A semiconductor structure and a method for manufacturing the same

By prefabing the sacrificial layer in the low K dielectric layer and performing plasma etching to form through holes and trenches, the problem of damage to low K materials during etching is solved, the increase in the dielectric constant K value is reduced, and the semiconductor device is improved performance.

CN110957263BActive Publication Date: 2024-11-15CHANGXIN MEMORY TECH INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811123264.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-09-26
Publication Date
2024-11-15
Estimated Expiration
2038-09-26

AI Technical Summary

Technical Problem

In the prior art, low K materials used in semiconductor interconnect dielectric layers are easily damaged during the etching process, resulting in an increase in the dielectric constant K value, increasing parasitic capacitance, and affecting device performance.

Method used

The sacrificial layer is prefabricated in the low K dielectric layer, and through holes and trenches are formed by plasma etching to avoid direct etching of the low K material and reduce the increase in the dielectric constant K value.

Benefits of technology

It effectively prevents damage to the low K dielectric layer in the etching process, reduces parasitic capacitance, and improves device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110957263B_ABST
    Figure CN110957263B_ABST
Patent Text Reader

Abstract

The present invention provides a semiconductor structure and a method for manufacturing the same, the method comprising the following steps: S1: providing a substrate having an etch stop layer on its surface; S2: forming a sacrificial layer on the surface of the etch stop layer; S3: removing the portion of the sacrificial layer outside a preset area and exposing the etch stop layer; S4: filling the space left after the sacrificial layer is removed with a low-K dielectric layer; S5: removing the remaining sacrificial layer, leaving a conductive material receiving space in the preset area. The present invention prefabricates a sacrificial layer in a low-K dielectric layer, and then performs plasma etching on the sacrificial layer to form through holes and grooves for metal interconnection, thereby avoiding etching damage caused by directly etching through holes and grooves on the low-K material, thereby preventing the low-K dielectric layer from being damaged during the etching process and causing its dielectric constant K value to increase, reducing the problem of significant increase in parasitic capacitance caused by the increase in K value, and improving device performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of integrated circuits and relates to a semiconductor structure and a manufacturing method thereof. Background Art

[0002] As integrated circuits develop towards high density and low power consumption, the feature size of devices is getting smaller and smaller, the cross-section of interconnect leads and the line spacing are also continuously reduced, and the parasitic effects caused by resistance and capacitance are increasingly affecting the performance of devices.

[0003] Currently, in the metal interconnect structure of dynamic random access memory (DRAM), low-resistivity Cu is used as the interconnect line and SiO2 is used as the interconnect medium. However, as the process node continues to shrink, the RC delay problem in Cu / SiO2 interconnection becomes more and more serious. Traditional SiO2 dielectric materials can no longer meet the needs of improving the performance of integrated circuits. In order to reduce RC delay, finding and developing new low-K materials as a new generation of interconnect medium and realizing Cu / low-K interconnection has become a technical key. The signal delay formula caused by the interconnect line is: τ = RC = (ρL / Wt metal )*(kε0LW / t ILD ) It can be seen that the parasitic capacitance C is proportional to the relative dielectric constant K of the interlayer interconnect medium, so the low-K material with a low dielectric constant can be used in the Cu interconnect structure to greatly reduce the parasitic capacitance.

[0004] However, most low-K materials have properties that are incompatible with other materials used to manufacture semiconductor devices, such as being not resistant to high temperatures, being brittle, and being easily damaged by etching processes.

[0005] Therefore, how to provide a semiconductor structure and a method for manufacturing the same to reduce the damage to the low-K dielectric layer during plasma etching of grooves and through holes in the Cu / low-K interconnect process, thereby reducing the problem of a significant increase in parasitic capacitance due to an increase in the dielectric constant K value, has become an important technical problem that needs to be urgently solved by those skilled in the art. Summary of the invention

[0006] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a semiconductor structure and a method for manufacturing the same, so as to solve the problem that in the prior art, when etching trenches or through holes, the interconnect dielectric layer formed of low-K material is easily damaged by plasma, resulting in an increase in the dielectric constant K value, thereby increasing the parasitic capacitance between the Cu interconnect lines and affecting the performance of the semiconductor memory device.

[0007] To achieve the above-mentioned object and other related objects, the present invention provides a method for manufacturing a semiconductor structure, comprising the following steps:

[0008] S1: providing a substrate having an etch stop layer on its surface;

[0009] S2: forming a sacrificial layer on the surface of the etch stop layer;

[0010] S3: removing the portion of the sacrificial layer outside the preset area, and exposing the etch stop layer;

[0011] S4: filling a low-K dielectric layer in the space left after the sacrificial layer is removed;

[0012] S5: removing the remaining sacrificial layer, leaving a conductive material receiving space in the preset area.

[0013] Optionally, in the step S2, after forming the sacrificial layer on the surface of the etch stop layer, an interconnection conductor area is defined, in the step S3, the preset area corresponds to the interconnection conductor area, and in the step S5, the conductive material receiving space is used as an interconnection groove.

[0014] Optionally, in the step S2, after forming the sacrificial layer on the surface of the etch stop layer, an interconnection through hole area is defined, in the step S3, the preset area corresponds to the interconnection through hole area, and in the step S5, the conductive material receiving space is used as an interconnection through hole.

