A multilayer ceramic capacitor and a method for preparing the same

By setting a combined reinforcement body of a high-strength material layer and a ceramic dielectric layer on the effective electrode layer of a multi-layer ceramic capacitor, the problem of insufficient strength of the ceramic dielectric material is solved, the flexural and bending strength of the capacitor is improved, and the application field is broadened. And reduces production costs and complexity.

CN110867321BActive Publication Date: 2024-11-29SHENZHEN THREE-CIRCLE ELECTRONICS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201911224000.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-02
Publication Date
2024-11-29
Estimated Expiration
2039-12-02

AI Technical Summary

Technical Problem

Existing multi-layer ceramic capacitors are prone to break due to vibration, welding or temperature fluctuations due to low strength of ceramic dielectric materials. Existing solutions such as the use of precious metal soft terminals or metal shrapnels increase costs and production complexity, and do not meet the conditions for mass production. .

Method used

Using a combination of a high-strength material layer and a ceramic dielectric layer, by setting multiple reinforcement units on the surface and inside of the effective electrode layer, high-strength materials such as zirconia, alumina, calcium zirconate, etc., pass the secondary The casting or screen printing process is evenly distributed to improve the flexural strength and bending strength of the capacitor.

Benefits of technology

The flexural strength and bending strength of multi-layer ceramic capacitors are significantly improved, meeting the needs of high-strength applications, broadening the use field, and reducing sintering stress by controlling the material thickness ratio and process parameters, and avoiding cracking problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110867321B_ABST
    Figure CN110867321B_ABST
Patent Text Reader

Abstract

The present invention discloses a multilayer ceramic capacitor, comprising an effective electrode layer and a reinforcement body, wherein the reinforcement body is arranged at least one of the upper surface of the effective electrode layer, the interior of the effective electrode layer and the lower surface of the effective electrode layer; the two end faces of the effective electrode layer and the reinforcement body are in contact with the end electrode; the reinforcement body is formed by stacking a plurality of reinforcement body units; the reinforcement body unit comprises a high-strength material layer and a ceramic dielectric layer, and the strength of the main material of the high-strength material layer is greater than the strength of the main material of the ceramic dielectric layer. The multilayer ceramic capacitor of the present invention is provided with a high-strength material layer uniformly distributed in the ceramic dielectric layer of the MLCC, which greatly improves the flexural strength and bending strength of the MLCC while ensuring the original electrical properties of the capacitor. The present invention also discloses a method for preparing a multilayer ceramic capacitor, which adopts a secondary casting or screen printing process to realize the distribution of the reinforcement material in the conventional dielectric layer, and can realize a more accurate and reasonable preparation of the reinforcement body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a capacitor and a preparation method thereof, and in particular to a high-strength multilayer ceramic capacitor and a preparation method thereof. Background Art

[0002] Multilayer ceramic capacitors are mainly divided into two categories, Class I high-frequency ceramic capacitors and Class II high-dielectric ceramic capacitors. Among them, Class II high-dielectric ceramic capacitors are prone to vibration during use, such as welding, board separation, or stress or temperature fluctuations, resulting in their breakage due to the low strength of the ceramic dielectric material used in them.

[0003] To solve the above problems, at this stage, flexible terminals or welded metal springs are used to reduce stress and improve the problem of breakage caused during product use. Among them, the use of precious metal soft terminal design is to add a layer of flexible precious metal and conductive resin material to the end of the product, so that when the product is subjected to external force or vibration, the flexible material at the end is slightly plastically deformed to absorb stress and protect the product from breaking. This solution has the following disadvantages: 1) The cost of precious metal resin slurry is relatively high, and it is prone to problems such as poor electroplating and tinning; 2) The drying and co-firing technology of flexible terminals requires fineness, which generally increases the loss value of the product; 3) Product production increases the operating process, which has a certain impact on the product production cycle and cost.

[0004] The design of welding metal springs at the product end is similar to the principle of flexible end. The elastic deformation of the metal springs is set to absorb the external stress to protect the product. This solution has the following disadvantages: 1) Increase the material and production costs of the metal springs, reducing market competitiveness; 2) The operability and production automation are not high, and the conditions for mass production are not met; 3) Product production increases the operating process, which has a certain impact on the product production cycle and cost. Summary of the invention

[0005] The object of the present invention is to overcome the deficiencies of the prior art and provide a high-strength multilayer ceramic capacitor and a preparation method thereof.

