Component for plasma etching device with improved plasma resistance and method for manufacturing the same

By depositing a rare earth metal thin film on quartz components for plasma etching equipment and performing heat treatment to form a thermal diffusion layer, problems such as insufficient plasma resistance and arc discharge are solved, and high durability and transparency are achieved, making it suitable for semiconductor applications. Process endpoint analysis.

CN111247627BActive Publication Date: 2024-10-25KOMICO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201880067718.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-09-14
Filing Date
2018-07-17
Publication Date
2024-10-25
Estimated Expiration
2038-07-17

AI Technical Summary

Technical Problem

Quartz components used in existing plasma etching devices have problems such as insufficient plasma resistance, arc discharge hazards, changes in dielectric constant, and degradation of material physical properties in highly integrated processes. In particular, they are prone to peeling and contamination during long-term use.

Method used

A rare earth metal film is deposited by vacuum deposition and heat treated in the atmosphere or protective atmosphere to form a thermal diffusion layer of the rare earth metal to improve the plasma resistance and transparency of the component.

Benefits of technology

It achieves no risk of peeling, maintains optical properties, reduces thermal stress, and improves durability and corrosion resistance. It is suitable for end-point analysis of semiconductor processes, and the process is simple and economical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111247627B_ABST
    Figure CN111247627B_ABST
Patent Text Reader

Abstract

The present invention relates to a component for a plasma etching device and a manufacturing method thereof, and more particularly, to a component for a plasma etching device and a manufacturing method thereof, which improves plasma resistance by depositing a rare earth metal film and performing surface heat treatment, maintains light transmittance, and can be used as a component for endpoint analysis of an etching process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a component for a photo plasma etching device and a method for manufacturing the same, and more particularly, to a technology for improving the plasma resistance of a component for a plasma etching device by utilizing the thermal diffusion phenomenon of a rare earth metal thin film. Background Art

[0002] In the semiconductor manufacturing process, the plasma dry etching process is becoming increasingly important for the microfabrication required for the high integration of circuits on substrates such as silicon wafers.

[0003] The plasma etching process can make the vertical etching rate much greater than the horizontal etching rate, so the final aspect ratio of the etched pattern can be appropriately controlled. If the plasma etching process is actually used, an extremely fine pattern with a large aspect ratio can be formed in a film with a thickness of about 1 micron.

[0004] The equipment chamber environment for performing such dry etching processes requires high cleanliness as the processing level becomes more and more micronized. However, in various processes for micro-processing, highly corrosive gases such as fluoride and chloride are used, and there is a problem that such process gases corrode not only the wafer but also the interior of the chamber.

[0005] In order to be used in such an environment, materials with excellent plasma resistance are being used as chamber components, and representative materials include alumina, alumina sintered bodies, and quartz components.

[0006] Among them, as for quartz components, although the dry plasma etching rate is higher than other materials, it is still used because of special purposes. The situation where quartz components are used in large quantities is the edge ring surrounding the periphery of the wafer. The periphery of the wafer is only beneficial if it maintains an environment similar to that of the silicon wafer electrically. The byproduct produced during the etching process is SiF4 (silicon fluoride) which is easier to vaporize than other materials. Using this easily vaporized material will reduce the impact on the wafer yield, so most of the edge rings tend to use quartz components.

[0007] Another example of a quartz component used is an endpoint analysis component, which is an accessory that can be adjusted to etch the material to the desired depth by analyzing the wavelength generated during the etching process. The material suitable for observing the inside must be transparent, and the transparency of quartz is completely suitable for this purpose. However, since quartz has a much lower plasma resistance than other materials, there is a problem of having to replace the component in the long term.