[0015] Optionally, in the step S3, removing the portion of the sacrificial layer outside the interconnection through hole region comprises the following steps:

[0016] S3-1: forming an inorganic hard mask layer on the surface of the sacrificial layer;

[0017] S3-2: forming an inorganic hard mask layer opening corresponding to the interconnection through hole region in the inorganic hard mask layer;

[0018] S3-3: forming a metal hard mask layer in the opening of the inorganic hard mask layer;

[0019] S3 - 4 : using the metal hard mask layer as a mask to etch the inorganic hard mask layer and the sacrificial layer, and stopping on the etch stop layer.

[0020] Optionally, an etching selectivity ratio of the metal hard mask layer to the inorganic hard mask layer is greater than 1.5.

[0021] Optionally, in the step S5, before removing the remaining sacrificial layer, the following steps are further included:

[0022] S5-1: forming an upper etch stop layer on the surfaces of the sacrificial layer and the low-K dielectric layer;

[0023] S5-2: forming an upper sacrificial layer on the surface of the upper etch stop layer;

[0024] S5-3: defining an interconnection trench region, removing a portion of the upper sacrificial layer outside the interconnection trench region, and exposing the upper etch stop layer;

[0025] S5 - 4 : Filling the upper low-K dielectric layer in the space left after the upper sacrificial layer is removed.

[0026] Optionally, in the step S5-3, removing the portion of the upper sacrificial layer outside the interconnection trench region comprises the following steps:

[0027] S5-3-1: forming an inorganic hard mask layer on the surface of the upper sacrificial layer;

[0028] S5-3-2: forming an inorganic hard mask layer opening corresponding to the interconnect trench region in the inorganic hard mask layer;

[0029] S5-3-3: forming a metal hard mask layer in the opening of the inorganic hard mask layer;

[0030] S5-3-4: etching the inorganic hard mask layer and the upper sacrificial layer with the metal hard mask layer, and stopping on the upper etch stop layer.

[0031] Optionally, an etching selectivity ratio of the metal hard mask layer to the inorganic hard mask layer is greater than 1.5.

[0032] Optionally, in the step S5, removing the remaining sacrificial layer to form the interconnection through hole comprises the following steps:

[0033] S5-5: forming a photoresist layer on the surface of the upper sacrificial layer and the upper low-K dielectric layer;

[0034] S5-6: forming a photoresist layer opening corresponding to the interconnection through hole region in the photoresist layer;

[0035] S5-7: Using the photoresist layer as a mask, sequentially etching and removing the upper sacrificial layer, the upper etch stop layer and the sacrificial layer located in the interconnection through hole region.

[0036] Optionally, an etching gas containing CHF3 and O2 is used, and the upper sacrificial layer, the upper etch stop layer and the sacrificial layer are etched in one step by adjusting the proportion of O2.

[0037] Optionally, in the step S5, the following steps are further included:

[0038] S5-8: forming a photoresist layer opening corresponding to the interconnection trench region in the photoresist layer;

[0039] S5-9: using the photoresist layer as a mask, etching and removing the upper sacrificial layer located in the interconnection trench region to obtain an interconnection trench;

[0040] S5-10: removing the photoresist layer;

[0041] S5-11: removing the upper etch stop layer located in the interconnect trench region and the etch stop layer located in the interconnect through hole region.

[0042] Optionally, a front-layer interconnection layer is formed in the substrate, and the interconnection through hole exposes the front-layer interconnection layer.

[0043] Optionally, the dielectric constant of the sacrificial layer is greater than 3.8, and the dielectric constant of the low-K material layer is less than 3.8.

[0044] Optionally, the material of the sacrificial layer includes SiO2.

[0045] The present invention also provides a semiconductor structure, comprising:

[0046] substrate;

[0047] an etch stop layer formed on the substrate;

[0048] a sacrificial layer prefabrication area, defined above the etch stop layer;

[0049] A low-K dielectric layer is formed on the etch stop layer and is located around the sacrificial layer prefabricated region;

[0050] The conductive material receiving space corresponds to the sacrificial layer prefabricated area and penetrates the etching stop layer from top to bottom.

[0051] Optionally, the sacrificial layer prefabricated area corresponds to an interconnection wire area, and the conductive material receiving space serves as an interconnection groove.

[0052] Optionally, the sacrificial layer prefabricated area corresponds to an interconnection through hole area, and the conductive material receiving space serves as an interconnection through hole.

[0053] Optionally, the semiconductor structure further comprises:

[0054] an upper etch stop layer formed on the low-K dielectric layer;

[0055] an upper sacrificial layer prefabrication area, defined above the upper etch stop layer and corresponding to the location of the interconnect wire;

[0056] an upper low-K dielectric layer formed on the upper etch stop layer and located around the upper sacrificial layer prefabricated region;

[0057] The interconnection groove corresponds to the sacrificial layer prefabrication area and penetrates the upper etch stop layer from top to bottom.

[0058] Optionally, a front-layer interconnection layer is formed in the substrate, and the interconnection through hole exposes the front-layer interconnection layer.

[0059] Optionally, the dielectric constant of the low-K material layer is less than 3.8.