[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a multilayer ceramic capacitor, including an effective electrode layer and a reinforcement body, wherein the reinforcement body is arranged at least one of the upper surface of the effective electrode layer, the inside of the effective electrode layer and the lower surface of the effective electrode layer; the reinforcement body is formed by stacking a plurality of reinforcement body units; the reinforcement body unit includes a high-strength material layer and a ceramic dielectric layer; the material of the high-strength material layer contains a high-strength material, and the strength of the main material of the high-strength material layer is greater than the strength of the main material of the ceramic dielectric layer.

[0007] The reinforcement body used in the present invention can significantly improve the strength defects of the multilayer ceramic capacitor material itself, and greatly improve the flexural strength and bending strength of the multilayer ceramic capacitor while ensuring the original electrical properties of the capacitor. The flexural strength of the multilayer ceramic capacitor of the present invention can be made ≥10kgf; the bending strength value is ≥7mm, which broadens the application field of MLCC products. The multilayer ceramic capacitor of the present invention can be widely used in electronic and electrical products. As a conventional passive electronic component, the multilayer ceramic capacitor can be used in energy-saving lamps, vehicle-mounted electronic appliances (such as car navigation, driving recorders, vehicle-mounted audio, etc.), and other fields with relatively high requirements on product strength due to its higher strength.

[0008] Preferably, the reinforcement is arranged on the upper surface of the effective electrode layer and the lower surface of the effective electrode layer. The reinforcement is arranged on the upper and lower surfaces of the effective electrode layer of the multilayer ceramic capacitor to further improve the body strength of the product, especially for capacitors with larger capacity and more electrode layers, the effect is more obvious (because capacitors with a large number of electrode layers are more likely to have ceramic body fractures and poor strength problems).

[0009] Preferably, the reinforcement is arranged on the upper surface of the effective electrode layer, inside the effective electrode layer and on the lower surface of the effective electrode layer. The reinforcement arranged inside the effective electrode layer can form a ceramic capacitor with more balanced stress, which is easier to achieve especially for capacitors with smaller capacity and fewer electrode layers.

[0010] The reinforcement body is arranged on the upper and lower surfaces of the effective electrode layer, which is equivalent to the role of the capacitor protection cover. The effective electrode layer includes a ceramic dielectric layer and a metal electrode layer (for example, Ni or Cu). The effective electrode layer preferably uses a screen printing process to evenly apply the electrode material to the surface of the ceramic dielectric layer, and then undergoes a subsequent co-firing process to achieve densification. The effective electrode layer includes a plurality of staggered and stacked effective electrode units, which are stacked to form two end faces. The reinforcement body includes a plurality of stacked reinforcement body units, which are stacked to form two end faces, and the two end faces are in contact with the end electrodes respectively.

[0011] Preferably, the thickness ratio of the high-strength material layer to the ceramic dielectric layer is: high-strength material layer: ceramic dielectric layer = 0.1-0.9:1; preferably, the thickness ratio of the high-strength material layer to the ceramic dielectric layer is: high-strength material layer: ceramic dielectric layer = 0.2-0.5:1.

[0012] The high-strength material layer and the ceramic dielectric layer have inconsistent shrinkage behaviors due to the difference in shrinkage rate during the sintering process. By controlling the thickness and composition ratio of the high-strength material layer and the ceramic dielectric layer, the high-strength material layer can be evenly distributed between the ceramic dielectric layers with a thinner thickness using a similar internal electrode distribution principle. This uniform distribution of thin layers effectively disperses and balances the shrinkage stress, greatly reducing the stress concentration during the sintering process, that is, the high-strength material layer is thinned and evenly distributed in the reinforcement, effectively reducing the stress concentration during the sintering process. If the thickness ratio between the high-strength material layer and the ceramic dielectric layer is too small, that is, the high-strength material layer accounts for too little, the capacitor cannot meet the expected strength requirements; if the thickness ratio between the two is too high, that is, the high-strength material layer accounts for too high a proportion, it is easy to cause stress cracking due to the large difference in sintering shrinkage between the ceramic dielectric layer and the high-strength material layer.

[0013] Preferably, the thickness of the high-strength material layer is 1 to 5 μm, and the thickness of the ceramic dielectric layer is 4 to 14 μm. Limited by the overall size of the chip container and the thickness ratio of the high-strength material layer to the ceramic dielectric layer, if the thickness of the two is too high, the size of the chip container will increase, which is not conducive to the miniaturization and lightweight of the chip container and its application in electronic devices; if the thickness of the two is too low, the strength effect they play is limited.

[0014] Preferably, the thickness of the reinforcement is greater than or equal to 20% of the thickness of the multilayer ceramic capacitor. If the thickness of the reinforcement is less than 20% of the thickness of the multilayer ceramic capacitor, the strength improvement effect of the reinforcement is not good. Theoretically, there is no upper limit as long as the capacity requirements of the product can be met. In addition, the number of reinforcement units in the reinforcement is determined according to the total thickness of the reinforcement and its own thickness.

