A hot-rolled thin-bellied, ultra-deep variable-section trapezoidal rib and its hot continuous rolling production process

Through hot rolling process and cross-section optimization design, combined with finite element analysis and hot cutting welding technology, the problems of existing ladder rib processing complexity and material waste are solved, and thin-bow, ultra-deep-variable cross-section ladder with economic saving and performance improvement are achieved. rib.

CN111495967BActive Publication Date: 2024-11-12HEBEI JINXI STEEL SHEET PILE SECTION STEEL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010365321.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-30
Publication Date
2024-11-12
Estimated Expiration
2040-04-30

AI Technical Summary

Technical Problem

The processing methods of existing ladder ribs are complex and inefficient, the materials are not economical, and they are prone to fatigue and crack problems, and lack new ladder ribs that are economical and economical and have better performance than cold-bent ladder ribs.

Method used

The thin-bone, ultra-deep variable cross-section ladder ribs are designed by hot rolling process. The Turkish head and thinning web are added through cross-section optimization, and the thickness of the bottom plate is reduced. Combined with hot-cut welding technology, the rib partition is set to improve overall stiffness and torsion resistance. , and optimize the rolling process through finite element analysis.

Benefits of technology

It has achieved a reduction in material use by 1-2%, reduced internal stress, improved welding quality, improved fatigue resistance and economicality, and solved the problems of material waste and stress concentration of existing ladder ribs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111495967B_ABST
    Figure CN111495967B_ABST
Patent Text Reader

Abstract

The present invention discloses a hot-rolled thin-bellied, ultra-deep variable-section trapezoidal rib and its hot continuous rolling production process. The cross-section of the thin-bellied and ultra-deep trapezoidal rib is optimized according to the load stress and strain finite element analysis calculation model, combined with the actual change of the load test stress amplitude, and the cross-section thickness is optimized by considering the welding of the inner and outer partitions and the position of the splicing plate, which can not only improve the force performance and reduce the amount of steel used, but also improve the fatigue resistance of the orthogonal anisotropic bridge deck. During production, the roll hole type is optimized according to the variable section model, and a special ultra-deep, thin-bellied, variable-section slot continuous casting and rolling hot rolling hole type design, continuous rolling process and special equipment are adopted. The initial rolling of the blank adopts the U-shaped cutting method, and the rough rolling adopts the upper roller large pressure down cutting rolling process to form the optimal metal elongation; the outer hole type of the finishing rolling web is a straight oblique line shape that remains unchanged, and the inner side of the web changes through a reasonable hole type slope, and forms a Turkish head through R angle gradual continuous rolling, and the bottom web adopts double R angle transition to form the best curvature arc radius.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of trapezoidal rib design and processing, and in particular to a hot-rolled thin-bellied, ultra-deep variable-section trapezoidal rib and a hot continuous rolling production process thereof. Background Art

[0002] At present, the trapezoidal ribs of domestic orthotropic plates are all formed by cold bending of flat plates, which has obvious shortcomings and defects:

[0003] 1. The processing method adopts manual or semi-mechanized production, with complex procedures, difficult processing and low efficiency, including leveling, cutting, milling, bending, shaping, drilling, etc., with high difficulty in quality control, poor processing accuracy and large internal stress of cold-formed structure;

[0004] 2. Due to the uniform thickness of the steel plate, the thin belly and the complex stress of the ultra-deep trapezoidal ribs, the stress and strain of each part are different, especially the end welding thickness is not enough due to the restriction of the plate thickness. After removing the blunt edge, the weld thickness is only 70%~75% of the plate thickness, and the weld is eccentrically stressed, where the stress amplitude is the largest, the residual stress is concentrated, and fatigue cracks are easily generated;

[0005] Although some existing patents have proposed designs of local thickening to reduce stress, there are no mature products on the market, and the existing improved technical solutions use more materials per linear meter than the existing cold-bent trapezoidal ribs, which is not economical. Therefore, it is a problem to be solved in the industry to design a new type of trapezoidal rib that uses less steel, is economical, and has indicators such as maximum deformation, stress and durability that are equal to or better than the existing cold-bent trapezoidal ribs. How to realize the production of new trapezoidal ribs is also a technical problem to be solved. Summary of the invention

[0006] In view of the shortcomings of the prior art, the first purpose of the present invention is to provide a hot-rolled thin-bellied, ultra-deep variable-section trapezoidal rib, which has the advantages of economic savings, small internal stress, and various material properties and technical indicators that are superior to existing products.