[0060] As described above, the semiconductor structure and the manufacturing method thereof of the present invention have the following beneficial effects: the present invention avoids etching damage caused by directly etching through holes and grooves on the low-K material by prefabricating a sacrificial layer in the low-K dielectric layer and then performing plasma etching on the sacrificial layer to form through holes and grooves for metal interconnection, thereby preventing the low-K dielectric layer from being damaged during the etching process and causing its dielectric constant K value to increase, reducing the problem of significant increase in parasitic capacitance caused by the increase in K value, and improving device performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1a-1h It shows a schematic diagram of the cross-sectional structure presented in each step of the through-hole dual damascene process in the prior art.

[0062] Figure 2a-2f It is a schematic cross-sectional structure diagram of each step of the manufacturing method of the semiconductor structure of the present invention in the first embodiment.

[0063] Figure 3a-3f It is a schematic cross-sectional structure diagram of each step of the manufacturing method of the semiconductor structure of the present invention in the second embodiment.

[0064] Figure 4a-4u It is a schematic diagram of the cross-sectional structure presented in each step of the manufacturing method of the semiconductor structure of the present invention in the third embodiment.

[0065] Figure 5 It is a schematic cross-sectional structure diagram of the semiconductor structure of the present invention in the fourth embodiment.

[0066] Figure 6 It is a schematic cross-sectional structure diagram of the semiconductor structure of the present invention in the fifth embodiment.

[0067] Figure 7 It is a schematic cross-sectional structure diagram of the semiconductor structure of the present invention in the sixth embodiment.

[0068] Component number description

[0069] 1 Substrate

[0070] 2 First etch stop layer

[0071] 3. First low-K dielectric layer

[0072] 4 Second etch stop layer

[0073] 5 Second low-K dielectric layer

[0074] 6 Front Interconnect Layer

[0075] 7 First photoresist layer

[0076] 8 First Opening

[0077] 9 Through Holes

[0078] 10 Second photoresist layer

[0079] 11 Second Opening

[0080] 12 Grooves

[0081] 101 Substrate

[0082] 102 Front Interconnect Layer

[0083] 103 Etch stop layer

[0084] 104 Sacrificial Layer

[0085] 105 Low K Dielectric Layer

[0086] 106 Interconnection vias

[0087] 201 Substrate

[0088] 202 Front Interconnect Layer

[0089] 203 Etch stop layer

[0090] 204 Sacrificial Layer

[0091] 205 Low K Dielectric Layer

[0092] 206 Interconnection Grooves

[0093] 301 substrate

[0094] 302 Cu layer

[0095] 303 Etch stop layer

[0096] 304 Sacrificial Layer

[0097] 305 Inorganic hard mask layer

[0098] 306 Photoresist layer

[0099] 307 Photoresist layer opening

[0100] 308 Inorganic hard mask layer opening

[0101] 309 Metal Hard Mask Layer

[0102] 310 Low K Dielectric Layer

[0103] 311 Upper etch stop layer

[0104] 312 Upper Sacrificial Layer

[0105] 313 Inorganic hard mask layer

[0106] 314 Photoresist layer

[0107] 315 Photoresist layer opening

[0108] 316 Inorganic hard mask layer opening

[0109] 317 Metal Hard Mask Layer

[0110] 318 Upper low-K dielectric layer

[0111] 319 Photoresist layer

[0112] 320 Photoresist layer opening

[0113] 321 Interconnection Vias

[0114] 322 Photoresist layer opening

[0115] 323 Interconnection Groove

[0116] 401 substrate

[0117] 402 Front Interconnection Layer

[0118] 403 Etch stop layer

[0119] 404 Low K Dielectric Layer

[0120] 405 Sacrificial layer prefabrication area

[0121] 406 Interconnect Via

[0122] 501 substrate

[0123] 502 Front Interconnect Layer

[0124] 503 Etch stop layer

[0125] 504 Low K Dielectric Layer

[0126] 505 Sacrificial layer prefabrication area

[0127] 506 Interconnect Groove

[0128] 601 Substrate

[0129] 602 Front Interconnect Layer

[0130] 603 Etch stop layer

[0131] 604 Low K Dielectric Layer

[0132] 605 Upper etch stop layer

[0133] 606 Upper low-K dielectric layer

[0134] 607 Sacrificial layer prefabrication area

[0135] 608 Interconnection Via

[0136] 609 Upper sacrificial layer prefabrication area

[0137] 610 Interconnection Groove DETAILED DESCRIPTION

[0138] Figure 1a-1h The current via-first dual damascene process is shown. Figure 1a As shown, a stacked structure is provided, which includes a substrate 1, a first etch stop layer 2, a first low-K dielectric layer 3, a second etch stop layer 4 and a second low-K dielectric layer 5 from bottom to top, wherein a Cu layer 6 is formed in the substrate. Figure 1b As shown, a first photoresist layer 7 is formed on the second low-K dielectric layer, and a first opening 8 is formed in the first photoresist layer. Figure 1c As shown, the first photoresist layer is used as a mask to etch downwards, and the etching stops on the first etching stop layer to obtain a through hole 9 (Via). Figure 1d As shown, the first photoresist layer is removed. Figure 1e As shown, a second photoresist layer 10 is formed on the second low-K dielectric layer, and a second opening 11 is formed in the second photoresist layer. Figure 1f As shown, the second photoresist layer is used as a mask to etch downwards, and the etching stops on the second etching stop layer to obtain a trench 12. Figure 1g As shown, the second photoresist layer is removed. Figure 1h As shown, the first etch stop layer at the bottom of the through hole is removed.