[0008] In order to solve this problem, various methods are being discussed as existing technologies. As for quartz components for plasma etching devices, in order to improve plasma resistance, a method of melting and coating with a hydrogen-oxygen flame or a method of coating a melt of yttrium or yttrium compound or YAG and heating and melting is being used. In addition, due to the recent development of spraying technology used in the semiconductor field, plasma spraying, high-speed flame spraying, aerosol deposition, etc. are being applied. However, there are many problems with this conventional technology.

[0009] In particular, if a film of other materials with a thickness of more than 10μm is formed on the edge ring surrounding the silicon wafer in the quartz component, there is a risk of arc discharge caused by differences in electrical characteristics between the electrode and the wafer. In addition, there is a possibility that process parameters such as CD and EPD will change due to changes in the dielectric constant around the chamber.

[0010] In the case of the plasma spraying method, which has been mainly used recently, roughness is formed by performing a bead blasting process on the surface of the quartz component. Due to this physical impact, the surface of the quartz component is damaged, and from a long-term perspective, there are problems such as cracking and fatigue damage that limit recycling. There is a limit that the film level below 10μm cannot be uniformly controlled.

[0011] In addition, as a process feature of the spraying method, there is a quenching effect. Quartz, as a material with strong bonding force from an atomic point of view, is very fragile to thermal shock. Due to the quenching effect that occurs during the application, thermal stress accumulates, and the material properties deteriorate due to residual stress, which can also become a problem.

[0012] As for the aerosol deposition that is being studied recently, a film at the 10μm level is also formed. Although this is technically feasible, due to the low adhesion caused by the simple mechanical fit between the film and the surface, problems such as peeling may occur when used for a long time. With the help of CF4 plasma ions and free radicals used in the dry etching process, the film is etched and particles are generated, which will contaminate the chip.

[0013] Recently, as a method of changing the material used, dry etching process equipment manufacturers have also proposed a method of using an amorphous plasma-resistant glass composition or silicon carbide, but this is not cost-effective and has limitations in use.

[0014] The following briefly describes the prior art in the field to which the present invention belongs, and then describes the technical matters that the present invention is to achieve differently by comparing the prior art.

[0015] First, Korean Patent No. 10-0727672 (June 5, 2007) relates to a component for a plasma etching device, and more specifically, to a component for a plasma etching device, in which an yttrium oxide or YAG film having a thickness of not less than 10 μm, a thickness deviation of not more than 10%, and a surface roughness Ra of not more than 1 μm is formed on the surface of a component composed of quartz glass, aluminum, acid-resistant aluminum or a combination thereof, and a manufacturing technology for forming an yttrium oxide or YAG film having a thickness of not less than 10 μm, a thickness deviation of not more than 10%, and a surface roughness Ra of not more than 1 μm by using a method of plasma thermal spraying yttrium oxide or YAG on the surface of the component, a method of melting and coating yttrium oxide or YAG powder with a hydrogen-oxygen flame, a method of coating a molten yttrium or yttrium compound or YAG and heating and melting it, and a combination thereof.

[0016] In addition, Korean Patent No. 10-0689889 (February 26, 2007) relates to plasma-resistant quartz glass and a method for manufacturing the same, and more specifically, provides a quartz glass and a quartz glass fixture or a method for manufacturing the same, wherein the quartz glass is excellent in plasma corrosion resistance, especially corrosion resistance to fluorine-based plasma gas, as a fixture material for plasma reaction used in semiconductor manufacturing, and can be used without causing abnormalities to silicon wafers. The technology is a quartz glass containing a sum of two or more metal elements of 0.1 to 20 weight %, wherein the metal elements are composed of at least one first metal element selected from Group 3B of the periodic table and at least one second metal element selected from the group consisting of Mg, Ca, Sr, Ba, Sc, Y, Ti, Zr, Hf, lanthanide elements and actinide elements, and the maximum concentration of each second metal element is 2.0 weight % or less, thereby improving corrosion resistance.

[0017] However, the plasma-resistant components of the prior art documents also have the limitations of the above-mentioned process technology such as the spraying method, or the doped quartz glass components manufactured by mixing with different elements, heating and melting, which are not economical in terms of the ratio of different elements.

