A method for preparing a stabilizer for synthesizing polymer polyols

By reacting polyether polyol with TMI under nitrogen protection, combined with specific alcohol starting agents, epoxy compounds and catalysts, the problems of long reaction time and high viscosity in the prior art are solved, and process simplification is achieved and the improvement of dispersion effect, suitable for the synthesis of high solid content and low viscosity polymer polyols.

CN110283308BActive Publication Date: 2024-12-03NANJING JINQI CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910542928.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-06-21
Publication Date
2024-12-03
Estimated Expiration
2039-06-21

AI Technical Summary

Technical Problem

When the existing large monomer stabilizers synthesize high-solid polymer polyols, the reaction time is long and the process flow is complicated. The synthesized dispersant has a large viscosity, resulting in unsatisfactory dispersion effect and affecting the application of downstream products.

Method used

Under nitrogen protection, polyether polyols react with 3-isopropyl-dimethylbenzyl isocyanate (TMI) through specific polyfunctional alcohol starters, 1,2-epoxy compounds and catalysts In combination, the reaction conditions such as temperature and pressure are controlled to prepare a stabilizer with low viscosity.

Benefits of technology

The process flow is simplified, the product viscosity is reduced, and the dispersion effect is improved. It is suitable for the synthesis of polymer polyols with high solid content and low viscosity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a stabilizer for synthesizing polymer polyols, and the preparation method comprises the following steps: under nitrogen protection, polyether polyols react with 3-isopropyl-dimethylbenzyl isocyanate (TMI) to prepare a stabilizer, wherein the functionality of the polyether polyols is 3-8, and the molecular weight of the polyether polyols is 3000-14500. The novel stabilizer synthesized by the polyether polyols synthesized by the new process and the TMI isocyanate has the advantages of simple process, low viscosity, good dispersion effect, and can be used to synthesize polymer polyols (POPs) with high solid content and low viscosity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This patent relates to the technical field of high molecular polymer material preparation, specifically a method for preparing a stabilizer for synthesizing polymer polyols. Background Art

[0002] Most of the existing macromonomer stabilizers are produced by esterification of polyether polyols and maleic anhydride, and then end-capped with ethylene oxide (EO) or propylene oxide (PO) under the action of a catalyst. The reaction time is long, the process is complicated, and the viscosity of the synthesized dispersant is relatively high. When synthesizing polymer polyols with high solid content, the dispersion effect is not ideal, resulting in a high viscosity of the product, which affects the application of downstream products. Summary of the invention

[0003] In order to solve the above problems, the present invention discloses a method for preparing a stabilizer for synthesizing polymer polyols.

[0004] In order to achieve the above purpose, the present invention provides the following technical solutions:

[0005] The invention provides a method for preparing a stabilizer for synthesizing polymer polyols. The method comprises the following steps: under nitrogen protection, polyether polyol (functionality 3-8, molecular weight 3000-14500) is reacted with 3-isopropyl-dimethylbenzyl isocyanate (TMI) to prepare the stabilizer.

[0006] In the present invention, the preparation method of the polyether polyol is as follows: a multifunctional alcohol initiator and a 1,2-epoxy compound are catalyzed and synthesized by a catalyst A under reaction conditions to prepare the polyether polyol.

[0007] Furthermore, the multifunctional alcohol initiator includes one or more of glycerol, ethylene glycol, propylene glycol, trimethylolpropane, pentaerythritol, sorbitol, mannitol, sucrose, and xylitol.

[0008] Furthermore, the 1,2-epoxy compound includes one or more of ethylene oxide (ethylene oxide), propylene oxide (propylene oxide), 1,2-butylene oxide (butylene oxide), and 1,4-butylene oxide (tetrachlorofuran).

[0009] Furthermore, the catalyst A includes an alkaline catalyst and a bimetallic catalyst (DMC), wherein the alkaline catalyst includes sodium hydroxide, potassium hydroxide, potassium methoxide, and sodium methoxide.