[0139] In the prior art, when etching trenches or vias, the interconnect dielectric layer formed of low-K material is easily damaged by plasma, causing the dielectric constant K value to increase, thereby increasing the parasitic capacitance between the Cu interconnect lines and affecting the performance of the semiconductor memory device.

[0140] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0141] See also Figures 2a to 7 It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0142] Embodiment 1

[0143] This embodiment provides a method for manufacturing a semiconductor structure, which manufactures an interconnection via (Via) for forming a conductive plug, comprising the following steps:

[0144] like Figure 2a As shown, step S1 is performed: providing a substrate 101 having an etch stop layer 103 on its surface.

[0145] Specifically, the material of the substrate 101 includes but is not limited to conventional semiconductor substrates such as silicon, germanium, germanium silicon, and III-V compounds, and the material of the etch stop layer 103 includes but is not limited to SiC.

[0146] As an example, a front interconnection layer 102 is also formed in the substrate 101. In this embodiment, the front interconnection layer 102 includes a copper layer.

[0147] like Figure 2b As shown, step S2 is performed: forming a sacrificial layer 104 on the surface of the etch stop layer 103 .

[0148] Specifically, the dielectric constant K of the sacrificial layer 104 is greater than 3.8, and the material of the sacrificial layer 104 includes but is not limited to SiO 2 .

[0149] like Figure 2c As shown, step S3 is performed: a dry etching process is used to remove the portion of the sacrificial layer 104 outside the preset area, and the etching stop layer 103 is exposed.

[0150] Specifically, an interconnection through-hole area is defined. In this embodiment, the preset area corresponds to the interconnection through-hole area.

[0151] like Figure 2dAs shown, step S4 is performed: filling the low-K dielectric layer 105 in the space left after the sacrificial layer 104 is removed.

[0152] Specifically, the dielectric constant K of the low-K dielectric layer is less than 3.8, and the material of the low-K dielectric layer includes but is not limited to SiCOH.

[0153] like Figure 2e As shown, step S5 is performed: using a dry etching process to remove the remaining sacrificial layer 104 , leaving a conductive material receiving space in the preset area. In this embodiment, the conductive material receiving space is used as an interconnection through hole 106 .

[0154] Further, such as Figure 2f As shown, the method further includes etching downward to remove the etch stop layer 103 at the bottom of the interconnection through hole 106 to expose the copper layer.

[0155] The method for manufacturing a semiconductor structure of the present invention prefabricates a sacrificial layer in a low-K dielectric layer, and then performs plasma etching on the sacrificial layer to form a through hole for metal interconnection, thereby avoiding etching damage caused by directly etching the low-K material through the through hole, thereby preventing the low-K dielectric layer from being damaged during the etching process and causing its dielectric constant K value to increase, reducing the problem of significant increase in parasitic capacitance caused by the increase in K value, and improving device performance.

[0156] Embodiment 2

[0157] This embodiment provides a method for manufacturing a semiconductor structure, showing a single damascene process, and manufacturing an interconnection trench for forming a metal wire, including the following steps:

[0158] like Figure 3a As shown, step S1 is performed: providing a substrate 201 having an etch stop layer 203 on its surface.

[0159] Specifically, the material of the substrate 201 includes but is not limited to conventional semiconductor substrates such as silicon, germanium, germanium silicon, and III-V compounds, and the material of the etch stop layer 203 includes but is not limited to SiC.

[0160] As an example, a front interconnection layer 202 is also formed in the substrate 201. In this embodiment, the front interconnection layer 202 includes conductive pillars.

[0161] like Figure 3b As shown, step S2 is performed: forming a sacrificial layer 204 on the surface of the etch stop layer 203 .

[0162] Specifically, the dielectric constant K of the sacrificial layer 204 is greater than 3.8, and the material of the sacrificial layer 204 includes but is not limited to SiO 2 .

[0163] like Figure 3c As shown, step S3 is performed: a dry etching process is used to remove the portion of the sacrificial layer 204 outside the preset area, and the etching stop layer 203 is exposed.

[0164] Specifically, an interconnection conductor area is defined. In this embodiment, the preset area corresponds to the interconnection conductor area.

[0165] like Figure 3d As shown, step S4 is performed: filling the low-K dielectric layer 205 in the space left after the sacrificial layer 204 is removed.

[0166] Specifically, the dielectric constant K of the low-K dielectric layer is less than 3.8, and the material of the low-K dielectric layer includes but is not limited to SiCOH.

[0167] like Figure 3e As shown, step S5 is performed: the remaining sacrificial layer 204 is removed by dry etching process, leaving a conductive material receiving space in the preset area. In this embodiment, the conductive material receiving space is used as the interconnection groove 206.

[0168] Further, such as Figure 3f As shown, the method further includes etching downward to remove the etch stop layer 203 at the bottom of the interconnection trench 206 to expose the conductive pillar.

[0169] At this point, interconnection grooves for forming metal conductors are fabricated. The method for fabricating a semiconductor structure of the present invention prefabricates a sacrificial layer in a low-K dielectric layer, and then performs plasma etching on the sacrificial layer to form grooves for metal interconnection, thereby avoiding etching damage caused by directly etching the low-K material, thereby preventing the low-K dielectric layer from being damaged during the etching process and causing its dielectric constant K value to increase, reducing the problem of significant increase in parasitic capacitance caused by the increase in K value, and improving device performance.

