlled by the susceptor 104. Since the substrate S is placed on the susceptor 104, the temperature of the substrate S may be approximately the same as or similar to the temperature Ts of the susceptor 104.

[0066] For the temperature control of the substrate S, the temperature Ts of the susceptor 104 on which the substrate S is placed can be set to be the lowest in the entire configuration of the plasma etching apparatus 10 (e.g., in the configuration in the processing chamber 101 and the processing chamber 101). During the etching process, the temperature Ts of the susceptor 104 can be maintained lower than the inner wall temperature Tc of the processing chamber 101. The inner wall temperature Tc of the processing chamber 101 can be higher than room temperature, and the temperature Ts of the susceptor 104 can be lower than room temperature. According to an exemplary embodiment, the temperature Ts of the susceptor 104 can be maintained at a temperature lower than the inner wall temperature Tc of the processing chamber 101, e.g., about 10 °C or lower. Although the inner wall temperature Tc of the processing chamber 101 is reduced to be lower than the evaporation points of CuCl and CuCl 2 e.g., reduced to about 100 °C, the thermal energy or ion bombardment in the plasma is dispersed, so that the substrate S can be locally heated with respect to the particles having high energy to vaporize CuCl and CuCl 2 . When the temperature Ts of the susceptor 104 is sufficiently reduced to, for example, lower than about 10 °C, the entire substrate S can be maintained at a temperature lower than the evaporation points of CuCl and CuCl 2 .

[0067] It may be advantageous when the temperature of the susceptor 104 is as low as possible, but if the temperature is too low, process errors may occur due to condensation in the plasma etching apparatus 10. Therefore, the temperature Ts of the susceptor 104 can be higher than the temperature that causes condensation. For example, the temperature Ts can be higher than about -50 °C. The temperature Ts of the susceptor 104 can be controlled using a cooling device 106 connected to the susceptor 104, and for example, the temperature Ts of the susceptor 104 can be set to a predetermined temperature by circulating a coolant to the susceptor 104.

[0068] When the temperature Ts of the susceptor 104 is maintained at a sufficiently low level less than about 10 °C (i.e., Ts < Tc), an etching reaction of the third reaction stage is carried out to effectively generate CuH and Cu 3 Cl 3 .

[0069] Referring to Figure 3 , CuCl is formed by the reaction of copper (Cu) and chlorine (Cl) radicals, and chlorine is continuously supplied for the additional reaction of CuCl and chlorine radicals in the second reaction stage, so that the portion of the copper layer where copper is to be etched (i.e., the portion not covered by the mask M) is saturated with CuCl 2 . In the third reaction stage, CuH and Cu 3 Cl 3 (which is from CuCl 2The copper is completely etched by the reaction of hydrogen radicals (substances that remain gaseous at room temperature and pressure and then vaporize). Hydrogen chloride (HCl) is also produced in the third reaction stage, and the hydrogen chloride is separated into hydrogen radicals and chlorine radicals by the plasma source and thus reused in the copper etching process. 3 Cl 3 It has material stability and thus does not separate, and thus can be exhausted to the outside of the process chamber 101 in a gaseous state.

[0070] In order to continuously maintain the etching reaction in the third reaction stage, hydrogen ions and radicals may be supplied in an amount equal to or greater than that of chlorine ions and radicals.

[0071] N H自由基 ≥N Cl自由基

[0072] According to an exemplary embodiment, hydrogen chloride gas is used as an etching gas. By using an ECR plasma source to separate hydrogen chloride, it is possible to generate hydrogen radicals and chlorine radicals at the same ratio. In addition, hydrogen gas is supplied to increase the number of hydrogen radicals. When H 2 Free Radicals and CuCl 2 reacts and thus forms Cu 3 Cl 3 When H is supplied, heat absorption occurs, which may reduce the temperature of the substrate S placed on the susceptor 104. 2 The gas can inhibit unnecessary CuCl and CuCl 2 Vaporization of reactants and improved process stability.

[0073] When an ECR plasma source is used in an etching process, it may be advantageous in the process because the ECR plasma source includes a high density plasma (e.g., about 10 11 / cm 3 or higher) and high energy (e.g., about 1 eV to about 10 eV). 2 With a high energy bond of about 4.52 eV at room temperature, an ECR plasma source may be desirable to efficiently form hydrogen radicals. As described above, the microwave generator 102 and the magnetic field generator 103 of the plasma etching apparatus 10 may be used as an ECR plasma source.