[0007] The above-mentioned purpose of the present invention is achieved through the following technical scheme: adopting the U-2 equal-thickness U-shaped rib in the industry standard YB / T4624-2017 as the basic cross-section structure, the depth of the thin-bellied, ultra-deep variable-section trapezoidal rib formed by the hot rolling process is 280mm, the thickness of the bottom plate is thickened to 10mm, the thickness of the upper end of the web is thickened to 10mm to form a Turkish head, and the thickness of the straight section of the web is thinned to 7mm; the variable section of the straight section of the web and the Turkish head at the top of the web and the variable section of the bottom plate and the web are smoothly transitioned.

[0008] Through the above technical scheme, the trapezoidal rib is designed to be thickened within the high stress amplitude line range of the web end where the stress is the largest, forming a Turkish head. The plate thickness is appropriately thinned at the low stress amplitude part where the stress is small on the web, and the bottom plate with greater stress is thickened. Through the above cross-section optimization, the steel consumption of the product is reduced by about 1-2% compared with the existing cold-rolled trapezoidal rib on the basis of improving material performance and technical indicators. At the same time, the trapezoidal rib processed by hot rolling reduces stress concentration. The trapezoidal rib with changed cross-sectional dimensions according to the changes in the stress of each part of the product makes the stress distribution more uniform, especially reducing the stress at the weld between the end of the trapezoidal rib and the bridge deck, thereby improving the fatigue resistance and durability of the trapezoidal rib. At the same time, due to the reduction in the thickness of the web, steel is greatly saved and the economy is improved.

[0009] The present invention is further configured as follows: the thickened portion of the Türkiye head at the end of the trapezoidal rib web is located on the inner side of the web, and the outer side wall of the web is a plane.

[0010] The above technical solution does not affect the welding between the outer wall of the web and the diaphragm, thereby improving the welding quality.

[0011] The present invention is further configured such that the end of the trapezoidal rib is formed into an arc-shaped weld groove by hot cutting.

[0012] Through the above technical solution, the amount of weld metal deposition is reduced and the welding quality is improved.

[0013] The present invention is further configured as follows: a plurality of rib inner partitions are arranged inside the trapezoidal ribs at intervals, and two side edges of the rib inner partitions are welded to the inner wall of the trapezoidal ribs.

[0014] Through the above technical solution, the overall stiffness and torsional resistance of the trapezoidal ribs are increased, and weld cracking between the trapezoidal ribs and the arc-shaped incisions of the transverse partitions is eliminated.

[0015] The second object of the present invention is to provide a hot rolling production process for hot-rolled thin-bellied, ultra-deep variable-section trapezoidal ribs. The third object is to provide trapezoidal ribs produced by hot rolling technology, which has the advantages of being able to realize the processing of ultra-deep variable-section trapezoidal ribs, with simple steps and reliable quality of the produced trapezoidal ribs.

[0016] The above object of the present invention is achieved through the following technical solution: The process comprises the following processing steps:

[0017] Blooming and initial rolling: the billet is placed vertically, and the billet height is greater than the final depth of the trapezoidal rib; the billet enters the initial rolling mill, and the upper and lower surfaces of the billet are U-shaped cut in the first pass; the upper surface of the billet is further U-shaped cut in the second pass, and the lower surface of the billet is flattened, so that the bottom plate of the trapezoidal rib has sufficient metal volume; by cutting the upper surface of the billet, the web part has sufficient metal volume; after blooming and initial rolling, the height of the billet is less than the designed depth of the trapezoidal rib;

[0018] Secondary rough rolling: The first pass makes the angle between the bottom and the outer side of the billet basically the same as the angle between the designed trapezoidal rib bottom plate and the web plate. After this pass, the outer bottom surface of the billet is basically formed and the amount of metal is basically fixed; multiple passes continue to U-cut the upper surface with high pressure, and the hole shape of the last pass makes the height of the billet less than the designed depth of the trapezoidal rib;

[0019] Finishing rolling: In the first pass, the upper surface is continued to be U-shaped cut, and the web height is increased to close to the designed web height; in the second pass, the bottom plate and web thickness are continued to be thinned, and the web height is reduced by 7%-20%; in the third pass, the bottom plate and web thickness are continued to be thinned, and the web height is increased to the designed web height; in the subsequent passes, the bottom plate and web thickness are continued to be thinned, and the Turkish head at the top of the web is pressed out through a closed hole, and then the end of the rolled piece is hot cut to form a welding groove; in each pass of finishing rolling, the variable cross-sections of the trapezoidal rib are simultaneously processed with smooth transition, and finally a hot-rolled thin-webbed, ultra-deep variable-section trapezoidal rib is formed.

