Solid aluminum profile flatness shaping method and shaping device

By adjusting the flatness by zoning water spray cooling when the aluminum profile is extruded from the mold, the bending deformation problem of solid aluminum profiles caused by stress and temperature changes is solved, an efficient and damage-free shaping effect is achieved, and the shaping quality and efficiency are improved.

CN110695119BActive Publication Date: 2024-10-29JIANGSU ZHONGFU ALUMINUM MAGNESIUM TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201911132936.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-11-19
Publication Date
2024-10-29
Estimated Expiration
2039-11-19

AI Technical Summary

Technical Problem

Flat solid aluminum profiles are prone to bending and deformation due to stress and temperature changes after extrusion, resulting in flatness that does not meet design requirements. Existing shaping methods are inefficient and easily damage the surface.

Method used

When the aluminum profile is extruded from the extrusion die, the flatness is adjusted through water spray cooling in different zones. Different water spray flow rates are used to achieve cooling speed differences, resulting in stress differences, and then the flatness required by the design is achieved through deformation compensation.

Benefits of technology

It achieves efficient shaping without damaging the surface of aluminum profiles, simplifies the shaping process, improves shaping quality and efficiency, and ensures that the flatness meets the design requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110695119B_ABST
    Figure CN110695119B_ABST
Patent Text Reader

Abstract

The present invention relates to a shaping method for aluminum profiles, in particular to a flatness shaping method for solid aluminum profiles, wherein one of the flat side surfaces of the aluminum profile is partitioned for water spray cooling, the partitions are no less than two, the partitions are divided along the width direction of the flat side surface of the aluminum profile, each partition is individually sprayed with water for cooling, the water spray flow rate of each partition is different, and the water spray cooling is located at the discharge end of the aluminum profile extrusion die. The solid aluminum profile flatness shaping method provided by the present invention is cooled when the aluminum profile is extruded into the die, and the flatness of the aluminum profile is adjusted by different cooling speeds of different partitions. The shaping method is simple, the shaping effect is good, and the surface of the aluminum profile will not be damaged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a shaping method for aluminum profiles, in particular to a flatness shaping method and a shaping device for solid aluminum profiles. Background Art

[0002] Flat aluminum profiles are wide and thin, similar to long strips of aluminum plates. Flat aluminum profiles include hollow and solid ones. Flat solid aluminum profiles are prone to deformation due to stress and temperature changes after being extruded from the mold. Flat surfaces are prone to bowing after leaving the mold. Such deformation is consistent and bends in the same direction. The deformation causes the flatness to fail to meet the design requirements.

[0003] At present, the main method used is post-shaping, that is, the aluminum profile is shaped after leaving the extrusion equipment and completely cooling down. During shaping, the flatness is first detected, and the parts that need shaping are marked. Then, the profile is placed on the fixture and shaped by extrusion or knocking. Due to the long length of the aluminum profile, usually 4-8 meters, the shaping workload is large, and the shaping process relies on the experience of the operator, resulting in low shaping efficiency. Sometimes over-shaping occurs, and reverse shaping is required. The overall shaping quality is not good. In the entire shaping process, the surface of the aluminum profile needs to be contacted with a ruler for multiple flatness tests, as well as extrusion and knocking, which makes it easy to scratch the surface of the aluminum profile. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a solid aluminum profile flatness shaping method which is cooled during aluminum profile extrusion die extrusion and adjusts the flatness of the aluminum profile by different cooling rates of different partitions. The shaping method is simple, the shaping effect is good, and the surface of the aluminum profile will not be damaged. The specific technical scheme is as follows:

[0005] A method for flatness shaping of a solid aluminum profile comprises spraying water to cool a flat side of the aluminum profile, wherein the partitions are no less than two and are divided along the width direction of the flat side of the aluminum profile. Each partition is sprayed with water to cool the flat side of the aluminum profile separately, and the water spray flow rate of each partition is different. The water spray cooling is located at the discharge end of the aluminum profile extrusion die.

[0006] By adopting the above technical solution, the temperature of the aluminum profile after being extruded from the mold is relatively high, reaching above 400-500℃. Spraying water on the aluminum profile will quickly cool down the aluminum profile. Rapid cooling causes drastic changes in the stress inside the aluminum profile. Since it is a solid flat aluminum profile, the stress change will cause the wide side to change. The different water spray flow rates of each partition result in different cooling speeds. A large flow rate per unit time leads to a fast cooling speed, and the aluminum profile temperature drops quickly. A small flow rate leads to a slow cooling speed, and the aluminum profile cools slowly. A temperature difference occurs between the partitions, and the temperature difference leads to different stresses. Therefore, different cooling speeds lead to different stresses, and different stresses lead to different deformations of each partition. Different deformations achieve different compensations, so that the flatness meets the design requirements after compensation. The flow rate of each partition is set based on the test data before the cooling method is used for shaping. The specific data corresponding to the flow rate and deformation can be obtained through experiments.