[0010] Furthermore, the reaction conditions include appropriate reaction temperature conditions, reaction pressure conditions, and reaction environment adjustment, wherein the reaction temperature is 100-150° C., the reaction pressure is 0-0.5 MPa, and the reaction environment has an oxygen concentration of less than 80 ppm.

[0011] In the present invention, the preparation method of polyether polyol is specifically as follows:

[0012] The first step is the preparation of oligomers. The multifunctional alcohol initiator and the alkaline catalyst are added to the reaction vessel at room temperature, replaced with nitrogen and then evacuated. After evacuation, the temperature is raised to 100-120 degrees Celsius, and a single 1,2-epoxy compound is slowly added. The temperature in the kettle is maintained at 110-115±5°C and the pressure is 0.3±0.1MPa. After the 1,2-epoxy compound is added, the temperature is raised to 120-130 degrees Celsius again to continue the reaction until the reaction pressure is negative pressure. After the reaction is complete, the unreacted 1,2-epoxy compound is removed by vacuum, and then the reaction product is transferred to a refining kettle, and water, phosphoric acid, and a refining agent are added in sequence for refining. After dehydration after refining, it is filtered to obtain an oligomer.

[0013] The second step is the preparation of polyether. The oligomer and bimetallic catalyst (DMC) are added into the reaction vessel at room temperature. After replacing with nitrogen, the temperature is raised to 140-150 degrees Celsius. After evacuation, dehydration is carried out. The temperature is maintained at 140-150 degrees Celsius. Two or more mixed 1,2-epoxide compounds are slowly added in batches to induce continued reaction. The temperature in the kettle is maintained at 125-135 degrees Celsius and the pressure is less than 0.05 MPa. After all the mixed 1,2-epoxide compounds are added, the temperature is raised to 140 degrees Celsius to continue the reaction until the pressure is negative. The unreacted 1,2-epoxide compounds are removed in vacuo to obtain polyether.

[0014] In the present invention, the molar ratio of the polyether polyol to TMI is 1:0.3-1:0.8.

[0015] In the present invention, under nitrogen protection, the reaction temperature of polyether polyol (functionality 3-8, molecular weight 3000-14500) and 3-isopropyl-dimethylbenzyl isocyanate (TMI) is 65-120°C.

[0016] In the present invention, under nitrogen protection, the catalyst used in the reaction of polyether polyol (functionality 3-8, molecular weight 3000-14500) with 3-isopropyl-dimethylbenzyl isocyanate (TMI) is an organic metal salt catalyst, and the organic metal salt catalyst includes stannous octoate and dibutyltin dilaurate.

[0017] In the present invention, the prepared stabilizer has a colorless and transparent appearance and a viscosity of 1000-3000 (mPa·s / 25°C).

[0018] The present invention has the following beneficial effects:

[0019] 1. Synthesis of polyether polyols for preparing stabilizers; 2. Preparation of the stabilizer. 3. Synthesis of polyether polyols: selection of appropriate alcohol initiators (i.e., functionality), ratio of 1,2-epoxide compounds, determination of reaction conditions. 4. Preparation of stabilizers: amount of catalyst, ratio of polyether and TMI, reaction temperature.

[0020] The new stabilizer synthesized by the polyether polyol synthesized by the new process and combined with TMI isocyanate has the advantages of simple process, low viscosity, good dispersion effect, and can be used to synthesize polymer polyols (POP) with high solid content and low viscosity. DETAILED DESCRIPTION

[0021] The present invention will be further explained below in conjunction with specific implementation modes. It should be understood that the following specific implementation modes are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0022] Example 1