[0018] The inventor felt the limitations of this film formation method and material change method, and attempted to provide an effective and excellent method for improving plasma resistance through surface reforming. After unremitting research on the technology of manufacturing components for plasma etching devices with excellent plasma resistance through a continuous process of metal film deposition and heat treatment, the present invention was finally completed. Summary of the invention

[0019] Technical issues

[0020] The main object of the present invention is to provide a method for manufacturing a component for a plasma etching device, which not only improves the plasma resistance during the semiconductor process, but also maintains light transmittance and can be used for endpoint analysis of the etching process.

[0021] Technical Solution

[0022] In order to achieve the above-mentioned purpose, an embodiment of the present invention provides a method for manufacturing components for plasma etching equipment, comprising the following steps: a) depositing a rare earth metal film including rare earth metals on a substrate with a thickness of 0.01 μm to 2.0 μm by vacuum deposition; and b) heat treating the substrate with the rare earth metal film deposited at 1000°C to 2000°C for 2 hours to 40 hours in an atmosphere of air, nitrogen, oxygen or argon.

[0023] In a preferred embodiment of the present invention, the vacuum deposition method may be electron beam physical vapor deposition (EBPVD) or sputtering.

[0024] In a preferred embodiment of the present invention, the rare earth metal may be any one or more of yttrium, ytterbium, and samarium.

[0025] In a preferred embodiment of the present invention, the melting point of the substrate material may be above 1000°C.

[0026] In a preferred embodiment of the present invention, the substrate may be any one of quartz, alumina sintered body, and sapphire.

[0027] In a preferred embodiment of the present invention, the heat treatment time in step b) can be 2 hours to 20 hours.

[0028] Another embodiment of the present invention provides a component for a plasma etching device, which is manufactured by the manufacturing method and has a thermal diffusion layer of the rare earth metal with a thickness of 0.1 μm to 10 μm.

[0029] Another embodiment of the present invention provides a transparent member for a plasma etching device manufactured by the manufacturing method, wherein the rare earth metal thermal diffusion layer has a thickness of 0.1 μm to 10 μm.

[0030] Technical Effects

[0031] The components for the plasma etching device of the present invention do not have changes in electrical properties (breakdown voltage and dielectric constant) due to the effects of rare earth metal doping, thereby minimizing the possibility of changes in process parameters. By utilizing chemical bonding by thermal diffusion methods, there is no risk of peeling, etc. The thermal stress of the material is eliminated by the heat treatment effect, which can prevent the physical properties of the material from degrading. After deposition, the transparency is protected by atmosphere heat treatment, and the original optical properties of the component are maintained, so that it can be used as an original endpoint analysis component, etc.

[0032] In addition, the manufacturing method of the present invention provides the advantages of being reasonable in cost and time through simple deposition and heat treatment, and does not include a pre-treatment process that causes physical damage such as a bead blasting process. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a schematic diagram of an edge ring member for a plasma etching device.

[0034] Figure 2 This is a process of forming a rare earth metal thick film in order to improve the plasma resistance of a member for a plasma etching apparatus according to the present invention.

[0035] Figure 3 The SIMS analysis results of elemental analysis at each depth before (A) and after (B) the heat treatment of Example 1 are shown.

[0036] Figure 4 The SIMS analysis results of elemental analysis at each depth before (A) and after (B) the heat treatment of Example 2 are shown.

[0037] Figure 5 (A) and (B) are the three-dimensional orbital XPS analysis results of yttrium present on the surface before (A) and after (B) heat treatment of Example 1.

[0038] Figure 5 (C) and (D) are the three-dimensional orbital XPS analysis results of yttrium present inside Example 1 before (C) and after (D) heat treatment.

[0039] Figure 6 (A) and (B) are the XPS analysis results of the yttrium three-dimensional orbits at various depths before (A) and after (B) the heat treatment of Example 3.