[0007] The partitioning along the width direction refers to the division according to the deformation compensation range formed by spraying water on the side of the aluminum profile. If a partition line is set, the partition line extends along the length direction of the aluminum profile and is divided along the width direction.

[0008] Different water spray flow rates are used to achieve different cooling rates.

[0009] Furthermore, the water spraying direction is perpendicular to the flat side surface of the aluminum profile or is inclined along the length direction of the aluminum profile.

[0010] Furthermore, the water spray of each partition is located in the same cross-section.

[0011] By adopting the above technical solution, the cross section refers to the surface perpendicular to the length direction of the aluminum profile. Cooling is performed in the same cross section so that the cooling deformation is located in the same cross section, which can ensure the consistency of the deformation speed and avoid the mutual influence caused by the asynchronous cooling of each partition. That is, cooling in the same cross section will lead to a sequence of cooling deformation, and the later cooling deformation will affect the earlier cooling deformation. Although controlling the cooling speed through experimental data can eliminate the influence of inconsistent cooling, adjusting the flow rate is complicated and requires more experimental data.

[0012] Another object of the present invention is to provide a solid aluminum profile flatness shaping device, including a water spray pipe, no less than two of the water spray pipes, the water spray pipes being located on one side of the flat side of the aluminum profile, and the water spray pipes being distributed along the width direction of the flat side of the aluminum profile, the water spray pipes being located at the discharge end of the aluminum profile extrusion die, the water spray pipes being used to spray cooling water onto the flat side of the aluminum profile for zoned water spray cooling; valves, the number of the valves being consistent with the number of the water spray pipes, the valves being connected to each of the water spray pipes respectively, the valves being used to control the switch and flow regulation of the water spray pipes; a water pump, the valves being connected to the water pump; and a cooling water trough, the cooling water trough being filled with cooling water, the water pump being connected to the cooling water trough.

[0013] By adopting the above technical solution, the water pump presses the cooling water in the cooling water tank into the water spray pipe, and the water spray pipe sprays the cooling water onto the side of the aluminum profile for cooling.

[0014] The water spray pipes are distributed along the width direction of the flat side of the aluminum profile to partition the flat side of the aluminum profile.

[0015] The valve can be a ball valve followed by a gate valve. The valve can control the flow rate, thereby controlling the flow rate of each water spray pipe to achieve different cooling speeds.

[0016] Furthermore, it also includes a float flowmeter, the number of which is consistent with the water spray pipes, the float flowmeter is installed between the water spray pipes and the water pump, and the float flowmeter is used to display the flow of each water spray pipe.

[0017] By adopting the above technical solution, the float flowmeter is used to cooperate with the valve to accurately control the flow, thereby achieving high-precision regulation and improving the accuracy and effect of shaping.

[0018] Furthermore, the water spray pipes are arranged side by side.

[0019] Furthermore, a temperature sensor is installed on the water spray pipe, and the temperature sensor is used to detect the temperature of the sprayed water.

[0020] By adopting the above technical solution, the temperature sensor can use PT100 or thermocouple to monitor the temperature of cooling water and avoid the influence of large fluctuation of cooling water temperature on shaping.

[0021] Furthermore, the cooling water tank is a constant temperature water tank.

[0022] By adopting the above technical solution, the constant temperature water tank ensures deformation stability, reduces the influence of temperature on shaping, improves the stability of shaping, and ensures the shaping effect.

[0023] Furthermore, it also includes a nozzle, which is fixed at the water outlet end of the water spray pipe.

[0024] By adopting the above technical solution, the nozzle can adjust the shape of the sprayed water flow.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The solid aluminum profile flatness shaping method provided by the present invention cools the aluminum profile when it is extruded through a die, and adjusts the flatness of the aluminum profile by different cooling rates of different partitions. The shaping method is simple, the shaping effect is good, and the surface of the aluminum profile will not be damaged. The solid aluminum profile flatness shaping device provided by the present invention has a simple structure, good shaping effect, and is easy to use. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a front view of a solid aluminum profile flatness shaping device;

[0028] Figure 2 is a side view of a solid aluminum profile flatness shaping device;

[0029] Figure 3 It is a schematic diagram of zone cooling, and the arrows in the figure indicate the direction of movement of the aluminum profile. DETAILED DESCRIPTION

[0030] The present invention will be further described with reference to the accompanying drawings.