[0170] Embodiment 3

[0171] This embodiment provides a method for manufacturing a semiconductor structure, showing a via-first dual damascene process, manufacturing an interconnection via (Via) for forming a conductive plug and an interconnection trench (Trench) for forming a metal conductor, including the following steps:

[0172] like Figure 4a As shown, step S1 is performed: providing a substrate 301 having an etch stop layer 303 on its surface.

[0173] Specifically, the material of the substrate 301 includes but is not limited to conventional semiconductor substrates such as silicon, germanium, germanium silicon, and III-V compounds, and the material of the etch stop layer 303 includes but is not limited to SiC.

[0174] As an example, a front-layer interconnection layer 302 is also formed in the substrate 301. In this embodiment, the front-layer interconnection layer 302 includes a copper layer.

[0175] like Figure 4a As shown, step S2 is performed: forming a sacrificial layer 304 on the surface of the etch stop layer 303 .

[0176] Specifically, the dielectric constant K of the sacrificial layer 304 is greater than 3.8, and the material of the sacrificial layer 304 includes but is not limited to SiO 2 .

[0177] like Figure 4a-4e As shown, step S3 is performed: removing the portion of the sacrificial layer 304 outside the preset area, and exposing the etch stop layer.

[0178] Specifically, an interconnection through-hole area is defined, and the preset area corresponds to the interconnection through-hole area.

[0179] As an example, this step includes the following sub-steps:

[0180] Step S3-1: Figure 4a As shown, an inorganic hard mask layer 305 is formed on the surface of the sacrificial layer 304 , and the material of the inorganic hard mask layer includes but is not limited to tetraethyl orthosilicate (TEOS), carbon, etc.

[0181] Step S3-2: Figure 4a As shown, a photoresist layer 306 is formed on the inorganic hard mask layer 305, and a photoresist layer opening 307 corresponding to the interconnection through hole region is formed by a photolithography process, and then Figure 4b As shown, the inorganic hard mask layer 305 is dry-etched using the patterned photoresist layer 303 as a mask to form an inorganic hard mask layer opening 308 corresponding to the interconnection through hole region in the inorganic hard mask layer 305 .

[0182] Step S3-3: Figure 4c As shown, a metal hard mask layer 309 is formed in the inorganic hard mask layer opening 308, and as shown Figure 4d As shown, the metal hard mask layer 309 is polished by chemical mechanical polishing (CMP) to remove the excess metal hard mask layer on the surface of the inorganic hard mask layer 305. The material of the metal hard mask layer 309 includes but is not limited to TiN, Cu3N and the like.

[0183] Step S3-4: Figure 4e As shown, the inorganic hard mask layer 305 and the sacrificial layer 304 are dry-etched using the metal hard mask layer 309 as a mask, and the etching stops on the etching stop layer 303 .

[0184] Specifically, when the inorganic hard mask layer 305 is dry-etched using the metal hard mask layer 309 as a mask, a high etching selectivity ratio is required between the two. In this embodiment, the etching selectivity ratio of the metal hard mask layer 309 to the inorganic hard mask layer 305 is greater than 1.5.

[0185] like Figure 4f-4g As shown, step S4 is performed: filling the low-K dielectric layer 310 in the space left after the sacrificial layer is removed.

[0186] Specifically, Figure 4f As shown, a low-K dielectric layer 310 is filled in the structure etched in step S3 by using a spin coating method (SOD), and as shown in FIG. Figure 4g As shown, the low-K dielectric layer 310 is polished by a chemical mechanical polishing process until the metal hard mask layer 309 is removed.

[0187] like Figure 4h-4u As shown, step S5 is performed: removing the remaining sacrificial layer 304 , leaving a conductive material receiving space in the preset area, and the conductive material receiving space serves as an interconnection through hole 321 .

[0188] As an example, this step includes the following sub-steps:

[0189] Step S5-1: Figure 4h As shown, an upper etch stop layer 311 is formed on the surface of the sacrificial layer 304 and the low-K dielectric layer 310 by chemical vapor deposition (CVD).

[0190] Step S5-2: Figure 4h As shown, a chemical vapor deposition (CVD) method is then used to form an upper sacrificial layer 312 on the surface of the upper etch stop layer 311 .

[0191] Step S5-3: Figure 4h-Figure 4m As shown, an interconnection trench region is defined, a portion of the upper sacrificial layer 312 outside the interconnection trench region is removed, and the upper etch stop layer 311 is exposed.

[0192] As an example, first perform step S5-3-1: Figure 4hAs shown, an inorganic hard mask layer 313 is formed on the surface of the upper sacrificial layer 312 by chemical vapor deposition (CVD). The material of the inorganic hard mask layer 313 includes but is not limited to tetraethyl orthosilicate (TEOS), carbon, and the like.

[0193] Then execute step S5-3-2: Figure 4i As shown, a photoresist layer 314 is formed on the surface of the inorganic hard mask layer 313, and a photoresist layer opening 315 corresponding to the interconnection groove region is formed in the photoresist layer 314 by using a conventional photolithography process (exposure, development, etc.), and then Figure 4j As shown, the inorganic hard mask layer 313 is dry-etched using the patterned photoresist layer 314 as a mask to form an inorganic hard mask layer opening 316 corresponding to the interconnection trench region in the inorganic hard mask layer 313.