[0023] 1. Synthesis of polyether polyols

[0024] A. Weigh 363g of solid sorbitol, 90g of glycerol and 10g of potassium hydroxide, add them into a 5L high-pressure reactor at room temperature, replace with nitrogen for 5 times, detect the oxygen content of 67ppm, evacuate to ≤-0.097MPa, after evacuation, heat to 110℃, slowly introduce 3547g of propylene oxide (PO), maintain the temperature in the reactor at 110±5℃ and the pressure at 0.3±0.1MPa, heat to 120℃ and continue the reaction until the pressure in the reactor is negative pressure, remove the unreacted propylene oxide (PO) in vacuum, transfer to a refining reactor for post-treatment, add 160g of water, 19g of 85% phosphoric acid, 60g of 600 # Refining preparation, and then dehydrating to the qualified water content (<0.05%). Then filter and test the polyether index to obtain oligomer a. Put it into barrels for later use. Index analysis: hydroxyl value 209.2mgKOH / g, water content 0.03%.

[0025] B. Weigh 536g of oligomer a and 0.2g of DMC, add them to a 5L autoclave at room temperature, replace with nitrogen 5 times, detect the oxygen content of 63ppm, then heat to 140℃, vacuum dehydrate for 2h, maintain the temperature at 140℃, slowly introduce an appropriate amount of pre-mixed mixture of propylene oxide (PO) (3083g) and ethylene oxide (EO) (381g) for induction, after the induction reaction, maintain the temperature in the autoclave at 125-135℃, pressure <0.05MPa, and heat to 140℃ after the remaining mixture is passed to continue the reaction until the pressure of the autoclave is negative pressure, vacuum remove the unreacted propylene oxide (PO) and ethylene oxide (EO), obtain the finished polyether a, and detect the analysis indicators. Index analysis: hydroxyl value 28.17mgKOH / g, moisture 0.03%, viscosity 2013 mPa·s / 25℃.

[0026] 2. Preparation of stabilizer

[0027] At room temperature, 2000g of polyether a, 25.79g of TMI and 0.075g of stannous octoate were weighed and added to a reaction kettle. After nitrogen replacement, a slight positive pressure was maintained in the kettle, and then the temperature was slowly raised to 65°C, kept warm for 2h, cooled and discharged to obtain stabilizer a.

[0028] Example 2

[0029] A. Weigh 521g of pentaerythritol and 12g of potassium hydroxide, add them to a 5L high-pressure reactor at room temperature, replace with nitrogen 5 times, detect the oxygen content of 62ppm, evacuate to ≤-0.097 MPa, then introduce 70g of PO, heat to 110℃, and slowly introduce 3409g of PO when the pressure in the reactor drops significantly, keep the temperature in the reactor at 110±5℃, and the pressure at 0.3±0.1MPa. After the introduction, heat to 120℃ and continue the reaction until the pressure in the reactor is negative pressure, vacuum remove the unreacted propylene oxide (PO), transfer to the refining reactor for post-treatment, add 160g of water, 19g of 85% phosphoric acid, and 60g of 600# refining agent in sequence, and then dehydrate until the water content is qualified (<0.05%). Then filter and test the polyether index to obtain oligomer b. Put it into barrels for later use. Index analysis: hydroxyl value 216.1mgKOH / g, moisture 0.02%.

[0030] B. Weigh 415g of oligomer b and 0.2g of DMC, add them to a 5L autoclave at room temperature, replace with nitrogen 5 times, detect the oxygen content of 59ppm, heat to 140℃, vacuum dehydrate for 2h, maintain the temperature at 140℃ after completion, slowly pass in an appropriate amount of a pre-mixed mixture of PO (3011g) and EO (574g) for induction, and after the induction reaction, maintain the temperature in the autoclave at 125-135℃ and the pressure <0.05MPa. After passing the remaining mixture, heat to 140℃ and continue the reaction until the pressure in the autoclave is negative pressure, vacuum remove the unreacted propylene oxide (PO) and ethylene oxide (EO), and obtain the finished polyether b, and test the analysis indicators. Index analysis: hydroxyl value 21.8mgKOH / g, moisture 0.03%, viscosity 2245 mPa·s / 25℃.