[0040] Figure 6 (C) and (D) are the XPS analysis results of the aluminum three-dimensional track at each depth before (C) and after (D) heat treatment of Example 3. DETAILED DESCRIPTION

[0041] Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as those commonly understood by experts skilled in the art to which the invention belongs. Generally speaking, the nomenclature used in this specification is well known and commonly used in the art.

[0042] Throughout the specification of the present application, when it is mentioned that a certain part “includes” a certain constituent element, unless there is any special description to the contrary, it means that other constituent elements are not excluded and other constituent elements may be included.

[0043] In the semiconductor manufacturing process, gate etching devices, insulating film etching devices, resist film etching devices, sputtering devices, CVD devices, etc. are used. On the other hand, in the liquid crystal manufacturing process, etching devices for forming thin film transistors are used. In addition, in these manufacturing devices, a structure equipped with a plasma generating mechanism is adopted for the purpose of high integration based on micro-processing.

[0044] In these manufacturing processes, halogen-based corrosive gases such as fluorine and chlorine are used as processing gases in the above-mentioned devices due to their high reactivity. Fluorine-based gases may be, for example, SF6, CF4, CHF3, ClF3, HF, NF3, etc., and chlorine-based gases may be, for example, Cl2, BCl3, HCl, CCl4, SiCl4, etc. In an atmosphere into which these gases are introduced, if microwaves or high frequencies are introduced, these gases are converted into plasma. In device components exposed to these halogen-based gases or their plasma, there is little metal on the surface other than the material components, and high corrosion resistance is required. Therefore, the present invention aims to provide a method for manufacturing components for plasma etching devices having excellent plasma resistance.

[0045] One aspect of the present invention provides a method for manufacturing components for a plasma etching device, comprising: a) depositing a rare earth metal film with a thickness of 0.01 μm to 2.0 μm on a substrate by vacuum deposition; and b) heat treating the substrate with the rare earth metal film deposited at 1000°C to 2000°C for 2 hours to 40 hours in an atmosphere of air, nitrogen, oxygen or argon.

[0046] A representative example of the member for a plasma etching apparatus is mainly used as an edge ring. Figure 1 A schematic diagram representing the shape of an edge ring is shown in FIG. In addition, the edge ring is not only used in a plasma etching device, but can also be used in a chamber for plasma PVD, CVD, ion implantation, etc.

[0047] The melting point of the substrate material is preferably above 1000°C. When the melting point of the substrate is less than 1000°C, thermal damage to the substrate will occur during the heat treatment. In addition, if the melting point is too high, the deposited material cannot be fully thermally diffused, and the diffusion depth cannot be controlled. The high temperature treatment used to control this will also induce deformation of the deposited material.

[0048] The substrate is often an oxide ceramic, an oxidized metal, or a metal composed of one or more elements selected from Group 4, Group 5, Group 13, and Group 14 of the periodic table (for example, one or more elements selected from silicon and aluminum). Representative examples of such a processing member may be, for example, one or more selected from silicon dioxide or glass, alumina, anodized aluminum, processed aluminum, silicon, and aluminum, and specifically, preferably quartz, alumina sintered body, or sapphire.

[0049] The quartz material can be selected from the group consisting of different silicon-containing materials suitable for forming glass, synthetic silica, fused silica, fused quartz, high-purity quartz, quartz sand and quartz glass compositions. The quartz material can also be obtained by any suitable process.

[0050] In the present invention, any substrate having a melting point of 1000° C. or higher can be used, and can be easily used as a material for chamber components of a dry etching device used in a semiconductor manufacturing process.

[0051] The vacuum deposition method may be electron beam physical vapor deposition (EBPVD) or sputtering. The rare earth metal thin films finally obtained by the two methods have almost no quality difference.