[0194] Then execute step S5-3-3: Figure 4k As shown, a metal hard mask layer 317 is formed in the inorganic hard mask layer opening 316, and as shown Figure 4l As shown, the metal hard mask layer 317 is polished by chemical mechanical polishing (CMP) to remove the excess metal hard mask layer on the surface of the inorganic hard mask layer 313. The material of the metal hard mask layer 317 includes but is not limited to TiN, Cu3N and the like.

[0195] Then execute step S5-3-4: Figure 4m As shown, the inorganic hard mask layer 313 and the upper sacrificial layer 312 are dry-etched with the metal hard mask layer 317 , and the etching stops on the upper etch stop layer 311 .

[0196] Specifically, when the inorganic hard mask layer 313 is dry-etched using the metal hard mask layer 317 as a mask, a high etching selectivity ratio is required between the two. In this embodiment, the etching selectivity ratio of the metal hard mask layer 317 to the inorganic hard mask layer 313 is greater than 1.5.

[0197] Furthermore, the step S5 also includes step S5-4: Figure 4n-4o As shown, an upper low-K dielectric layer 318 is filled in the space left after the upper sacrificial layer 312 is removed.

[0198] As an example, Figure 4n As shown, the upper low-K dielectric layer 318 is filled in the structure etched in step S5-3 by using a spin coating method (SOD), and as shown in FIG. Figure 4o As shown, the upper low-K dielectric layer 318 is polished by a chemical mechanical polishing process until the metal hard mask layer 317 is removed.

[0199] Step S5-5: Figure 4p As shown, a photoresist layer 319 is formed on the surface of the upper sacrificial layer 312 and the upper low-K dielectric layer 318 .

[0200] Step S5-6: Figure 4p As shown, a photoresist layer opening 320 corresponding to the interconnection through hole region is formed in the photoresist layer 319 by using a photolithography process.

[0201] Step S5-7: Figure 4q As shown, the patterned photoresist layer 319 is used as a mask, and a dry etching process is adopted to sequentially etch away the upper sacrificial layer 313 , the upper etch stop layer 311 and the sacrificial layer 304 located in the interconnection through hole area, and finally stop on the etch stop layer 303 .

[0202] Specifically, an etching gas containing CHF 3 is used. In this embodiment, the etching gas also contains O 2 , and the upper sacrificial layer 313 , the upper etch stop layer 311 and the sacrificial layer 304 are etched in one step by adjusting the proportion of O 2 .

[0203] Furthermore, the step S5 also includes step S5-8: Figure 4r As shown, a photoresist layer opening 322 corresponding to the interconnection trench region is formed in the photoresist layer 319 by a photolithography process. It should be noted that the photoresist layer 319 may be removed in advance, another photoresist layer is formed, and the photoresist layer opening 322 is formed in the newly formed photoresist layer.

[0204] Step S5-9: Figure 4s As shown, the patterned photoresist layer 319 is used as a mask, and a dry etching process is adopted to remove the upper sacrificial layer 312 located in the interconnection groove area, and the etching stops on the upper etch stop layer 311 to obtain the interconnection groove 323.

[0205] Step S5-10: Figure 4t As shown, the photoresist layer 319 is removed by dry method.

[0206] Step S5-11: Figure 4u As shown, the upper etch stop layer 311 located in the interconnect trench region and the etch stop layer 303 located in the interconnect through hole region are removed by a dry etching process.

[0207] At this point, interconnection vias 321 (Via) for forming conductive plugs and interconnection trenches 323 (Trench) for forming metal conductors are fabricated. The method for fabricating a semiconductor structure of the present invention prefabricates a sacrificial layer in a low-K dielectric layer, and then performs plasma etching on the sacrificial layer to form vias and trenches for metal interconnection, thereby avoiding etching damage caused by directly etching vias and trenches on low-K materials, thereby preventing the low-K dielectric layer from being damaged during the etching process and causing its dielectric constant K value to increase, reducing the problem of significant increase in parasitic capacitance caused by the increase in K value, and improving device performance.

[0208] Embodiment 4

[0209] This embodiment provides a semiconductor structure. Figure 5 , which is a schematic diagram of the cross-sectional structure of the semiconductor structure, including: a substrate 401, an etch stop layer 403, a sacrificial layer prefabricated area 405, a low-K dielectric layer 404 and a conductive material accommodating space.

[0210] Specifically, the material of the substrate 401 includes but is not limited to conventional semiconductor substrates such as silicon, germanium, germanium silicon, III-V compounds, etc. A front interconnection layer 402 is also formed in the substrate 401. In this embodiment, the front interconnection layer 402 includes a copper layer.

[0211] Specifically, the etch stop layer 403 is formed on the substrate 401 , and its material includes but is not limited to SiC.

[0212] Specifically, the sacrificial layer prefabricated area 405 (such as Figure 5 The low-K dielectric layer 404 is formed on the etch stop layer 403 and is located around the sacrificial layer prefabricated area 405. The dielectric constant K of the low-K dielectric layer 404 is less than 3.8, and the material of the low-K dielectric layer 404 includes but is not limited to SiCOH.