[0020] Through the above technical scheme and the above process, the metal quantity at the bottom plate and the web is guaranteed. Through the measures of raising, lowering, and raising the web height in the finishing rolling step, the web reaches the optimal metal quantity, and the web and bottom plate reach the optimal metal elongation. The Turkey head at the top of the web is pressed out through a closed hole die, so that the Turkey head has enough metal quantity, ensuring the processing accuracy of this part; at the same time, through reasonable processing, the trapezoidal ribs with complex variable cross-sections and ultra-deep and ultra-thin webs are processed and formed.

[0021] The present invention is further configured as follows: the rough rolling and finish rolling steps also include a cycle of 1-2 open holes-closed holes-open holes, and the upper end surface of the web of the rolled piece is pressed down through the closed hole profile.

[0022] Through the above technical solution, by reasonably setting the cycle of open hole-closed hole-open hole, it is ensured that there is sufficient metal on the upper end of the web.

[0023] The present invention is further configured as follows: during the finishing rolling process, after the web is first formed into an inverted trapezoidal cross section, a Turkish head at the top of the web is pressed out through a closed hole die, and a smooth transition is made between the straight section of the web and the Turkish head.

[0024] Through the above technical solution, the inverted trapezoidal cross-section ensures that there is sufficient metal at the upper end of the web, while improving the forming accuracy of the web end.

[0025] The present invention is further configured as follows: before the initial rolling of the slab, a finite element analysis model is established using finite element analysis software, an elasto-plastic thermo-mechanical coupling simulation is performed on the hot rolling process pass system of the variable-section thin belly and ultra-deep trapezoidal rib, the hot rolling process is calculated, the filling condition and rolling force condition of the rolled piece obtained by the simulation are comprehensively analyzed, the stress and strain distribution and heating temperature of typical passes, and the metal flow law are analyzed, and the pass system and rolling parameters are optimized.

[0026] Through the above technical solution, the hot rolling passes, hole types and parameters are simulated in advance on the software, so that they can be continuously corrected, reducing the number of factory tests and greatly saving test costs. It is particularly suitable for the processing and production of trapezoidal ribs of non-standard sizes.

[0027] In summary, the present invention has the following beneficial effects:

[0028] 1. Through cross-section optimization and hot-rolled production, the variable-section thin belly and ultra-deep trapezoidal ribs not only have small internal stress and large weld thickness, but also have better material properties and technical indicators than the existing cold-rolled trapezoidal ribs. In addition, the steel consumption is reduced by 1-2% year-on-year, which greatly improves the economy and durability of orthotropic plates and solves the problem that the industry has always wanted to break through.

[0029] 2. By setting the inner rib partition, the overall rigidity and torsional resistance of the trapezoidal rib are increased, and the weld cracking between the trapezoidal rib and the arc-shaped incision of the transverse partition is eliminated;

[0030] 3. The hot-rolled profiles with thin belly and ultra-deep grooves with complex cross-sections have complex deformation process of hot rolling and great difficulty in precision control, which places high requirements on the entire rolling process and equipment. The present invention has repeatedly tested and optimized the hot rolling process of variable-section thin belly and ultra-deep trapezoidal ribs, especially the design of each hole type, to achieve the technical effect of smooth surface of rolled workpiece, small residual stress inside the metal, good metallographic structure and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Design cross-section diagram for hot-rolled thin-web and ultra-deep trapezoidal rib variable section;

[0032] Figure 2 It is a schematic diagram of the welding and longitudinal extension connection between the hot-rolled variable-section thin-web, ultra-deep trapezoidal rib and the bridge deck (or bridge bottom deck), transverse diaphragm, and rib inner diaphragm;

[0033] Figure 3 for Figure 1 A partial enlarged view of the middle Türkiye head;

[0034] Figure 4 This is a schematic diagram of the U-2 ladder-type auxiliary force model in the industry standard;

[0035] Figure 5Schematic diagram of the stress model of hot-rolled variable-section trapezoidal rib designed for variable cross-section;

[0036] Figure 6 This is a schematic diagram of the maximum deformation of the U-2 model ladder type;

[0037] Figure 7 Schematic diagram of maximum deformation of hot-rolled variable-section trapezoidal rib;

[0038] Figure 8 This is the U-2 model ladder-type auxiliary stress distribution diagram (with emphasis on the stress distribution at the weld);

