Quaternary phosphonium salt flame retardant and synthesis method and application thereof

A synthesis method and flame retardant technology, which is applied in the field of chemical compounds in the field of chemical technology, can solve the problems of complex synthesis process, low yield and harsh conditions of sulfonate phosphonium salt flame retardant, and achieve excellent flame retardant effect and high yield High and mild synthetic conditions

CN111233923AActive Publication Date: 2020-06-05SHANGHAI JIAO TONG UNIV
7 Cites 2 Cited by

Patent Information

Authority / Receiving Office
CN · China
Current Assignee / Owner
Publication Date
2020-06-05

Smart Images

  • Figure 1
    Figure 1
  • Figure 2
    Figure 2
  • Figure 3
    Figure 3
Patent Text Reader

Abstract

The invention provides a quaternary phosphonium salt flame retardant and a synthesis method and application thereof, and the method comprises the following steps: by taking an acidic compound, ortho-formic acid trisubstituted ester and an organic phosphine compound III or IV as raw materials, carrying out a one-step reaction process to prepare the quaternary phosphonium salt flame retardant I or II. The flame retardant disclosed by the invention has good thermal stability and has an excellent flame-retardant effect when being applied to various polymers. The method is simple and convenient insynthesis operation, low in raw material price, mild in synthesis condition and high in yield. According to the synthesis method, introduction of halogen ions is avoided, and dozens of anions are successfully introduced. By adding a small amount of the flame retardant, the obtained PC flame-retardant composite material UL-94 can reach the V-0 grade.
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention relates to compounds in the technical field of chemical industry, in particular to a quaternary phosphonium salt flame retardant and its synthesis method and application. Background technique

[0002] The most commonly used synthesis method of organic quaternary phosphonium salts is to react phosphine with chlorinated alkanes to generate quaternary phosphonium halides, and the resulting products are anion-exchanged with metal salts and remove metal halides to obtain the target product. In most applications of organic quaternary phosphonium salts, weakly coordinating anions such as BF4-, PF6-, SbF6-, and (CF3SO2)2N- are required, and residual metal halides in the product have been reported to reduce their usefulness. performance. Although this common synthetic method is very effective for the synthesis of organic quaternary phosphonium salts, the separation of inorganic metal halides in the anion exchange step is still quite challenging. ...

Examples

Embodiment 1

[0038] This embodiment is a synthetic method of a quaternary phosphonium salt flame retardant, and the specific steps are as follows:

[0039] Triphenylphosphine (0.0035 mol), diphenyl phosphate (0.00355 mol) and trimethyl orthoformate (1.8 ml) were successively added to the reaction tube, and a stirring bar was added. The reaction system was sealed and reacted at 110° C. for 24 hours. After the reaction was completed, it was cooled to room temperature, the solvent was evaporated under reduced pressure, and recrystallization was performed using dichloromethane and ethyl acetate. The obtained solid was washed with ethyl acetate and petroleum ether, and the white solid obtained after suction filtration was moved to a vacuum oven at 60°C for overnight drying to obtain a solid quaternary phosphonium salt flame retardant (PFR-1), the structural formula of which was:

[0040]

[0041] It is the quaternary phosphonium salt flame retardant I, and the yield is about 94%.

[0042] ...

Embodiment 2

[0050] This embodiment is a synthetic method of a quaternary phosphonium salt flame retardant, and the specific steps are as follows:

[0051] Triphenylphosphine (0.0035 mol), binaphthol phosphate (0.00355 mol) and trimethyl orthoformate (2 ml) were successively added to the reaction tube, and a stirring bar was added. The reaction system was sealed and reacted at 110° C. for 30 hours. After the reaction was completed, it was cooled to room temperature, the solvent was evaporated under reduced pressure, and recrystallization was performed using dichloromethane and ethyl acetate. The obtained solid was washed with ethyl acetate and petroleum ether, and the white solid obtained after suction filtration was moved to a vacuum oven at 60°C for overnight drying. The obtained solid was a quaternary phosphonium salt flame retardant (PFR-2), and the structural formula was:

[0052]

[0053] It is the quaternary phosphonium salt flame retardant I, and the yield is about 81%.

[005...

Embodiment 3

[0062] This embodiment is a synthetic method of a quaternary phosphonium salt flame retardant, and the specific steps are as follows:

[0063] Triphenylphosphine (0.223 mol), p-toluenesulfonic acid monohydrate (0.223 mol) and trimethyl orthoformate (130 ml) were successively added to the two-necked flask, and a stirring bar was added. Heat to reflux at 110°C for 12 hours. After the reaction was completed, it was cooled to room temperature, and the solvent was evaporated under reduced pressure. Using dichloromethane, ethyl acetate and petroleum ether for recrystallization, the obtained solid was washed with ethyl acetate and petroleum ether, and the white solid obtained after suction filtration was moved to a vacuum oven at 60°C for overnight drying to obtain a solid quaternary phosphonium Salt flame retardant (PFR-3), its structural formula is:

[0064]

[0065] It is the quaternary phosphonium salt flame retardant I, and the yield is about 90%.

[0066] On the other han...