[0015] Preferably, when the capacitor capacity is greater than 100 nF, the thickness of the high-strength material layer is 1-2.5 μm; when the capacitor capacity is less than or equal to 100 nF, the thickness of the high-strength material layer is 2.6-5.0 μm.

[0016] For medium and high capacitance products, that is, capacitance greater than 100nF, the thickness of the high-strength material layer is 1 to 2.5μm. Compared with forming the high-strength material layer by secondary casting on the film tape, the thickness of the high-strength material layer prepared by screen printing can be thinner, and its appearance and thickness consistency can also be controlled more accurately; in addition, the thinner the reinforcement provided in the effective electrode layer, the smaller the stress generated by sintering will be, which is more suitable for the production of high-capacity products.

[0017] For low-capacitance products, i.e., capacitance less than or equal to 100nF, the thickness of the high-strength material layer is 2.6 to 5.0μm, and it is formed by a secondary casting process. By controlling the secondary casting process, the prepared high-strength material layer has a uniform structure, and its film strength, toughness, viscosity, etc. can meet the later lamination requirements.

[0018] In addition, when the capacitor capacity is greater than 100 nF, the thickness of the ceramic dielectric layer in the reinforcement is 4 to 7.5 μm; when the capacitor capacity is less than or equal to 100 nF, the thickness of the ceramic dielectric layer in the reinforcement is 8 to 14 μm.

[0019] The material of the high-strength material layer includes a high-strength material, and the high-strength material includes at least one of zirconium oxide, aluminum oxide, calcium zirconate, strontium zirconate, and calcium strontium zirconate titanate.

[0020] Zirconium oxide (ZrO2), aluminum oxide (Al2O3), calcium zirconate (CaZrO3), strontium zirconate (SrZrO3) and their composites calcium strontium zirconate titanate (Ca x Sr 1-x Zr y Ti 1-y O3) are all high-strength ceramic materials with a three-point bending strength of more than 300MPa and a small thermal expansion coefficient. The strength and thermal expansion coefficient of each material are shown in Table 1.

[0021] Table 1

[0022]

[0023] The present invention adopts zirconium oxide (ZrO2), aluminum oxide (Al2O3), calcium zirconate (CaZrO3), strontium zirconate (SrZrO3) and their composite calcium strontium zirconate titanate (CaZrO3) x Sr 1-x Zr y Ti 1-y At least one material with higher strength in (O3) is used as a high-strength material layer in the reinforcement body, which is evenly distributed on the upper and lower surfaces or the upper and lower surfaces and the effective electrode layer of the multilayer ceramic capacitor, effectively improving the flexural strength and bending strength of the multilayer ceramic capacitor.

[0024] Preferably, the high-strength material is at least one of zirconium oxide, calcium zirconate and strontium zirconate. These three materials have high strength, high sintering shrinkage matching, and excellent matching with the ceramic dielectric layer sintering. Among them, zirconium oxide has the best material strength, and its expansion coefficient is very similar to that of the ceramic dielectric layer material, and its matching with the ceramic dielectric layer sintering is more excellent. Preferably, the high-strength material layer also contains auxiliary materials, and the auxiliary materials contain at least one of calcium oxide, magnesium oxide, silicon oxide and yttrium oxide; the weight ratio of the high-strength material and the auxiliary material is: high-strength material: auxiliary material = (80-99.5): (0.5-20). Calcium oxide, magnesium oxide, silicon oxide and yttrium oxide serve as auxiliary materials of the high-strength material layer, acting as sintering aids to promote the sintering of the main material. Without changing the electrical properties of the multilayer ceramic capacitor itself, the content of the high-strength material and the auxiliary material within the above-mentioned ratio range can inhibit the diffusion of sintering elements and affect the electrical properties, and adjust the sintering shrinkage rate. More preferably, the weight ratio of the high-strength material to the auxiliary material is: high-strength material: auxiliary material = (87-98): (2-13). More preferably, the weight ratio of the high-strength material to the auxiliary material is: high-strength material: auxiliary material = (90-95): (5-10).

[0025] Preferably, the high-strength material is zirconium oxide, calcium zirconate and / or strontium zirconate. Calcium zirconate and strontium zirconate have high strength, high sintering shrinkage matching, and better matching with the ceramic dielectric layer during sintering.

[0026] Preferably, the material of the ceramic dielectric layer and the material of the effective electrode layer include BaTiO3, BaTi 1-x Zr x At least one of O3 and BaSrTiO3. The ceramic dielectric layer is made of a type II dielectric material with relatively excellent dielectric properties. Preferably, in the same capacitor, the main material of the ceramic dielectric layer is the same as the main material of the effective electrode layer.