[0052] The film formation mechanism of the electron beam physical vapor deposition method (EB-PVD) is to accelerate electrons with energy of several keV or more, irradiate the target material to melt the material, and the molten material moves in a gaseous state and is deposited on the substrate. Compared with the resistance heating deposition method or sputtering using a filament, the electron beam physical vapor deposition method can heat the target material to a high temperature in a short time, which is beneficial for manufacturing thin films of high melting point ceramics such as oxides. Specifically, the method for manufacturing rare earth metal thin films provided by the present invention is characterized in that a solid rare earth metal raw material is prepared as a target in a vacuum chamber, the target is melted and vaporized using an electron beam, and the vaporized target material is deposited on a substrate.

[0053] In addition, in the present invention, the sputtering method is effective in the case of depositing a metal film on a member for a plasma etching device of a complex shape. Specifically, the sputtering method can easily obtain a high-quality film, and is therefore widely used. The sputtering method is a method of stacking a metal film and an insulator on a wafer. The principle of sputtering is a physical process like throwing a steel ball at a concrete wall. The colliding ball throws up fragments having chemical and physical properties like concrete. If this process is repeated, the vicinity of the collision site is covered with concrete fragments. In sputtering, the "steel ball" is an ionized argon atom, and the "concrete wall" is a plate of sputtered material, called a target. The sputtering process is performed in a vacuum chamber. Ionized argon gas is injected into the reaction chamber where the sputtered material target and the wafer are located. Compared with the positively charged argon gas, the target is negatively charged. Therefore, the argon atoms are accelerated, and unlike ion injection, the argon atoms do not nail into the target in sputtering. Instead, they collide like a steel structure and throw out some of the target. The reaction chamber is a vacuum, so the fallen material is stacked everywhere in the reaction chamber including the wafer.

[0054] The rare earth metals are a general term for 17 elements of the lanthanum group including lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71, scandium (Sc) with atomic number 21, and yttrium (Y) with atomic number 39. The rare earth metal elements used in the component of the present invention are preferably rare earth metal elements selected from Y, Sc, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu, and more preferably, rare earth metal elements selected from Y, Sm and Yb. These rare earth metal elements can be used alone or in combination of two or more.

[0055] In particular, yttrium oxide, which is an oxide of yttrium, has a number of advantages over quartz. First, yttrium oxide has a higher sputtering critical energy than quartz, and is therefore a better sputtering resistor. Second, yttrium oxide has a lower tendency to form a volatile layer than quartz, so the yttrium oxide film can last longer, and the average replacement cycle of the yttrium oxide film component is longer. Third, yttrium oxide has a higher dielectric constant of more than 11 times, while quartz has a dielectric constant of approximately 3.5, and the desired RF connection can be obtained between the ground extension and the plasma.

[0056] Another advantage of using yttrium oxide thin film is that fluorine-containing process gases can be used more effectively. That is, when carbon fluoride process gas is used in conjunction with a quartz ring, the fluorine ion concentration can be removed at the edge of the wafer due to the formation of volatile compounds, thereby inducing a lack of uniformity and a lower edge etching rate in the overall etching of the wafer substrate compared to the use of yttrium oxide rings. However, yttrium oxide thin film components are better sputtering resistors than quartz rings and are not prone to forming fluorine compounds. Therefore, the use of yttrium oxide thin film components can further improve the critical width and etching rate uniformity of the entire wafer substrate, and can effectively generate a more uniform plasma.

[0057] The rare earth metal film has a thickness of 0.01 μm to 2.0 μm, which is preferred in terms of improving the plasma resistance of the components for the plasma etching apparatus of the present invention. Specifically, if the thickness of the rare earth metal film is less than 0.01 μm, the thermal diffusion depth of the rare earth metal component is reduced, and the rare earth metal component cannot have a sufficient doping effect, and the effect of improving the plasma resistance to be achieved by the present invention is insufficient. If the thickness of the rare earth metal film exceeds 2.0 μm, it is not preferred in terms of economy.