[0213] Specifically, the conductive material receiving space corresponds to the sacrificial layer prefabricated area 405 and vertically penetrates the etch stop layer 403. In this embodiment, the conductive material receiving space serves as an interconnection through hole 406, and the interconnection through hole 406 exposes the copper layer.

[0214] In the semiconductor structure of the present invention, through holes for metal interconnection are formed in a prefabricated area of ​​a sacrificial layer, thereby avoiding etching damage caused by directly etching the through holes on the low-K material, thereby preventing the low-K dielectric layer from being damaged during the etching process and causing its dielectric constant K value to increase, reducing the problem of a significant increase in parasitic capacitance caused by an increase in the K value, and improving device performance.

[0215] Embodiment 5

[0216] This embodiment provides a semiconductor structure. Figure 6 , which is a schematic diagram of the cross-sectional structure of the semiconductor structure, including: a substrate 501, an etch stop layer 503, a sacrificial layer prefabricated area 505, a low-K dielectric layer 504 and a conductive material accommodating space.

[0217] Specifically, the material of the substrate 501 includes but is not limited to conventional semiconductor substrates such as silicon, germanium, germanium silicon, III-V compounds, etc. A front interconnection layer 502 is also formed in the substrate 501. In this embodiment, the front interconnection layer 402 includes conductive pillars.

[0218] Specifically, the etch stop layer 503 is formed on the substrate 501 , and its material includes but is not limited to SiC.

[0219] Specifically, the sacrificial layer prefabricated area 505 (such as Figure 6 The low-K dielectric layer 504 is formed on the etch stop layer 503 and is located around the sacrificial layer prefabricated region 505. The dielectric constant K of the low-K dielectric layer 504 is less than 3.8, and the material of the low-K dielectric layer 504 includes but is not limited to SiCOH.

[0220] Specifically, the conductive material receiving space corresponds to the sacrificial layer prefabricated area 505 and vertically penetrates the etch stop layer 503. In this embodiment, the conductive material receiving space serves as an interconnection groove 506, and the interconnection groove 506 exposes the conductive column.

[0221] In the semiconductor structure of the present invention, the grooves for metal interconnection are formed in the prefabricated area of ​​the sacrificial layer, thereby avoiding etching damage caused by directly etching the low-K material, thereby preventing the low-K dielectric layer from being damaged during the etching process and causing its dielectric constant K value to increase, reducing the problem of significant increase in parasitic capacitance caused by the increase in K value, and improving device performance.

[0222] Embodiment 6

[0223] This embodiment provides a semiconductor structure. Figure 7 , which is a schematic diagram of the cross-sectional structure of the semiconductor structure, including: a substrate 601, an etch stop layer 603, a sacrificial layer prefabricated region 607, a low-K dielectric layer 604, an upper etch stop layer 605, an upper sacrificial layer prefabricated region 609, an upper low-K dielectric layer 606, an interconnection through hole 608 and an interconnection groove 610.

[0224] Specifically, the material of the substrate 601 includes but is not limited to conventional semiconductor substrates such as silicon, germanium, germanium silicon, III-V compounds, etc. A front interconnection layer 602 is also formed in the substrate 601. In this embodiment, the front interconnection layer 602 includes a copper layer.

[0225] Specifically, the etching stop layer 603 is formed on the substrate 601 , and its material includes but is not limited to SiC.

[0226] Specifically, the sacrificial layer prefabricated area 607 (such as Figure 7 The low-K dielectric layer 604 is formed on the etch stop layer 603 and is located around the sacrificial layer prefabricated area 607. The dielectric constant K of the low-K dielectric layer 604 is less than 3.8, and the material of the low-K dielectric layer 604 includes but is not limited to SiCOH.

[0227] Specifically, the interconnection through hole 608 serves as a conductive material receiving space, corresponds to the sacrificial layer prefabricated area 607, and penetrates the etching stop layer 603 from top to bottom to expose the copper layer.

[0228] Specifically, the upper etch stop layer 605 is formed on the low-K dielectric layer 605 , and its material includes but is not limited to SiC.

[0229] Specifically, the upper sacrificial layer prefabricated area 609 (such as Figure 7 The upper low-K dielectric layer 606 is formed on the upper etch stop layer 605 and is located around the sacrificial layer prefabricated region 609. The dielectric constant K of the upper low-K dielectric layer 606 is less than 3.8, and the material of the upper low-K dielectric layer 606 includes but is not limited to SiCOH.

[0230] Specifically, the interconnection groove 610 corresponds to the sacrificial layer prefabricated region 609 and penetrates the upper etch stop layer 605 from top to bottom.

[0231] In the semiconductor structure of the present invention, through holes and grooves for metal interconnection are formed in a prefabricated area of ​​a sacrificial layer, thereby avoiding etching damage caused by directly etching through holes and grooves on a low-K material, thereby preventing the low-K dielectric layer from being damaged during the etching process and causing its dielectric constant K value to increase, reducing the problem of a significant increase in parasitic capacitance caused by an increase in the K value, and improving device performance.

[0232] In summary, the semiconductor structure and the manufacturing method of the present invention prefabricate a sacrificial layer in the low-K dielectric layer, and then perform plasma etching on the sacrificial layer to form through holes and grooves for metal interconnection, thereby avoiding etching damage caused by directly etching through holes and grooves on the low-K material, thereby preventing the low-K dielectric layer from being damaged during the etching process and causing its dielectric constant K value to increase, reducing the problem of significant increase in parasitic capacitance caused by the increase in K value, and improving device performance. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has a high industrial utilization value.