[0074] Figure 4 are photographs showing etching results depending on application of reactive ion etching.

[0075] exist Figure 4, the left figure is a photograph showing a copper layer sample etched by using an ECR plasma source with a power of 900 watts (W), and the right figure is a photograph showing a copper layer sample etched by applying a self-bias voltage of -150 volts (V) together with an ECR plasma source with a power of 900 W. When combined with the RIE mode (for example, when used on the susceptor 104), an ion reaction is added so that anisotropic etching can be improved. Reactive ion etching can be implemented by applying radio frequency to the susceptor 104, for example, using the RF generator 107.

[0076] Figure 5 is shown according to the hydrogen chloride and H 2 The photo of the etching result of the gas flow rate ratio and Figure 6 is to show that hydrogen chloride and H 2 This is a scanning electron microscope photograph of the etching results when the gas flow rate ratio is 47.5:12.5.

[0077] When the number of hydrogen radicals is too large, CuCl 2 It may take a long time to reach the saturation state, and etching may be interrupted. Therefore, it may be advantageous to use an appropriate ratio. In order to obtain (e.g., achieve) etching results according to the gas ratio, the ECR power is set to 900 W, the RIE is set to 50 W (-150 V), and the gap between the plasma source and the substrate (corresponding to Figure 1 The gap between the opposing electrode 105 and the substrate S in the etching process is set to 1 cm, and the treatment time is set to 300 seconds, and the copper layer is etched by adjusting the hydrogen chloride and H 2 The gas ratio is adjusted by adjusting the gas flow rate. Figure 5 Some etching results are shown.

[0078] With H 2 As the flow rate ratio of HCl:H increases, the etching rate decreases, and when 2 When the flow rate ratio of H becomes 40:20, the copper layer is not etched within 300 seconds, and when 2 The flow rate ratio relative to hydrogen chloride (H 2 When the flow rate ratio (H / HCl) is between 0 and 0.5, various and effective copper etching rates and various copper micropatterns can be obtained (e.g., achieved). 2 When the flow rate ratio (H / HCl) exceeds 0.5, the etching time increases rapidly, which may be caused by the insufficient amount of chlorine radicals. 2 / HCl) exceeds 1, CuCl x The layer is not fully formed, thereby interrupting etching.

[0079] In addition, when HCl:H 2When the flow rate ratio is 47.5:12.5, Figure 6 As shown in Figure 2, the critical dimension (CD) of copper etching can be precisely controlled. That is, when the flow rate ratio (H 2 / HCl) is about 0.263, with about A copper layer having a thickness of about 100 nm and a width of about 1 nm to about 2 nm can be micropatterned at a high etching rate of about 300 nm / min. Therefore, when the etching rate and the etching critical dimension are considered together, when the flow rate ratio (H 2 / HCl) is about 0.263 or less (i.e., when HCl is relative to H 2 The flow rate ratio (HCl / H 2 ) is about 3.8 or greater). In terms of process, it may be advantageous when the total flow rate of the etching gas is increased according to the substrate size, pattern design, and process environment, and for example, the total flow rate may be increased to about 100 cubic centimeters per minute (sccm), and the flow rate ratio of the hydrogen chloride may be changed according to the process conditions.

[0080] Figure 7 is a graph showing OES intensity according to etching time, and Figure 8 are photographs showing etching results according to etching time.

[0081] The etching reaction in the third stage can be confirmed by the optical emission spectroscopy (OES) data and the copper etching results according to the etching time. As process conditions, the ECR power was set to 900 W, the RIE was set to 50 W (-150 V), the gap between the plasma source and the substrate was set to 1 cm, and the HCl:H 2 The flow rate ratio of was set to 47.5:12.5, and the etching time was set to 120 seconds (s), 180s, 240s and 300s, and the etching results were compared. Figure 7 As shown, from the moment the plasma is turned on, through the free radical reaction of copper and chlorine, CuCl x The intensity of CuCl increases fastest, reaching a peak at 120 seconds. x The growth reaches saturation and then is vaporized into CuH or Cu by reacting with hydrogen radicals. 3 Cl 3 , making CuCl x Through this experiment, the third stage etching reaction according to the exemplary embodiment can be verified.