[0058] The step b) of heat treatment is performed in air, nitrogen, oxygen or argon atmosphere to dope the rare earth metal into the plasma etching device component through thermal diffusion phenomenon, and the concentration of the final thermal diffusion layer will vary depending on the atmosphere.

[0059] The heat treatment step b) is preferably performed at 1000° C. to 2000° C. For quartz components, if the temperature is less than 1000° C., the rare earth metal component cannot be fully diffused into the component, and if the temperature exceeds 2000° C., it will change into other phases due to approaching the glass transition temperature. In addition, the heat treatment temperature is preferably set differently depending on the deposition atmosphere and the type of component for the plasma etching device.

[0060] The temperature rise and fall characteristics of rare earth metal films, that is, the temperature rise and fall rate and the temperature distribution within the surface during temperature rise and fall are different depending on the material, thickness and material properties. Therefore, the heating time and cooling time need to be adjusted according to the type of thin film metal.

[0061] Furthermore, by appropriately adjusting the temperature rise time required to reach the set temperature and the temperature drop time required to reach room temperature after heat treatment, the durability of the rare earth metal thin film can be improved.

[0062] The heat treatment time of step b) is preferably 2 to 40 hours, more preferably 2 to 20 hours. If the heat treatment time is less than 2 hours, the thermal diffusion depth of the rare earth metal cannot reach the range of 0.1 μm to 1 μm, and if the heat treatment time exceeds 40 hours, the physical properties of the components of the plasma etching device may be reduced due to thermal deformation of the components.

[0063] Generally speaking, a plasma processing apparatus includes a reaction chamber, a gas supply unit installed inside the reaction chamber and supplying source gas required for generating plasma gas to the inside of the reaction chamber, an electrode unit on which a wafer is placed and which also acts as an electrode, and a gas distribution means for uniformly spraying the source gas supplied from the gas supply unit toward the wafer.

[0064] Furthermore, a view port is provided in the reaction chamber to enable observation of the interior of the chamber. The chamber view port (or commonly known as the end point window) is typically a transparent component made of quartz or sapphire. A variety of optical sensors can be protected by the view port, through which optical sensor readings can be performed. Additionally, the view port allows a user to visually inspect or observe the wafer during processing. Both quartz and sapphire have poor resistance to plasma erosion. As the plasma chemicals erode the view port and make the surface rough, the optical properties of the view port change. For example, the view port may become blurred / the optical signal that can pass through the view port may be distorted. This may impair the ability of the optical sensor to collect accurate readings. However, since such a coating may block the view port, a thick film protective layer may not be suitable for use on the view port.

[0065] The appearance characteristics of the rare earth metal film obtained by the vacuum deposition method in the step a) show metallic luster and are in a state of lacking light transmittance before heat treatment. On the contrary, the surface of the component for the plasma etching device including the thermal diffusion layer of the rare earth metal that has been heat-treated in the step b) loses its metallic luster in appearance and appears to be transparent and reformed.

[0066] This is different from the aerosol deposition or spraying method where the color of the original deposited material is maintained and the film has a white color after formation. In the case of the present invention, the luster of the rare earth metal component disappears through atmosphere heat treatment after deposition, and transparency is exhibited, maintaining the original optical properties of the component, providing the advantage of being able to be used as an original endpoint analysis component, etc. In addition, it can be used as an accessory of equipment that requires a window component, and the corrosion resistance of the window component is improved, so the device can be used for a long life.

[0067] exist Figure 2In the figure, a method for manufacturing a quartz component for a plasma etching device of the present invention is shown in a schematic diagram. If the quartz component on which the yttrium metal film is deposited is heat-treated within the heat treatment temperature range, the yttrium metal component moves into the interior of the quartz component by means of a diffusion phenomenon from a high concentration to a low concentration, and at the same time, the silicon component existing in the quartz component moves into the yttrium metal film. As a result, the yttrium thin film layer forms a three-component system Y-Si-O thin film layer composed of yttrium metal component, silicon component and oxygen component. This film in the form of a rare earth metal oxide doped film is a coating that imparts etching resistance and plasma resistance to the surface of the quartz component.

