A hole system and rolling method for rolling hexagonal cross-section titanium and titanium alloy profiles

Through hot rolling of elliptical, regular rhombus, special hexagonal and regular hexagonal pass systems and cold rolling shaping of rhombus pass systems, the manufacturing process of hexagonal cross-section titanium and titanium alloy profiles has been optimized and the material utilization rate has been solved. It solves the problems of low production efficiency and low production efficiency, and achieves efficient and low-cost profile processing.

CN111360080BActive Publication Date: 2024-10-15BAOJI TIANGANG TITANIUM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010161630.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-03-10
Publication Date
2024-10-15
Estimated Expiration
2040-03-10

AI Technical Summary

Technical Problem

The existing manufacturing methods of titanium and titanium alloy profiles with hexagonal cross-sections have low material utilization rate, many rolling passes, low production efficiency and high cost.

Method used

A pass system including elliptical pass, regular rhombus pass, special hexagon pass and regular hexagon pass is used for hot rolling to gradually reduce the size of the blank, and then cold rolling and shaping is performed through the rhombus pass to optimize rolling. Process to obtain a hexagonal cross-section profile.

Benefits of technology

The material utilization rate is improved, the number of cold rolling passes is reduced, the processing efficiency is improved, the production cost is reduced, and finished hexagonal cross-section profiles with consistent specifications are obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111360080B_ABST
    Figure CN111360080B_ABST
Patent Text Reader

Abstract

A hole system and rolling method for rolling hexagonal cross-section titanium and titanium alloy profiles, the hole system includes hot rolling hole and cold rolling hole, the hot rolling hole includes elliptical hole, regular rhombus hole, special hexagonal hole and regular hexagonal hole; the cold rolling hole is a rhombus hole. Rolling method: hot rolling a round billet into a square cross-section billet through an elliptical hole and a regular rhombus hole, and then hot rolling it into a regular hexagonal cross-section billet through a special hexagonal hole and a regular hexagonal hole, and finally cold rolling and shaping it through a rhombus hole to obtain a regular hexagonal cross-section finished profile. High raw material utilization, high processing efficiency, and low production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium and titanium alloy profile processing, and particularly relates to a hole system and a rolling method for rolling titanium and titanium alloy profiles with hexagonal cross-sections. Background Art

[0002] At present, the manufacturing method of hexagonal cross-section titanium and titanium alloy profiles is to hot-roll the bar billet to the required size and then polish it, and then cold-roll the polished round profile into a hexagonal cross-section profile through a diamond hole for multiple passes. This method has low material utilization, many rolling passes, low production efficiency and high rolling cost. Summary of the invention

[0003] The invention provides a hole system and a rolling method for rolling titanium and titanium alloy profiles with rectangular cross-sections, so as to overcome the shortcomings of the prior art.

[0004] The technical solution adopted by the present invention is: a hole system for rolling hexagonal cross-section titanium and titanium alloy profiles, the hole system includes a hot rolling hole and a cold rolling hole, the hot rolling hole includes an elliptical hole, a regular rhombus hole, a special hexagonal hole and a regular hexagonal hole; the special hexagonal hole is a hexagonal hole that is symmetrical up and down and left and right, and the angle α between the left and right sides of the hexagonal hole is (97-105)°, and the upper and lower sides are both arc-shaped and symmetrical to each other, which are convex to the center of the hole; the cold rolling hole is a rhombus hole.

[0005] The arc height A of the circular arc is 0.156×h, wherein h is the depth of the special hexagonal hole.

[0006] The included angle β between the left and right sides of the diamond-shaped hole is 120°.

[0007] A method for rolling titanium and titanium alloy profiles with hexagonal cross-sections using the pass system,

[0008] In the first step, the titanium or titanium alloy billet is heated and then sent into an elliptical die to roll out an elliptical billet, and then the elliptical billet is sent into a regular rhombus die to roll out a square billet, and then the square billet is sent into an elliptical die to roll out an elliptical billet, and the elliptical die and the regular rhombus die are gradually reduced, and the rolling is repeated until a square billet of the required specification is rolled;

[0009] In the second step, the square billet rolled in the first step is fed into a special hexagonal die to roll out a special hexagonal billet with concave upper and lower surfaces, and then the special hexagonal billet with concave upper and lower surfaces is rotated 90 degrees and fed into a regular hexagonal die to be rolled into a hexagonal cross-section profile billet.

[0010] The third step is to feed the hexagonal cross-section profile blank obtained in the second step into the diamond hole for cold rolling and shaping for 6-9 times. During rolling, a guide device is used to ensure that four faces of the hexagonal cross-section profile blank are in contact with the four faces of the diamond hole respectively, and the blank is rotated 60° after the previous rolling and then rolled for the next time. After 6-9 rolling passes, each face of the hexagonal cross-section profile blank is cold rolled 2-3 times to obtain a hexagonal cross-section profile finished product.