[0082] According to an exemplary embodiment, an etching apparatus and an etching method capable of etching copper at room temperature without additional energy can be provided. By using an ECR plasma source to form a high-density plasma and using HCl as an etching gas, chlorine and hydrogen can be continuously supplied at the same ratio. Optionally, hydrogen gas is added to increase the density of hydrogen radicals, thereby improving process stability, and the etching reaction of the third reaction can accelerate the process for forming CuCl and CuH reactants (gaseous at room temperature and atmospheric pressure). 2 The temperature Ts of the susceptor 104 on which the substrate S (on which the foregoing reaction occurs) is placed is maintained significantly lower than the temperature of other components of the etching apparatus 10 (e.g., Ts < Tc) to suppress the evaporation of non-volatile etching by-products, thereby stably maintaining the process. However, different from the typical method of etching copper by increasing the temperature of the substrate S, according to the exemplary embodiment, copper can be etched with a precise critical dimension while maintaining the temperature Ts of the susceptor 104 at about 10 °C or lower to suppress the evaporation of CuCl and CuCl2. The temperature Ts of the susceptor 104 is lowered to the lowest in the overall configuration of the etching apparatus 10, so that the temperature of the substrate S can be reduced. 3 Cl 3 For the copper etching reaction of the third reaction, it can be advantageous to supply the number of hydrogen radicals equal to or greater than the number of chlorine radicals. Therefore, hydrogen gas can be added to hydrogen chloride as an etching gas, and H2 and CuCl2 undergo a chemical reaction, resulting in endothermic heat absorption. When etching copper by forming hydrogen radicals and chlorine radicals only using hydrogen chloride gas, it may be limited in some cases. For example, due to the heat generated by the process of forming CuCl and CuCl2 and the plasma heat, a certain part in the processing chamber 101 may be temporarily overheated. Although the temperature Ts of the susceptor 104 is maintained at less than about 10 °C to reduce the temperature of the substrate S, it may also apply excessive heat to the copper layer of the substrate or the mask formed on the copper layer. When the mask is a photoresist or the substrate S is formed of plastic (e.g., an organic polymer), the mask or the substrate S may be damaged due to the instantaneous high heat. When H2 is supplied, H2 and CuCl2 react with each other, causing endothermic heat absorption while forming CuCl, and then the internal temperature of the processing chamber 101 can be reduced, thereby suppressing CuCl and CuCl2

[0083] Come back to reference Figure 1 ,其上放置有基板S(在该基板S上发生前述反应)的基座104的温度Ts被保持为比蚀刻设备10的其他构成元件的温度显著更低(例如,Ts<Tc),以抑制非挥发性蚀刻副产物的蒸发,从而稳定地保持该过程。然而,不同于其中通过增加基板S的温度来蚀刻铜的典型方法,根据示例性实施方式,可以以精确的临界尺寸蚀刻铜同时保持基座104的温度Ts在约10℃或更低,以抑制CuCl和CuCl 2 的蒸发。在蚀刻设备10的整体配置中基座104的温度Ts降低到最低,使得可以降低基板S的温度。

[0084] 对于第三反应的铜蚀刻反应,将氢自由基的数量供应为等于或大于氯自由基的数量可以有利的。因此,可以将H 2 气添加到作为蚀刻气体的氯化氢中,并且H 2 和CuCl 2 发生化学反应,从而发生吸热。当通过仅使用氯化氢气体形成氢自由基和氯自由基来蚀刻铜时,在一些情况下可能会受到限制。例如,由于形成CuCl和CuCl 2 的过程产生的热量和等离子体热,处理室101中的某个部分可能暂时被过度加热。虽然为了降低基板S的温度而将基座104的温度Ts保持为小于约10℃,但也可能对基板的铜层或形成于铜层上的掩模施加过高的热量。当掩模是光刻胶或基板S由塑料(例如,有机聚合物)形成时,掩模或基板S可能由于瞬间的高热量而被损坏。当供应H 2 时,H 2 和CuCl 2 彼此反应,使得在引起吸热的同时形成Cu 3 Cl 3 ,然后可以降低处理室101的内部温度,由此抑制CuCl和CuCl2 of vaporization and release or remove process limitations.

[0085] Hereinafter, a display panel will be described, which is one of various electronic devices and electronic components to which the above-mentioned etching method can be applied. The etching method can be used to manufacture a display panel such as an organic light emitting display panel, a liquid crystal display panel, etc.

[0086] Fig. 9 is a schematic cross-sectional view of an organic light emitting display panel according to an exemplary embodiment, and Fig.10 is a schematic cross-sectional view of a liquid crystal display panel according to an exemplary embodiment.

[0087] As will be understood by one of ordinary skill in the art, the display panel may include various configurations other than those shown. First, an organic light emitting display panel will be described, and a liquid crystal display panel will be described focusing on their differences.