[0068] In the present invention, the deposited rare earth metal diffuses into the component through the heat treatment process in step b), and the thickness of the thermal diffusion layer means the distance from the surface of the rare earth metal film to the point where the concentration of the main element of the component is the same as the concentration of the rare earth metal.

[0069] Through the heat treatment step, a rare earth metal thermal diffusion layer with a thickness of 0.1 μm to 10 μm is formed on the surface of the component for the plasma etching device. Depending on the composition of the substrate, a Y-Si-O thin film or an Al-YO (YAG) thin film layer can be formed.

[0070] The component in the form of a rare earth metal component doped on the surface by the heat treatment step of the present invention is preferred in terms of no change in electrical characteristics (breakdown voltage and dielectric constant). Specifically, this is because the geometric structure of the edge ring and the material forming the edge ring affect the etching rate curve. That is, if the dielectric constant (dielectric value) of the material forming the edge ring of the plasma device changes, it is necessary to change the coupling to the lower electrode in the edge area of ​​the wafer and adjust the process parameters. However, in the present invention, by partially doping yttrium oxide in the quartz component, there is no change in the dielectric constant, and the possibility of changes in the process parameters required to control the etching rate curve can be minimized.

[0071] In addition, the greater the difference in thermal expansion coefficients between two adjacent materials, the greater the possibility that one of the materials will eventually crack, peel off, or lose its bond to the other material. In the conventional film formation method, since it is a simple physical bond through a physical deposition method, it is exposed to the risk of separation such as peeling due to the difference in thermal expansion coefficients, but in the thermal diffusion method, there is no risk of peeling due to chemical bonding.

[0072] In addition, in the case of thermal spraying, although the thermal stress is high due to the quenching effect, the corresponding technology eliminates the thermal stress of the material due to the annealing effect by means of post-heat treatment, which can prevent the physical properties of the material from being reduced. Unlike the thermal spraying method, the roughness is not given to the surface of the quartz component through the bead blasting process, so there is no physical damage to the material, and it is preferred for long-term use.

[0073] Compared to changing materials, surface reforming through simple deposition and heat treatment would be a reasonable alternative in terms of cost and time.

[0074] The present invention will be described in more detail below by way of examples. However, the following examples are merely illustrative of the present invention and the present invention is not limited by the examples.

[0075] <Examples 1 to 3>

[0076] Examples 1 to 3 Yttrium metal thin films were manufactured according to the structures and conditions described in Table 1 below.

[0077] [Table 1]

[0078]

[0079] The following experiment was conducted to analyze the element distribution of the examples.

[0080] <Experimental Example 1-Secondary Ion Mass Spectrometer>

[0081] The thermal diffusion depth of yttrium (Y) element in Example 1 and Example 2 was evaluated using a secondary ion mass spectrometer (hereinafter referred to as "SIMS"). First, in order to minimize the exposure of the sample protective film to the atmosphere, the sample was placed in a purge system, and a portion of the sample protective film was collected and attached to a sample holder for SIMS analysis. While maintaining the purge state, the sample holder was placed in the preparation chamber of the SIMS device, and the preparation chamber was pumped. After being placed in the experimental chamber, an oxygen ion gun was used to quantitatively analyze the yttrium (Y), silicon (Si) and oxygen (O) contents, and a depth profile graph was obtained.

[0082] The depth curves of Example 1 and Example 2 are shown in Figure 3 and Figure 4This takes into account that the positive ionization characteristics of each element are superior to the negative ionization characteristics. For more detailed analysis conditions, please refer to Table 2 below.