[0027] Preferably, the raw materials for preparing the high-strength material layer further include a binder, a dispersant and a solvent; the raw materials for preparing the ceramic dielectric layer further include an additive, a binder, a dispersant and a solvent. The types of additives, binders, dispersants and solvents can be selected from commonly used types in the art according to needs.

[0028] Preferably, the method for preparing the reinforcement body comprises the following steps:

[0029] (a) mixing raw materials for preparing the ceramic dielectric layer uniformly and then forming the ceramic dielectric layer by tape casting;

[0030] (b) after uniformly mixing the raw materials for preparing the high-strength material layer, a high-strength material layer is formed on the ceramic dielectric layer in step (a) by a secondary casting process or a screen printing process to obtain a reinforcement unit;

[0031] (c) Repeating steps (a) and (b), stacking a plurality of reinforcement units obtained in step (b) to obtain the reinforcement.

[0032] The present invention also aims to provide a method for preparing the multilayer ceramic capacitor, comprising the following steps:

[0033] (1) mixing raw materials for preparing the ceramic dielectric layer uniformly and forming the ceramic dielectric layer by tape casting;

[0034] (2) after uniformly mixing the raw materials for preparing the high-strength material layer, a high-strength material layer is formed on the ceramic dielectric layer in step (1) by a secondary casting process or a screen printing process to obtain a reinforcement unit;

[0035] (3) mixing the raw materials for preparing the effective electrode layer uniformly and then tape-casting to obtain a ceramic membrane tape;

[0036] (4) using Ni or Cu electronic paste as the inner electrode paste to screen print the ceramic membrane tape obtained in step (3) to obtain the effective electrode unit;

[0037] (5) stacking the effective electrode units to form an effective electrode layer; stacking the reinforcing body units obtained in step (2) on two opposite surfaces of the effective electrode layer perpendicular to the stacking direction to obtain a stacked body unit;

[0038] (6) stacking at least one stacking unit to obtain a stacking body;

[0039] (7) The stacked body obtained in step (6) is subjected to pressing, cutting, debinding, sintering, chamfering, copper termination and surface treatment in sequence to obtain the multilayer ceramic capacitor.

[0040] The present invention adopts a secondary casting or screen printing process to achieve uniform distribution of the high-strength material layer on the conventional dielectric layer, which can effectively achieve the dispersion of sintering stress and the prevention of cracking problems. Casting, secondary casting and screen printing processes are aimed at preparing a film layer of corresponding thickness, and conventional process conditions in the field can be adopted. The process conditions such as pressing, cutting, debinding, sintering, chamfering, copper termination and surface treatment can all adopt conventional process conditions in the field.

[0041] Preferably, the raw material for preparing the ceramic dielectric layer in step (1) is the same as the raw material for preparing the effective electrode layer in step (3).

[0042] Preferably, in step (2), when the thickness of the high-strength material layer is 1 to 2.5 μm, the high-strength material layer is formed by a screen printing process; when the thickness of the high-strength material layer is 2.5 to 5.0 μm, the high-strength material layer is formed by a secondary casting process.

[0043] For medium and high capacitance products, the thickness of the high-strength material layer is 1 to 2.5 μm. Compared with the high-strength material layer formed by secondary casting on the film strip, the thickness of the high-strength material layer prepared by the screen printing process can be thinner, and its appearance and thickness consistency can also be controlled more accurately; in addition, the thinner the reinforcement body in the effective electrode layer, the smaller the stress generated by sintering, which is more suitable for the production of high-capacity products. By controlling the screen printing process, the prepared high-strength material layer has a uniform structure and appearance, and its film strip strength, toughness, viscosity, etc. can meet the later lamination requirements; the screen printing process parameters include the selection of printing film, printing speed, drying temperature and printing thickness, etc.

[0044] For low-capacitance products, the thickness is 2.6 to 5.0 μm and is formed by a secondary casting process. By controlling the secondary casting process, the prepared high-strength material layer has a uniform structure, and its film strength, toughness and viscosity can meet the later lamination requirements; the secondary casting process parameters include casting speed, drying temperature, casting thickness and film density.

[0045] In step (4), the qualified ceramic film tape of the intermediate casting is screen-printed according to the film specified in the design parameters, preferably using Ni electronic paste as the internal electrode paste to print a qualified electrode pattern;

[0046] Preferably, in step (5), the effective electrode units are staggered and stacked together to form effective electrical properties.