[0031] 2. Preparation of stabilizer

[0032] At room temperature, 2000g of polyether b, 21.5g of TMI and 0.05g of dibutyltin dilaurate were weighed and added to the reaction kettle. After nitrogen replacement, the kettle was kept at a slight positive pressure, and then the temperature was slowly raised to 80°C, kept at this temperature for 2h, and then cooled and discharged to obtain stabilizer b. Index analysis: viscosity 2601 mPa·s / 25°C

[0033] Example 3

[0034] A. Weigh 485g of solid sorbitol and 12g of potassium hydroxide, add them to a 5L high-pressure reactor at room temperature, replace with nitrogen 5 times, detect the oxygen content of 58ppm, evacuate to ≤-0.097 MPa, and after evacuation, heat up to 120℃, slowly pass 3547g of PO, maintain the temperature in the reactor at 115±5℃, and the pressure at 0.3±0.1MPa. After passing, heat up to 125℃ and continue to react until the pressure in the reactor is negative pressure. Vacuum remove unreacted propylene oxide (PO), transfer to the refining reactor for post-treatment after detection, add 160g of water, 22.8g of 85% phosphoric acid, and 60g of 600# refining agent in turn, and then dehydrate until the water content is qualified (<0.05%). Then filter and test the polyether index to obtain oligomer c. Barrel for use. Index analysis: hydroxyl value 225.1mgKOH / g, water content 0.03%.

[0035] B. Weigh 498g of oligomer c and 0.2g of DMC, add them to a 5L autoclave at room temperature, replace with nitrogen 5 times, detect the oxygen content of 61ppm, then heat to 140℃, vacuum dehydrate for 2h, maintain the temperature at 140℃ after the end, slowly pass in an appropriate amount of pre-mixed PO (2942g) and EO (560g) mixture for induction, after the induction reaction, maintain the temperature in the autoclave at 125-135℃, pressure <0.05MPa, and heat to 140℃ after passing the remaining mixture to continue the reaction until the pressure of the autoclave is negative pressure, vacuum remove unreacted propylene oxide (PO) and ethylene oxide (EO), obtain the finished polyether c, and detect and analyze the indicators. Indicator analysis: hydroxyl value 28.17mgKOH / g, moisture 0.03%, viscosity 2489 mPa·s / 25℃.

[0036] 2. Preparation of stabilizer

[0037] 2000g polyether a, 19.4g TMI and 0.03g stannous octoate were weighed and added to the reactor at room temperature. After nitrogen replacement, the reactor was kept at a slight positive pressure, and then the temperature was slowly raised to 100°C, kept for 2h, cooled and discharged to obtain stabilizer c. Index analysis: viscosity 2973 mPa·s / 25°C.

[0038] Of course, in other embodiments, in step A, the multifunctional alcohol initiator used may also be one of glycerol, ethylene glycol, propylene glycol, trimethylolpropane, pentaerythritol, sorbitol, mannitol, sucrose, and xylitol, a mixture of two or a mixture of three or more. The alkaline catalyst is one of sodium hydroxide, potassium hydroxide, potassium methoxide, and sodium methoxide.

[0039] Of course, in other embodiments, in step A, the 1,2-epoxy compound used is one of ethylene oxide, propylene oxide, 1,2-butylene oxide, and 1,4-butylene oxide; in step B, the 1,2-epoxy compound used can be ethylene oxide and 1,2-butylene oxide, or ethylene oxide and 1,4-butylene oxide, that is, the 1,2-epoxy compound is one or more of ethylene oxide, propylene oxide, 1,2-butylene oxide, and 1,4-butylene oxide.

[0040] The technical means disclosed in the scheme of the present invention are not limited to the technical means disclosed in the above-mentioned implementation mode, but also include technical schemes composed of any combination of the above-mentioned technical features. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also regarded as the protection scope of the present invention.