[0233] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for manufacturing a semiconductor structure, characterized in that: The following steps are involved: Providing a substrate having an etch stop layer on its surface; forming a sacrificial layer on the surface of the etch stop layer; Removing the portion of the sacrificial layer outside the preset area and exposing the etch stop layer; Filling the low-K dielectric layer in the space left after the sacrificial layer is removed; Removing the remaining sacrificial layer, leaving a conductive material receiving space in the preset area; After forming the sacrificial layer on the surface of the etch stop layer, an interconnection through hole region is defined, the preset region corresponds to the interconnection through hole region, and the conductive material receiving space serves as an interconnection through hole; Before removing the remaining sacrificial layer, the method further comprises the following steps: forming an upper etch stop layer on the surfaces of the sacrificial layer and the low-K dielectric layer; forming an upper sacrificial layer on the surface of the upper etch stop layer; Defining an interconnect trench region, removing a portion of the upper sacrificial layer outside the interconnect trench region, and exposing the upper etch stop layer; filling an upper low-K dielectric layer in the space left after the upper sacrificial layer is removed; and removing a portion of the upper sacrificial layer outside the interconnect trench region comprises the following steps: forming an inorganic hard mask layer on the surface of the upper sacrificial layer; forming an inorganic hard mask layer opening corresponding to the interconnect trench region in the inorganic hard mask layer; forming a metal hard mask layer in the opening of the inorganic hard mask layer; Etching the inorganic hard mask layer and the upper sacrificial layer with the metal hard mask layer, and stopping on the upper etch stop layer; Removing the remaining sacrificial layer to form the interconnection via comprises the following steps: forming a photoresist layer on the surface of the upper sacrificial layer and the upper low-K dielectric layer; forming a photoresist layer opening corresponding to the interconnection through hole region in the photoresist layer; Using the photoresist layer as a mask, the upper sacrificial layer, the upper etch stop layer and the sacrificial layer located in the interconnection through hole area are sequentially etched away; and the method for manufacturing the semiconductor structure further comprises the following steps: forming a photoresist layer opening corresponding to the interconnection trench region in the photoresist layer; Using the photoresist layer as a mask, etching and removing the upper sacrificial layer located in the interconnection groove region to obtain an interconnection groove; removing the photoresist layer; The upper etch stop layer located in the interconnect trench region and the etch stop layer located in the interconnect via region are removed.

2. The method for manufacturing a semiconductor structure according to claim 1, wherein: After forming the sacrificial layer on the surface of the etch stop layer, an interconnection conductor area is defined, the preset area corresponds to the interconnection conductor area, and the conductive material receiving space is used as an interconnection groove.

3. The method for manufacturing a semiconductor structure according to claim 1, wherein: Removing the portion of the sacrificial layer outside the interconnection through hole region comprises the following steps: forming an inorganic hard mask layer on the surface of the sacrificial layer; forming an inorganic hard mask layer opening corresponding to the interconnection via region in the inorganic hard mask layer; forming a metal hard mask layer in the opening of the inorganic hard mask layer; The inorganic hard mask layer and the sacrificial layer are etched using the metal hard mask layer as a mask, and the etching stops on the etching stop layer.

4. The method for manufacturing a semiconductor structure according to claim 1, wherein: A front-layer interconnection layer is formed in the substrate, and the interconnection through hole exposes the front-layer interconnection layer.

5. A semiconductor structure, characterized in that: The semiconductor structure is prepared using any one of the manufacturing methods of claims 1 to 4, include: substrate; an etch stop layer formed on the substrate; a sacrificial layer prefabrication area, defined above the etch stop layer; A low-K dielectric layer is formed on the etch stop layer and is located around the sacrificial layer prefabricated region; A conductive material receiving space corresponding to the sacrificial layer prefabricated area and penetrating the etching stop layer from top to bottom; A front-level interconnect layer is also formed in the substrate, and the front-level interconnect layer includes a copper layer.

6. The semiconductor structure according to claim 5, characterized in that: The sacrificial layer prefabricated area corresponds to the interconnection wire area, and the conductive material receiving space serves as an interconnection groove.

7. The semiconductor structure according to claim 5, characterized in that: The sacrificial layer prefabricated area corresponds to the interconnection through hole area, and the conductive material receiving space serves as the interconnection through hole.

8. The semiconductor structure according to claim 7, characterized in that: The semiconductor structure further comprises: an upper etch stop layer formed on the low-K dielectric layer; an upper sacrificial layer prefabrication area, defined above the upper etch stop layer and corresponding to the location of the interconnect wire; an upper low-K dielectric layer formed on the upper etch stop layer and located around the upper sacrificial layer prefabricated region; The interconnection groove corresponds to the sacrificial layer prefabrication area and penetrates the upper etch stop layer from top to bottom.

9. The semiconductor structure according to claim 8, characterized in that: A front-layer interconnection layer is formed in the substrate, and the interconnection through hole exposes the front-layer interconnection layer.

10. The semiconductor structure according to claim 5, characterized in that: The dielectric constant of the low-K dielectric layer is less than 3.8.