[0088] refer to Fig. 9 , the display panel 20 includes a substrate 110 , and signal lines and elements formed of a plurality of layers on the substrate 110 .

[0089] The substrate 110 may be a flexible substrate formed of a plastic (eg, polymer) film. For example, the substrate 110 may be formed of a polymer such as polyimide, polyamide, polyester (eg, polyethylene terephthalate), etc. The substrate 110 may be a hard substrate made of glass or silicon.

[0090] The substrate 110 may include a barrier layer (not shown) that prevents diffusion of impurities (degradation of semiconductor characteristics) and penetration of moisture or the like.

[0091] The semiconductor 131 of the transistor TR is located on the substrate 110, and the gate insulating layer 140 is located on the semiconductor 131. The semiconductor 131 includes a source region and a drain region and a channel region disposed between the source region and the drain region. The semiconductor 131 may include polycrystalline silicon, an oxide semiconductor, or amorphous silicon. The gate insulating layer 140 may be formed by depositing an inorganic insulating material such as silicon oxide, silicon nitride, etc.

[0092] A gate conductor including a gate line 121 and a gate 124 of the transistor TR is located on the gate insulating layer 140. The gate conductor may be formed by depositing a conductive material such as copper (Cu), aluminum (Al), silver (Ag), molybdenum (Mo), chromium (Cr), tantalum (Ta), titanium (Ti), etc. on the substrate 110 and patterning it.

[0093] When copper is used as the gate conductor, as an example, a copper layer is formed on the substrate 110 by sputtering. Next, a mask is formed or disposed on the copper layer, and then etching is performed by using the copper plasma etching method according to the above exemplary embodiment so as to form a gate conductor as a patterned copper layer. When the copper layer is etched, the temperature of the susceptor on which the substrate 110 is placed is maintained at about 10° C. or less, thereby lowering the temperature of the substrate 110, and H is additionally supplied to the etching gas. 2 With CuCl 2 The reaction, while causing heat absorption, allows the temperature of the substrate 110 to be reduced, and thus, a photoresist that may be sensitive to heat can be used as a mask. In addition, since the substrate 110 is kept at a low temperature, the substrate 110 is not damaged during dry etching of the copper layer even if, for example, a plastic substrate is used.

[0094] The interlayer insulating layer 160 is located on the gate conductor. The interlayer insulating layer 160 may include an inorganic insulating material. A data conductor including a data line 171 and a source 173 and a drain 175 of the transistor TR is disposed on the interlayer insulating layer 160. The source 173 and the drain 175 are connected to the semiconductor layer 131 through contact holes formed in the interlayer insulating layer 160 and the gate insulating layer 140, respectively. The data conductor may include a metal or metal alloy such as copper (Cu), aluminum (Al), silver (Ag), molybdenum (Mo), chromium (Cr), gold (Au), platinum (Pt), palladium (Pd), tantalum (Ta), tungsten (W), titanium (Ti), nickel (Ni), etc. When copper is used as the data conductor, the data conductor may be formed by etching the copper layer in the same manner as in the case of using copper as the gate conductor described above.

[0095] The planarization layer 180 may be located on the source electrode 173 and the drain electrode 175. The planarization layer 180 may include an organic insulating material or an inorganic insulating material.

[0096] The pixel electrode 191 is located on the planarization layer 180. The pixel electrode 191 is connected to the drain electrode 175 through a contact hole formed in the planarization layer 180 and receives a data signal therefrom. The portion including the layers from the substrate 110 to the pixel electrode 191 may be referred to as a transistor display panel or a thin film transistor display panel.

[0097] The pixel defining layer 360 is located on the planarization layer 180. The pixel defining layer 360 includes an opening overlapping the pixel electrode 191. The light emitting layer 370 is located on the pixel electrode 191 in the opening of the pixel defining layer 360, and the common electrode 270 is located on the light emitting layer 370. The pixel electrode 191, the light emitting layer 370 and the common electrode 270 form an organic light emitting diode (OLED). The pixel electrode 191 can be an anode of the organic light emitting diode, and the common electrode 270 can be a cathode of the organic light emitting diode. The common electrode 270 can include a transparent conductive material such as indium tin oxide (ITO), indium zinc oxide (IZO), etc. An encapsulation layer 390 protecting the organic light emitting diode is located on the common electrode 270.