[0047] Preferably, in step (6), the stacking unit is 1 or 2. The stacking unit can be 1 or plural. When the stacking unit is 1, the reinforcement is arranged on the upper and lower surfaces of the effective electrode layer; when the stacking unit is 2, the reinforcement is arranged on the upper and lower surfaces of the effective electrode layer and inside the effective electrode layer; when the stacking unit is n, the reinforcement is arranged on the upper and lower surfaces of the effective electrode layer and inside the effective electrode layer, and n-1 reinforcements are arranged inside the effective electrode layer, which can be arranged according to specific circumstances. Generally speaking, a high strength effect can be achieved when the stacking unit is 1 or 2.

[0048] The beneficial effects of the present invention are as follows: the present invention provides a multilayer ceramic capacitor, the multilayer ceramic capacitor of the present invention uses high-strength materials as the high-strength material layer in the reinforcement body, which is evenly distributed on the upper and lower surfaces or the upper and lower surfaces and the effective electrode layer of the multilayer ceramic capacitor, which can significantly improve the strength defects of the multilayer ceramic capacitor material itself, and greatly improve the flexural strength and bending strength of the multilayer ceramic capacitor while ensuring the original electrical properties of the capacitor, so that the flexural strength of the multilayer ceramic capacitor of the present invention is ≥10kgf; the bending strength value is ≥7mm, which broadens the application field of MLCC products. The present invention also provides a method for preparing a multilayer ceramic capacitor, which uses a secondary casting or screen printing process to achieve the distribution of the reinforcement material in the conventional dielectric layer, and can effectively prevent the problems of material sintering matching by controlling the proportion and relative distribution of the reinforcement components, and can achieve a more accurate and reasonable preparation of the reinforcement body. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 A schematic diagram of the structure of the multilayer ceramic capacitor described in Example 1;

[0050] Figure 2 A schematic diagram of the structure of the multilayer ceramic capacitor described in Example 2;

[0051] Among them, 1. effective electrode layer; 2. reinforcement body; 3. end electrode. DETAILED DESCRIPTION

[0052] The performance data testing method involved in the embodiments of the present invention is shown in Table 2.

[0053] Table 2

[0054]

[0055] Among them, the flexural strength test method is: use a tensile tester to test its flexural strength. The test conditions are to fix the product on the test bench mold and use the tensile tester to apply a pressure of 1mm / s to the product until the product breaks.

[0056] Among them, the bending strength test method is: use a tensile tester to test its bending strength. The test conditions are to weld the product on a special PVB board, and use a tensile tester to apply a pressure of 1mm / s to the PVB board in the reverse direction until the product capacity change rate is greater than 10%.

[0057] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0058] Example 1

[0059] The structural schematic diagram of the multilayer ceramic capacitor of this embodiment is shown in Figure 1 The multilayer ceramic capacitor includes an effective electrode layer 1 and a reinforcement body 2, wherein the reinforcement body 2 is arranged on the upper surface and the lower surface of the effective electrode layer 1, and the reinforcement body 2 is formed by stacking a plurality of reinforcement body units; the effective electrode layer 1 is formed by staggered stacking of a plurality of effective electrode units, and the effective electrode units and the reinforcement body units are stacked to form two end surfaces, and the two end surfaces are respectively in contact with the end electrodes 3.

[0060] The reinforcing body unit includes a high-strength material layer and a ceramic dielectric layer; the material of the high-strength material layer includes high-strength material and auxiliary material, the high-strength material includes at least one of zirconium oxide, aluminum oxide, calcium zirconate, strontium zirconate and calcium strontium zirconate titanate; the auxiliary material includes at least one of calcium oxide, magnesium oxide, silicon oxide and yttrium oxide, and the weight ratio of the high-strength material to the auxiliary material is: high-strength material: auxiliary material = (80-99.5): (0.5-20); the weight ratio of the high-strength material to the auxiliary material is more preferably: high-strength material: auxiliary material = (87-98): (2-13); the weight ratio of the high-strength material to the auxiliary material is most preferably: high-strength material: auxiliary material = (90-95): (5-10). The material of the ceramic dielectric layer and the material of the effective electrode layer include BaTiO3, BaTi 1-x Zr x At least one of O3 and BaSrTiO3.

[0061] The thickness of the high-strength material layer is 1-5 μm, the thickness of the ceramic dielectric layer is 4-14 μm, and the thickness ratio of the high-strength material layer to the ceramic dielectric layer is: high-strength material layer: ceramic dielectric layer = 0.1-0.9:1.