[0031] A method for flatness shaping of a solid aluminum profile comprises spraying water to cool one of the flat side partitions of the aluminum profile 2, wherein the partitions are no less than two and are divided along the width direction of the flat side of the aluminum profile 2. Each partition is sprayed with water to cool it separately, and the water spray flow rate of each partition is different. The water spray cooling is located at the discharge end of the extrusion die 11 of the aluminum profile 2.

[0032] Different water spray flow rates are used to achieve different cooling rates.

[0033] After the aluminum profile 2 is extruded from the die 11, the temperature is high, reaching above 400-500°C. Spraying water on the aluminum profile 2 will cause the aluminum profile 2 to cool down quickly. The rapid cooling causes the stress inside the aluminum profile 2 to change dramatically. Since it is a solid flat aluminum profile 2, the stress change will cause the flatness of the side with a large width to change. The different water spraying flow rates of each partition result in different cooling speeds. The larger the flow rate per unit time, the faster the cooling speed, and the faster the temperature of the aluminum profile 2 decreases. The smaller the flow rate per unit time, the slower the cooling speed, and the slower the cooling of the aluminum profile 2. A temperature difference occurs between the partitions, and the temperature difference causes different stresses. Therefore, different cooling speeds result in different stresses, and different stresses result in different deformations of each partition. Different deformations achieve different compensations, so that the flatness of the flat side of the aluminum profile 2 meets the design requirements of flatness after compensation. The flow rate of each partition is set based on the test data before the cooling method is used for shaping. The specific data corresponding to the flow rate and deformation can be obtained through experiments.

[0034] like Figure 3 As shown, dividing the partitions along the width direction refers to dividing the deformation compensation range according to the effective cooling range formed by spraying water on the side of the aluminum profile. If a partition line 21 is set, the partition line 21 extends along the length direction of the aluminum profile 2 and is divided along the width direction.

[0035] The direction of the water spray is perpendicular to the flat side of the aluminum profile 2 or is inclined along the length direction of the aluminum profile 2. The water spray of each partition is located in the same cross section.

[0036] The cross section refers to the surface perpendicular to the length direction of the aluminum profile 2. Cooling in the same cross section makes the cooling deformation in the same cross section, which can ensure the consistency of deformation speed and avoid the mutual influence caused by the asynchronous cooling of each partition. That is, cooling in different cross sections will lead to cooling deformation in sequence, and the later cooling deformation will affect the earlier cooling deformation. Although controlling the cooling speed through experimental data can eliminate the influence of inconsistent cooling, adjusting the flow rate is complicated and requires more experimental data.

[0037] Embodiment 1

[0038] like Figures 1 to 3As shown, the solid aluminum profile flatness shaping device includes a water spray pipe 13, there are no less than two water spray pipes 13, the water spray pipe 13 is located on one side of the flat side of the aluminum profile 2, and the water spray pipe 13 is distributed along the width direction of the flat side of the aluminum profile 2, the water spray pipe 13 is located at the discharge end of the aluminum profile 2 extrusion die 11, the water spray pipe 13 is used to spray cooling water onto the flat side of the aluminum profile 2 for zoned water spray cooling; valves 4, the number of valves 4 is consistent with the water spray pipe 13, the valves 4 are respectively connected to each water spray pipe 13, the valves 4 are used to control the switch and flow regulation of the water spray pipe 13; water pump 6, the valves 4 are all connected to the water pump 6; and a cooling water tank, the cooling water tank is filled with cooling water, and the water pump 6 is connected to the cooling water tank.

[0039] The water pump 6 presses the cooling water in the cooling water tank into the water spray pipe 13, and the water spray pipe 13 sprays the cooling water onto the side of the aluminum profile 2 for cooling.

[0040] The water spray pipes 13 are distributed along the width direction of the flat side of the aluminum profile 2 to realize the partitioned water spray cooling of the flat side of the aluminum profile 2. The water spray pipes 13 are arranged side by side. The water spray pipes 13 are fixed on the water pipe fixing plate 7. The fixing plate 7 is provided with waist-shaped holes to facilitate the adjustment of the positions of each water spray pipe 13.

[0041] The valve 4 can be a ball valve followed by a gate valve, and the valve 4 can control the size of the flow rate, thereby controlling the flow rate of each water spray pipe 13 to achieve different cooling speeds. The valve 4 can also close the water spray pipe 13 as needed.

[0042] The cooling water tank can be a cooling water tower, which provides cooling water. The cooling water tower cools down the high-temperature water after spray cooling, so that the cooling water can be recycled.