[0083] [Table 2]

[0084]

[0085] The SIMS analysis results showed that yttrium (Y) atoms moved to a deeper depth due to diffusion after the heat treatment, and it was confirmed that the yttrium (Y) thermal diffusion depth of Example 1 was 1.97 μm, and the yttrium (Y) thermal diffusion depth of Example 2 was 0.20 μm.

[0086] <Experimental Example 2—X-ray Photoelectron Spectroscopy>

[0087] X-ray photoelectron spectroscopy (XPS) (Thermo Fisher Scientific, using Al Kα (1486.6 eV) X-ray source) was used to investigate the chemical bonding state and atomic content of the specimens before and after plasma treatment. The basic pressure of the specimen chamber was adjusted to 10 -9 To, in the analysis, keep 10 -9 ~10 -7 Torr range. The measured spectra are plotted as a function of electron binding energy versus number of electrons at fixed, small-energy intervals. Peak area and peak height sensitivity factors are used for quantification. All surface compositions shown here are expressed in atomic % (atm %).

[0088] like Figure 5 As shown, the Y three-dimensional orbital exhibits Y 3d3 / 2 and 3d5 / 2 peaks due to LS coupling, and when yttrium oxide is formed, a 3d oxide peak is generated at a lower binding energy position due to chemical shifts. Figure 5 In (B), the surface shows a Y 3d oxide peak after heat treatment. Figure 5 In (D), the Y 3d xidem peak is also detected at depth after heat treatment.

[0089] like Figure 6 As shown in (A) and (B), it is shown that after the heat treatment of Example 3, the Y 3d peak position shifts to a high binding energy position with low chemical shifts. This chemical shift of binding energy is due to the chemical combination with the Al element component in the sapphire component. Figure 6In (C) and (D), it can be observed that the Al 2p peak position diffuses to the surface after the heat treatment of Example 3. This is because the Al component existing on the surface of the sapphire member diffuses into the Y film due to the thermal diffusion phenomenon.

[0090] The heat diffusion depth of Example 3 was measured under the conditions of Table 3. As a result of the analysis, the depth of the heat diffusion layer was confirmed to be 2.0 μm by converting the etching time to reach the diffusion layer based on Al in the member manufactured in Example 3.

[0091] [Table 3]

[0092]

[0093] The above detailed description of the specific parts of the present invention is only a preferred embodiment and does not limit the scope of the present invention. It is self-evident to those skilled in the art that the substantive scope of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for manufacturing a component for a plasma etching device, comprising the following steps: a) depositing a rare earth metal thin film including rare earth metals on a substrate with a thickness of 0.01 μm to 2.0 μm by vacuum deposition; and b) heat treating the substrate on which the rare earth metal thin film is deposited at 1200° C. to 2000° C. for 2 to 40 hours in an atmosphere of air, nitrogen, oxygen or argon; The vacuum deposition method is electron beam physical vapor deposition or sputtering.

2. The method for manufacturing a member for a plasma etching device according to claim 1, wherein: The rare earth metal is any one or more of yttrium, ytterbium and samarium.

3. The method for manufacturing a member for a plasma etching device according to claim 1, wherein: The melting point of the substrate material is above 1000°C.

4. The method for manufacturing a member for a plasma etching device according to claim 1, wherein: The substrate is any one of quartz, alumina sintered body and sapphire.

5. The method for manufacturing a member for a plasma etching device according to claim 1, wherein: The heat treatment time in step b) is 2 hours to 20 hours.

6. A component for a plasma etching device, manufactured by the manufacturing method according to any one of claims 1 to 5, wherein the rare earth metal heat diffusion layer has a thickness of 0.1 μm to 10 μm.

7. A transparent component for a plasma etching device, manufactured by the manufacturing method according to any one of claims 1 to 5, wherein the rare earth metal heat diffusion layer has a thickness of 0.1 μm to 10 μm.