[0062] The method for preparing the multilayer ceramic capacitor described in Example 1 comprises the following steps:

[0063] (1) mixing raw materials for preparing the ceramic dielectric layer uniformly and forming the ceramic dielectric layer by tape casting;

[0064] (2) after uniformly mixing the raw materials for preparing the high-strength material layer, a high-strength material layer is formed on the ceramic dielectric layer in step (1) by a secondary casting process or a screen printing process to obtain a reinforcement unit;

[0065] (3) mixing the raw materials for preparing the effective electrode layer uniformly and then tape-casting to obtain a ceramic membrane tape;

[0066] (4) using Ni electronic paste as the internal electrode paste to screen print the ceramic film tape obtained in step (3) according to the film specified in the design parameters, using Ni electronic paste as the internal electrode paste to print a qualified electrode pattern to obtain an effective electrode unit;

[0067] (5) stacking the reinforcement units obtained in step (2) according to product specifications to form a bottom reinforcement, and then stacking the effective electrode units obtained in step (4) to form an effective electrode layer, and then stacking the reinforcement units obtained in step (2) to form a top reinforcement, thereby obtaining a stacked body;

[0068] (6) The stacked body obtained in step (5) is subjected to pressing, cutting, debinding, sintering, chamfering, copper termination and surface treatment in sequence to obtain the multilayer ceramic capacitor.

[0069] Example 2

[0070] The structural schematic diagram of the multilayer ceramic capacitor of this embodiment is shown in Figure 2 The multilayer ceramic capacitor includes an effective electrode layer 1 and a reinforcement 2, wherein the reinforcement 2 is arranged on the upper surface, the lower surface and the inside of the effective electrode layer 1, and the reinforcement 2 is formed by stacking a plurality of reinforcement units; the effective electrode layer 1 is formed by staggered stacking of a plurality of effective electrode units, and the effective electrode units and the reinforcement units are stacked to form two end surfaces, and the two end surfaces are respectively in contact with the end electrodes 3.

[0071] The reinforcing body unit includes a high-strength material layer and a ceramic dielectric layer; the material of the high-strength material layer includes high-strength material and auxiliary material, the high-strength material includes at least one of zirconium oxide, aluminum oxide, calcium zirconate, strontium zirconate and calcium strontium zirconate titanate; the auxiliary material includes at least one of calcium oxide, magnesium oxide, silicon oxide and yttrium oxide, and the weight ratio of the high-strength material to the auxiliary material is: high-strength material: auxiliary material = (80-99.5): (0.5-20); the weight ratio of the high-strength material to the auxiliary material is more preferably: high-strength material: auxiliary material = (87-98): (2-13); the weight ratio of the high-strength material to the auxiliary material is most preferably: high-strength material: auxiliary material = (90-95): (5-10). The material of the ceramic dielectric layer and the material of the effective electrode layer include BaTiO3, BaTi 1-x Zr x At least one of O3 and BaSrTiO3.

[0072] The thickness of the high-strength material layer is 1-5 μm, the thickness of the ceramic dielectric layer is 4-14 μm, and the thickness ratio of the high-strength material layer to the ceramic dielectric layer is: high-strength material layer: ceramic dielectric layer = 0.1-0.9:1.

[0073] The method for preparing the multilayer ceramic capacitor described in Example 2 comprises the following steps:

[0074] (1) mixing raw materials for preparing the ceramic dielectric layer uniformly and forming the ceramic dielectric layer by tape casting;

[0075] (2) after uniformly mixing the raw materials for preparing the high-strength material layer, a high-strength material layer is formed on the ceramic dielectric layer in step (1) by a secondary casting process or a screen printing process to obtain a reinforcement unit;

[0076] (3) mixing the raw materials for preparing the effective electrode layer uniformly and then tape-casting to obtain a ceramic membrane tape;

[0077] (4) using Ni electronic paste as the internal electrode paste to screen print the ceramic film tape obtained in step (3) according to the film specified in the design parameters, using Ni electronic paste as the internal electrode paste to print a qualified electrode pattern to obtain an effective electrode unit;

[0078] (5) stacking the reinforcement unit obtained in step (2) according to the product specifications to form a bottom reinforcement, and then stacking the effective electrode unit obtained in step (4) in sequence to form an effective electrode layer, the reinforcement unit obtained in step (2), the effective electrode unit obtained in step (4), the reinforcement unit obtained in step (2), to obtain a stacked body;

[0079] (6) The stacked body obtained in step (5) is subjected to pressing, cutting, debinding, sintering, chamfering, copper termination and surface treatment in sequence to obtain the multilayer ceramic capacitor.