[0043] Embodiment 2

[0044] On the basis of the above-mentioned embodiment 1, a float flowmeter 4 is further included. The number of the float flowmeters 4 is consistent with the number of the water spray pipes 13. The float flowmeter 4 is installed between the water spray pipes 13 and the water pump 6. The float flowmeter 4 is used to display the flow of each water spray pipe 13. The float flowmeter 4 is used to cooperate with the valve 4 to accurately control the flow, thereby achieving high-precision regulation and improving the accuracy and effect of shaping.

[0045] Embodiment 3

[0046] On the basis of the above-mentioned embodiment 1 or embodiment 2, a temperature sensor is installed on the water spray pipe 13, and the temperature sensor is used to detect the temperature of the spray water. The cooling water tank is a constant temperature water tank.

[0047] The temperature sensor can be PT100 or thermocouple to monitor the temperature of cooling water to avoid the influence of large fluctuation of cooling water temperature on shaping. The constant temperature water tank ensures the stability of deformation, reduces the influence of temperature on shaping, improves the stability of shaping, and ensures the shaping effect.

[0048] The constant temperature water tank is a prior art, and the cooling water sent from the cooling tower can be further cooled by adding refrigeration equipment to ensure that the water temperature entering the water spray pipe 13 is stable.

[0049] Embodiment 4

[0050] On the basis of any of the above embodiments, a nozzle is further included, and the nozzle is fixed at the water outlet end of the water spray pipe 13. The nozzle can adjust the shape of the sprayed water flow.

[0051] During operation, the aluminum profile 2 is extruded from the mold 11, and then passes through the bottom roller 14 and the side roller 13 into the cooling box 12. The water spray pipe 13 is located between the mold 11 and the cooling box 12 and is close to the mold 11. The water spray pipe 13 sprays water upward from the bottom, and the water flow impacts the flat side of the aluminum profile 2. The water flow cools the flat side of the aluminum profile 2. The flow of each valve 4 is adjusted according to the experimental data or the flatness detected on site, and the float flowmeter 4 is observed for precise adjustment.

Claims

1. A solid aluminum profile flatness shaping method, which is achieved by means of a solid aluminum profile flatness shaping device, characterized in that: Spray water for cooling one of the flat side surfaces of the aluminum profile, the partitions are no less than two, the partitions are divided along the width direction of the flat side surface of the aluminum profile, each partition is sprayed with water for cooling separately, the spray flow rate of each partition is different, and the water spray cooling is located at the discharge end of the aluminum profile extrusion die; The direction of the water spray is perpendicular to the flat side of the aluminum profile or inclined along the length direction of the aluminum profile; The water spray of each partition is located in the same cross section; The partitioning along the width direction refers to the division according to the deformation compensation range formed by the effective temperature reduction range formed by spraying water on the side of the aluminum profile. A partition line is provided on the aluminum profile, and the partition line extends along the length direction of the aluminum profile and is divided along the width direction; The flow rate of each of the divided areas is set according to the detection data of the specific deformation amount of each of the divided areas when the aluminum profile is not cooled by water; The solid aluminum profile flatness shaping device comprises: A water spray pipe, wherein there are no less than two water spray pipes, the water spray pipes are located on one side of the flat side of the aluminum profile, and the water spray pipes are distributed along the width direction of the flat side of the aluminum profile, the water spray pipes are located at the discharge end of the aluminum profile extrusion die, and the water spray pipes are used to spray cooling water onto the flat side of the aluminum profile for zoned water spray cooling; Valves, the number of which is the same as the number of water spray pipes, the valves are connected to each water spray pipe respectively, and the valves are used to control the switch and flow rate of the water spray pipes; A water pump, and the valves are all connected to the water pump; and A cooling water tank, wherein cooling water is contained in the cooling water tank, and the water pump is connected to the cooling water tank; It also includes a float flowmeter, the number of which is consistent with the number of water spray pipes, the float flowmeter is installed between the water spray pipe and the water pump, and the float flowmeter is used to display the flow of each water spray pipe; The water spray pipes are arranged side by side; A temperature sensor is mounted on the water spray pipe.

2. The solid aluminum profile flatness shaping method according to claim 1, characterized in that: The cooling water tank is a constant temperature water tank.

3. The solid aluminum profile flatness shaping method according to claim 1, characterized in that: It also includes a spray head, which is fixed at the water outlet end of the spray pipe.

Citation Information

Patent Citations

  • Solid aluminum profile flatness shaping device

    CN210995859U

  • Extrusion molding apparatus and control method thereof

    KR101329555B1

  • KR1017469840000B1