[0011] The hexagonal cross-section profile blank rolled in the second step is placed in an acid-base bath to complete acid-base washing to remove impurities such as oxide scale and oil stains, and then the third step of cold rolling and shaping is carried out.

[0012] After removing the oxide scale, oil stains and other impurities, the surface of the hexagonal cross-section profile blank is repaired and then subjected to the third step of cold rolling and shaping.

[0013] The present invention optimizes the rolling process by innovatively designing a hole system, and hot-rolls the billet through an elliptical hole and a regular rhombus hole for several times to form a required square cross-section billet, and then hot-rolls it through a special hexagonal hole and a regular hexagonal hole to form a regular hexagonal cross-section billet, and finally cold-rolls it through a rhombus hole to obtain a regular hexagonal cross-section finished profile. Compared with the prior art of cold-rolling a circular profile through a rhombus hole for multiple passes into a hexagonal cross-section profile, not only is the raw material utilization rate high, but also the number of cold rolling passes is reduced, thereby improving processing efficiency and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a schematic diagram of the structure of the hole type required for hot rolling of the present invention;

[0015] Figure 2 It is a structural schematic diagram of the cold rolling pass type of the present invention;

[0016] Figure 3 It is a structural schematic diagram of the special hexagonal hole type of the present invention;

[0017] Figure 4 It is a schematic diagram of the hole system structure of an embodiment of the present invention;

[0018] Figure 5 It is a schematic diagram of the rolling state of the cold rolling pass profile of the present invention. DETAILED DESCRIPTION

[0019] The following is combined with Figure 1-5 The present invention is described in detail with specific embodiments.

[0020] A hole system for rolling titanium and titanium alloy profiles with hexagonal cross-sections, the hole system includes hot rolling hole and cold rolling hole, the hot rolling hole includes elliptical hole, regular rhombus hole, special hexagonal hole and regular hexagonal hole; the special hexagonal hole is a hexagonal hole that is symmetrical up and down and left and right, and the angle α between the left and right sides of the hexagonal hole is (97-105)°, and the upper and lower sides are both circular arcs that are convex to the center of the hole and symmetrical to each other; the cold rolling hole is a rhombus hole. The arc height A of the circular arc is 0.156×h, where h is the depth of the special hexagonal hole.

[0021] The included angle β between the left and right sides of the diamond-shaped hole is 120°.

[0022] Embodiment 1: A method for rolling titanium and titanium alloy profiles with hexagonal cross-sections using titanium and titanium alloy round billets as raw materials.

[0023] In the first step, the φ60mm titanium and titanium alloy round billet is heated and then sent into the elliptical hole type 1 with a specification of 80×21mm to roll out a 47×80mm elliptical billet, and then the 47×80mm elliptical billet is sent into the regular rhombus hole type 2 with a specification of 47.5mm to roll out a 47.5×47.5mm square billet; then the 47.5×47.5mm square billet is sent into the elliptical hole type 3 with a specification of 70×17.5mm to roll out a 40×70mm elliptical billet, and the 40×70mm elliptical billet is sent into the regular rhombus hole type 4 with a specification of 38.2×38.2mm to roll out a 38.2 ×38.2mm square billet; the 38.2×38.2mm square billet is fed into the oval hole 5 with a specification of 58×12.5mm to roll out a 30×58mm oval billet, the 30×58mm oval billet is fed into the regular rhombus hole 6 with a specification of 32×32mm to roll out a 32×32mm square billet; the 32×32mm square billet is fed into the oval hole 7 with a specification of 46×9.4mm to roll out a 24×46mm oval billet, the 24×46mm oval billet is fed into the regular rhombus hole 8 with a specification of 26×26mm to roll out a 26×26mm square billet;

[0024] The second step is to feed the 26×26mm square billet into a special hexagonal die 9 with a specification of 40(L)×8(h)mm for rolling, and roll out a 40×18mm hexagonal billet with concave upper and lower surfaces, and then rotate the 40×18mm hexagonal billet 90° and feed it into a 24×24 regular hexagonal die 10 for rolling, and roll out a 24×24mm hexagonal cross-section profile billet. The angle α between the left and right sides of the special hexagonal die 9 is 100°, and the arc height A of the arc is 0.156×8mm;

[0025] The third step is to put the hexagonal cross-section profile blank rolled in the second step into an acid-base bath for acid-base washing to remove impurities such as oxide scale and oil stains;

[0026] The fourth step is to perform a surface repair treatment on the hexagonal cross-section profile blank after removing impurities such as oxide scale and oil stains. The repair treatment specifically refers to: grinding surface cracks, removing surface burrs, etc., so as to eliminate surface defects of the hexagonal cross-section profile blank;

[0027] The fifth step is to feed the hexagonal cross-section profile blank that has been repaired into a 40×10 mm diamond pass 11 for cold rolling 6-9 times. During rolling, a guide device is used to ensure that four faces of the hexagonal cross-section profile blank are in contact with the four faces of the diamond pass respectively, and the blank is rotated 60° after the previous rolling before the next rolling. After 6-9 rolling passes, each face of the hexagonal cross-section profile blank is cold rolled 2-3 times, and finally a 22×22 mm hexagonal cross-section profile finished product is obtained;

[0028] The sixth step is to straighten the rolled 22×22mm hexagonal section profile through a straightening machine to ensure that the product meets the delivery requirements.