[0098] Regarding the liquid crystal display panel 30 Fig.10 The gate line 121 and the gate electrode 124 of the transistor TR are located on the substrate 110, and the gate insulating layer 140 is located on the gate line 121 and the gate electrode 124. The semiconductor 151 and the semiconductor 154 of the transistor TR are located on the gate insulating layer 140, the data line 171 is located on the semiconductor 151, and the source electrode 173 and the drain electrode 175 are located on the semiconductor 154.

[0099] When the gate conductor including the gate line 121 and the gate electrode 124 is formed of copper, a copper layer is formed on the substrate 110 and etched by using the copper plasma etching method according to the above exemplary embodiment to form a gate conductor (which is a patterned copper layer). When the data conductor including the data line 171, the source electrode 173, and the drain electrode 175 is formed of copper, a copper layer is formed on the substrate 110 and etched by using the copper plasma etching method according to the above exemplary embodiment to form a data conductor (which is a patterned copper layer).

[0100] A planarization layer 180 is located on the data conductor, and a pixel electrode 191 is located on the planarization layer 180. The pixel electrode 191 is connected to the drain electrode 175 through a contact hole formed in the planarization layer 180 and receives a data signal therefrom. The portion including the layers from the substrate 110 to the pixel electrode 191 may be referred to as a transistor display panel or a thin film transistor display panel.

[0101] The liquid crystal layer 3 including the liquid crystal molecules 31 is located on the pixel electrode 191, and the insulating layer 210 sealing the liquid crystal layer 3 with the substrate 110 is located on the liquid crystal layer 3. The insulating layer 210 may be in the form of a substrate. The liquid crystal molecules 31 may be disposed apart from each other in the microcavity.

[0102] The common electrode 270 is disposed under the insulating layer 210 to generate an electric field in the liquid crystal layer 3 together with the pixel electrode 191, thereby controlling the alignment direction of the liquid crystal molecules 31. An alignment layer (not shown) may be disposed between the pixel electrode 191 and the liquid crystal layer 3 and between the liquid crystal layer 3 and the common electrode 270. The common electrode 270 may be disposed between the substrate 110 and the liquid crystal layer 3.

[0103] While the invention has been described in connection with what are presently considered to be practical exemplary embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but on the contrary, the invention is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.

Claims

1. A copper plasma etching method, include: placing a substrate including a conductive layer including copper on a susceptor in a processing chamber of a plasma etching apparatus; supplying an etching gas containing hydrogen chloride into the processing chamber; plasma etching the conductive layer comprising copper on the substrate; and maintaining the temperature of the susceptor at 10° C. or less during the plasma etching, The etching gas further includes H 2 gas, and the H 2 The flow rate ratio of gas to hydrogen chloride is 0.5 or less, The plasma etching is performed for 120 seconds to 300 seconds.

2. The copper plasma etching method according to claim 1, wherein the plasma etching comprises the following reaction stages: The first reaction stage: Cu+Cl→CuCl(s) The second reaction stage: CuCl+Cl→CuCl 2 (s) The third reaction stage: CuCl 2 +3H→CuH(g)+2HCl(g); 3CuCl 2 +3H→Cu 3 Cl 3 (g) + 3HCl(g); and <h2 style=";text-align:left;direction:ltr">3CuCl<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> +3 / 2H<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> →Cu<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> Cl<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> (g)+3HCl(g)。 3. The copper plasma etching method according to claim 1, in, In the plasma etching, the number of hydrogen radicals is greater than or equal to the number of chlorine radicals.

4. The copper plasma etching method according to claim 1, wherein the plasma etching is performed using plasma formed by an electron cyclotron resonance plasma source.

5. The copper plasma etching method of claim 1, wherein the plasma etching comprises reactive ion etching.

6. The copper plasma etching method according to claim 1, wherein the plasma etching is carried out at 10 -2 Support up to 10 -4 The process is carried out under the pressure of the support.

7. The copper plasma etching method according to claim 1, in, In the plasma etching, a photoresist mask is used as an etching mask.

8. A method for manufacturing a display panel, include: forming a conductive layer containing copper on a substrate; placing the substrate having the conductive layer formed thereon on a susceptor in a processing chamber of a plasma etching apparatus; supplying an etching gas containing hydrogen chloride into the processing chamber; plasma etching the conductive layer; as well as maintaining the temperature of the susceptor at 10° C. or less during the plasma etching, The etching gas further includes H 2 gas, and the H 2 The flow rate ratio of gas to hydrogen chloride is 0.5 or less, The plasma etching is performed for 120 seconds to 300 seconds.