[0080] Example 3

[0081] In order to explore the influence of the thickness of the high-strength material layer and the ceramic dielectric layer on the performance of the multilayer ceramic capacitor, the thickness ratio of the high-strength material layer and the ceramic dielectric layer was changed according to the structure of the multilayer ceramic capacitor described in Example 1 and Example 2 to set the test groups 1 to 8 and the control groups 1 to 3 in Table 3, and the thickness ratio of the high-strength material layer and the ceramic dielectric layer was changed according to the structure of the multilayer ceramic capacitor described in Example 2 to set the test groups 9 to 16 and the control groups 4 to 6 in Table 3. A multilayer ceramic capacitor was prepared according to the 0805 specification sheet capacitor, wherein the high-strength material layer contained the following components in parts by weight: 83 parts of calcium zirconate, 2 parts of zirconium oxide, 2 parts of aluminum oxide, and 13 parts of auxiliary materials; the auxiliary materials were 3 parts of magnesium oxide, 3 parts of calcium oxide, and 5 parts of silicon oxide, and the ceramic dielectric layer and the effective electrode layer were barium titanate zirconate.

[0082] Table 3

[0083]

[0084] The test results of the MLCC structure described in Example 1 are shown in Table 4, and the test results of the MLCC structure described in Example 1 are shown in Table 5.

[0085] Table 4

[0086]

[0087] Table 5

[0088]

[0089]

[0090] From the test results in Table 4, it can be seen that when the H1 / H2 range is 0.1-0.9, the flexural strength of the product increases from 2.8 to 6.7-12.0 kgf; the bending strength increases from 3.3 mm to 5.9 mm-10.6 mm, indicating that the flexural strength and bending strength of the product using the reinforced body are significantly improved.

[0091] When H1 / H2=1.0, although the flexural strength and bending strength are both good, the product's welding resistance is 5ppm poor, indicating that the thickness of the high-strength layer is too thick, which affects the sintering shrinkage rate, making the effect of strengthening the uniform distribution of materials and thus dispersing stress in this technical solution weakened; there is a large residual stress in sintering, and when doing welding resistance testing, the product is subjected to thermal stress shock, and the release of sintering residual stress leads to thermal shock cracking; and the temperature characteristic TCC of the product has exceeded the standard and has deteriorated significantly. If H1 / H2 is less than 0.1, the bending strength cannot be improved well;

[0092] In addition, as the thickness of the high-strength material layer increases, the loss of the capacitor also increases, and the insulation resistance and withstand voltage performance also show a downward trend. Therefore, in order to ensure the multi-faceted performance of the product, the H1 / H2 ratio is preferably between 0.2 and 0.5.

[0093] The reinforcement in Example 2 is arranged on the upper surface, lower surface and inside of the effective electrode layer, while the reinforcement in Example 1 is only arranged on the upper surface and lower surface of the effective electrode layer. By comparing Table 4 and Table 5, it can be found that when H1 / H2 are the same, the strength of the MLCC structure described in Example 2 is greater, indicating that the more dispersed the reinforcement is, the more conducive it is to improving the strength of the multilayer container. The capacitor in Example 2 makes the distribution of high-strength materials in the product more uniform, with higher strength and better matching, and reduces the risk of stress cracking; however, the MLCC structure described in Example 2 also increases the volume proportion of the reinforcement component in the entire product, which reduces the proportion of the effective part, which is difficult to achieve for higher capacity products, especially for products with higher requirements for the number of effective electrode layers.

[0094] Example 4

[0095] In order to explore the influence of the materials of the high-strength material layer and the ceramic dielectric layer on the performance of the multilayer ceramic capacitor, the high-strength material and auxiliary materials and their proportions of the high-strength material layer and the ceramic dielectric layer were changed according to the structure of the multilayer ceramic capacitor described in Example 1, and the test groups 1 to 12 and the control groups 1 to 2 in Table 6 were set up. The multilayer ceramic capacitor was prepared according to the 0805 specification, wherein the thickness of the high-strength material layer was 2.5 μm and the ceramic dielectric layer was 7.5 μm, and the high-strength material and auxiliary materials in the high-strength material layer totaled 100 parts (proportion shown in Table 6). The ceramic dielectric layer and the effective electrode layer were barium zirconate titanate.

[0096] Table 6

[0097]

[0098] Note: “-” means no addition.

[0099] The test results are shown in Table 7.

[0100] Table 7

[0101]

[0102]

[0103] As can be seen from Table 7, if no auxiliary material is added to the high-strength material layer (control group 1), the product fails to sinter due to the high-strength material layer during product sintering. Because the sintering temperature of pure zirconia material is relatively high, multilayer ceramic capacitors are sintered at around 1200-1300 degrees Celsius, and the two are difficult to co-fire. Moreover, due to the size difference between the effective electrode layer and the high-strength protective layer after sintering, great stress is caused, and the stress is released when the temperature is lowered, causing the product to crack.