Claims

1. A method for preparing a stabilizer for synthesizing polymer polyols, characterized in that: The preparation method comprises the following steps: under the protection of nitrogen, polyether polyol reacts with 3-isopropyl-dimethylbenzyl isocyanate to prepare a stabilizer, wherein the pressure of the nitrogen is slightly positive; The preparation method of the polyether polyol is as follows: a multifunctional alcohol initiator and a 1,2-epoxy compound are catalyzed and synthesized by a catalyst A under reaction conditions to prepare the polyether polyol; The preparation method of polyether polyol is specifically as follows: The first step is the preparation of oligomers. The multifunctional alcohol initiator and the alkaline catalyst are added to a reaction vessel at room temperature, replaced with nitrogen and then evacuated. After evacuation, the temperature is raised to 100-120° C., and a single 1,2-epoxy compound is slowly added. The temperature in the kettle is maintained at 115±5° C. and the pressure is 0.3±0.1 MPa. After the 1,2-epoxy compound is added, the temperature is raised to 120-130° C. again to continue the reaction until the reaction pressure is negative pressure. After the reaction is complete, the unreacted 1,2-epoxy compound is removed by vacuum, and then the reaction product is transferred to a refining kettle, and water, phosphoric acid, and a refining agent are added in sequence for refining. After the refining is completed, it is dehydrated and filtered to obtain an oligomer. The second step is the preparation of polyether. The oligomer and the bimetallic catalyst are added to the reaction vessel at room temperature, replaced with nitrogen and heated to 140°C-150°C. After vacuuming, dehydration is carried out, and the temperature is maintained at 140°C-150°C. Two or more mixed 1,2-epoxy compounds are slowly added in batches to induce continued reaction. The temperature in the kettle is maintained at 125-135°C and the pressure is less than 0.05MPa. After all the mixed 1,2-epoxy compounds are added, the temperature is raised to 140°C and the reaction is continued until the pressure is negative pressure. The unreacted 1,2-epoxy compounds are removed in vacuo to obtain polyether. The multifunctional alcohol initiator includes one or more of glycerol, ethylene glycol, propylene glycol, trimethylolpropane, pentaerythritol, sorbitol, mannitol, sucrose, and xylitol; The functionality of the polyether polyol is 4-6, and the hydroxyl value of the polyether polyol is 21.8 mgKOH / g and 28.17 mgKOH / g; The molecular weight of the polyether polyol is 3000-14500; The stabilizer has a colorless and transparent appearance and a viscosity of 1000-3000 mPa·s / 25°C; The molar ratio of the polyether polyol to 3-isopropyl-dimethylbenzyl isocyanate is 1:0.3-1:0.

8.

2. The method for preparing a stabilizer for synthesizing polymer polyols according to claim 1, characterized in that: The 1,2-epoxy compound includes one or more of ethylene oxide, propylene oxide, 1,2-butylene oxide, and 1,4-butylene oxide.

3. The method for preparing a stabilizer for synthesizing polymer polyols according to claim 1, characterized in that: The catalyst A comprises an alkaline catalyst and a bimetallic catalyst, wherein the alkaline catalyst is selected from sodium hydroxide, potassium hydroxide, potassium methoxide, and sodium methoxide.

4. The method for preparing a stabilizer for synthesizing polymer polyols according to claim 1, characterized in that: The reaction conditions include a suitable reaction environment, wherein the reaction environment has an oxygen concentration of less than 80 ppm.

5. The method for preparing a stabilizer for synthesizing polymer polyols according to claim 1, characterized in that: Under nitrogen protection, the reaction temperature of the polyether polyol and 3-isopropyl-dimethylbenzyl isocyanate is 65-100° C. The catalyst used in the reaction of the polyether polyol and 3-isopropyl-dimethylbenzyl isocyanate is an organic metal salt catalyst, which is selected from stannous octoate and dibutyltin dilaurate.