[0029] Embodiment 2: A method for rolling titanium and titanium alloy profiles with hexagonal cross-sections from titanium and titanium alloy square billets.

[0030] After heating the 62mm×62mm titanium and titanium alloy square billet, a 22×22mm hexagonal cross-section profile product can be rolled according to the steps and hole specifications described in Example 1; the specific rolling process is basically the same as that in Example 1 and will not be repeated here.

[0031] The present invention rolls a special hexagonal billet with concave upper and lower surfaces by feeding a square billet into a special hexagonal die, and then rotates the special hexagonal billet 90 degrees and feeds it into a regular hexagonal die for rolling. By extruding the four planes of the special hexagonal billet, the two concave surfaces are extended outward to fill the concave part to form a plane, and the billet is formed into a regular hexagonal cross-section profile, which has high raw material utilization and high processing efficiency. The regular hexagonal cross-section profile billet is then cold-rolled and shaped into a regular hexagonal cross-section finished profile through a rhombus die, and the finished product has good consistency in specifications and dimensions and low production costs.

[0032] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the scope of implementation of the present invention. Therefore, all equivalent changes made to the contents described in the claims of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A hole system for rolling hexagonal cross-section titanium and titanium alloy profiles, characterized in that: The hole profile system includes a hot rolling hole profile and a cold rolling hole profile, and the hot rolling hole profile includes an elliptical hole profile, a regular rhombus hole profile, a special hexagonal hole profile and a regular hexagonal hole profile; the special hexagonal hole profile is a hexagonal hole profile that is symmetrical in the upper and lower parts and in the left and right parts, and the included angle α between the left and right sides of the hexagonal hole profile is (97-105)°, and the upper and lower sides are both circular arcs that are convex to the hole profile center and symmetrical to each other; the cold rolling hole profile is a rhombus hole profile.

2. A hole system for rolling hexagonal cross-section titanium and titanium alloy profiles according to claim 1, characterized in that: The arc height A of the circular arc is 0.156×h, wherein h is the depth of the special hexagonal hole.

3. A hole system for rolling hexagonal cross-section titanium and titanium alloy profiles according to claim 1 or 2, characterized in that: The included angle β between the left and right sides of the diamond-shaped hole is 120°.

4. A method for rolling hexagonal cross-section titanium and titanium alloy profiles using the pass system of claim 1, characterized in that: In the first step, the titanium or titanium alloy billet is heated and then sent into an elliptical die to roll out an elliptical billet, and then the elliptical billet is sent into a regular rhombus die to roll out a square billet, and then the square billet is sent into an elliptical die to roll out an elliptical billet, and the elliptical die and the regular rhombus die are gradually reduced, and the rolling is repeated until a square billet of the required specification is rolled; In the second step, the square billet rolled in the first step is fed into a special hexagonal die to roll out a special hexagonal billet with concave upper and lower surfaces, and then the special hexagonal billet with concave upper and lower surfaces is rotated 90 degrees and fed into a regular hexagonal die to roll into a hexagonal cross-section profile billet; The third step is to feed the hexagonal cross-section profile blank obtained in the second step into the diamond hole for cold rolling and shaping for 6-9 times. During rolling, a guide device is used to ensure that four faces of the hexagonal cross-section profile blank are in contact with the four faces of the diamond hole respectively, and the blank is rotated 60° after the previous rolling and then rolled for the next time. After 6-9 rolling passes, each face of the hexagonal cross-section profile blank is cold rolled 2-3 times to obtain a hexagonal cross-section profile finished product.

5. The method for rolling hexagonal cross-section titanium and titanium alloy profiles according to claim 4, characterized in that: The hexagonal section profile blank rolled in the second step is placed in an acid-base bath to complete acid-base washing to remove oxide scale and oil stains, and then the third step of cold rolling and shaping is carried out.

6. The method for rolling hexagonal cross-section titanium and titanium alloy profiles according to claim 4, characterized in that: The hexagonal cross-section profile blank rolled in the second step is placed in an acid-base bath to complete acid-base washing to remove oxide scale and oil stains. After the surface of the hexagonal cross-section profile blank after the oxide scale and oil stains are removed is repaired, the third step of cold rolling and shaping is performed.