[0104] It can also be seen from Table 7 that the strength of zirconium oxide, calcium zirconate and strontium zirconate as the main materials of the high-strength material layer is significantly better than that of aluminum oxide or calcium strontium zirconate titanate. When M1 / M2 is 78:22, the strength of the product decreases slightly, which may be caused by the decrease in the composition of high-strength zirconium oxide materials; when M1 / M2 is 95.5:0.5, the product has 1ppm of welding cracking resistance; when M1 / M2 is 78:22, the welding resistance of the product has significantly deteriorated (cracks of ≤10ppm appear). Therefore, the ratio of M1 / M2 should not be too large; when M1 / M2 is 90~95:5~10, the product strength and welding performance are good.

[0105] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A multilayer ceramic capacitor, characterized in that: The invention comprises an effective electrode layer and a reinforcing body, wherein the reinforcing body is arranged at least one of the upper surface of the effective electrode layer, the interior of the effective electrode layer and the lower surface of the effective electrode layer; both end surfaces of the effective electrode layer and the reinforcing body are in contact with the end electrode; the reinforcing body is formed by stacking a plurality of reinforcing body units; the reinforcing body unit comprises a high-strength material layer and a ceramic dielectric layer, and the main material strength of the high-strength material layer is greater than the main material strength of the ceramic dielectric layer; The high-strength material layer is distributed between the ceramic dielectric layers, and the thickness ratio of the high-strength material layer to the ceramic dielectric layer is: high-strength material layer: ceramic dielectric layer = 0.2~0.5:1, the thickness of the high-strength material layer is 1~5μm, and the thickness of the ceramic dielectric layer is 4~14μm; the material of the high-strength material layer includes high-strength material and auxiliary material, the high-strength material is at least one of zirconium oxide, calcium zirconate and strontium zirconate, and the auxiliary material includes at least one of calcium oxide, magnesium oxide, silicon oxide and yttrium oxide; the weight ratio of the high-strength material to the auxiliary material is: high-strength material: auxiliary material = (90~95): (5~10); the thickness of the reinforcement is greater than or equal to 20% of the thickness of the multilayer ceramic capacitor.

2. The multilayer ceramic capacitor according to claim 1, wherein: When the capacitor capacity is greater than 100 nF, the thickness of the high-strength material layer is 1-2.5 μm; when the capacitor capacity is less than or equal to 100 nF, the thickness of the high-strength material layer is 2.6-5.0 μm.

3. The multilayer ceramic capacitor according to claim 1, wherein: The material of the ceramic dielectric layer and the material of the effective electrode layer include BaTiO3, BaTi 1-x Zr x At least one of O3 and BaSrTiO3.

4. The multilayer ceramic capacitor according to claim 1, wherein: The preparation method of the reinforcement body comprises the following steps: (a) mixing raw materials for preparing the ceramic dielectric layer uniformly and then forming the ceramic dielectric layer by tape casting; (b) after uniformly mixing the raw materials for preparing the high-strength material layer, forming the high-strength material layer on the ceramic dielectric layer in step (a) by a secondary casting process or a screen printing process, thereby obtaining a reinforcement unit; (c) Repeating steps (a) and (b), and stacking a plurality of reinforcement units obtained in step (b) to obtain the reinforcement.

5. A method for preparing a multilayer ceramic capacitor according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Mixing the raw materials for preparing the ceramic dielectric layer uniformly and forming the ceramic dielectric layer by tape casting; (2) after uniformly mixing the raw materials for preparing the high-strength material layer, a high-strength material layer is formed on the ceramic dielectric layer in step (1) by a secondary casting process or a screen printing process to obtain a reinforcement unit; (3) Mixing the raw materials for preparing the effective electrode layer uniformly and then tape-casting to obtain a ceramic film strip; the raw materials for preparing the effective electrode layer include BaTiO3, BaTi 1-x Zr x At least one of O3 and BaSrTiO3; (4) using Ni or Cu electronic paste as the inner electrode paste to screen print the ceramic film tape obtained in step (3) to obtain an effective electrode unit; (5) stacking the effective electrode units to form an effective electrode layer; stacking the reinforcing body units obtained in step (2) on two opposite surfaces of the effective electrode layer perpendicular to the stacking direction to obtain a stacked body unit; (6) stacking at least one stacking unit to obtain a stacking body; (7) The stacked body obtained in step (6) is subjected to pressing, cutting, debinding, sintering, chamfering, copper termination and surface treatment in sequence to obtain the multilayer ceramic capacitor.

Citation Information

Patent Citations

  • Multilayer ceramic chip capacitor and manufacturing method thereof

    CN106169370A

  • Multilayer sheet-type ceramic capacitor

    CN203013529U

  • Multilayer ceramic capacitor

    CN211125377U