[0039] Fig. 9 This is the stress distribution diagram of hot-rolled variable-section trapezoidal rib (with emphasis on the stress distribution at the weld);

[0040] Fig.10 This is the stress distribution diagram of the trapezoidal rib of the U-2 model (with emphasis on the stress distribution on the web);

[0041] Fig.11 This is the stress distribution diagram of hot-rolled variable-section trapezoidal rib (with emphasis on the stress distribution on the web);

[0042] Fig.12 , 13 This is the hole type diagram of the initial rolling M and K holes;

[0043] Fig.14 , 15 , 16 for secondary rough rolling J, I, H hole Hole pattern diagram;

[0044] Figure 17-22 This is the hole pattern diagram of finishing rolling 1-6 (i.e. GB hole);

[0045] Fig.23 This is an enlarged schematic diagram of the Türkiye head at finishing rolling 6 (i.e. B hole);

[0046] Fig.24 This is the hole pattern diagram of finishing rolling 7 (i.e. hole A).

[0047] Figure numerals: 1, web; 11, Turkey head; 12, straight section of web; 2, weld groove; 3, bridge deck; 4, bottom plate; 5, spliced ​​plate; 6, cross partition; 7, rib inner partition; H, trapezoidal rib depth (or leg height); B1, opening width; B2, bottom plate width; R1, inner fillet radius; R2, outer fillet radius. DETAILED DESCRIPTION

[0048] The present invention is further described in detail below in conjunction with the accompanying drawings.

[0049] Embodiment 1: A hot-rolled thin-bellied, ultra-deep variable-section trapezoidal rib. The cross-section thickness of the thin-bellied, ultra-deep trapezoidal rib is optimized based on the load stress, strain finite element analysis calculation model, taking into account the welding of inner and outer partitions and the position of the splicing plate 5, so that the design size is more conducive to the stress state of the thin-bellied, ultra-deep trapezoidal rib, reduces the amount of steel used, and improves the fatigue resistance of the orthotropic bridge deck.

[0050] Specifically, the basic dimensions can be any type of equal-thickness U-shaped rib in the industry standard "Cold-formed steel with trapezoidal ribs for bridge steel structures" (YB / T4624-2017), and the finite element analysis calculation model can be used to perform force analysis and load fatigue tests based on the technical requirements of the trapezoidal ribs, section characteristic parameters, load stress, and strain conditions, and the section thickness optimization design can be performed by comprehensively considering the welding with the inner and outer partitions and the position of the splicing plate 5. Figure 1 As shown, the trapezoidal rib of model U-2 in the industry standard is introduced as an example. The depth H (i.e., limb height or leg height) of the trapezoidal rib is 280mm, the opening width B1 is 300mm, the width B2 of the bottom plate 4 is 170mm, and the thickness is 8mm. Taking this model of trapezoidal rib as the basic external dimensions, the thickness of its bottom plate 4 is increased by 2mm; the thickness of the upper end of the web 1 is increased by 2mm to form a Turkish head 11; the thickness of the straight section 12 of the web is reduced by 1mm; the variable cross-sections of the bottom plate 4 and the web 1, as well as the straight section 12 of the web and the top of the web 1 are all smoothly transitioned. The depth of the hot-rolled trapezoidal rib finally formed is 280mm, the thickness t1 of the bottom plate 4 is 10mm, the thickness t3 of the Turkish head 11 at the upper end of the web 1 is 10mm, and the height can be 24mm; the thickness t2 of the straight section 12 of the web is 7mm. The inner fillet radius R1 of the transition section between the bottom plate 4 and the web 1 is 38 mm, and the outer fillet radius R2 is 46 mm. Figure 2 The thickness of the Türkiye head 11 and the straight section 12 of the web adopts double R angle transition, and the transition height is 30-50mm.

[0051] The steel consumption is calculated as follows:

[0052] The inclined length of the trapezoidal rib web 1 of model U-2 in the industry standard is 286 mm. Since the width B2 of the bottom plate 4 includes the rounded arc section, the actual thickened width of the bottom plate 4 is less than 170 mm, and the value can be 160 mm.

[0053] The base plate 4 increases the thickness by 2mm×width by 160mm=320mm².

[0054] Two Türkiye heads 11 increase thickness 2mm × (height 20~30mm) × 2 = 80~120mm²

[0055] Total increase 400~440mm²

[0056] Web 1 reduced thickness 1mm × (length 210~250mm) * 2 = 420~500mm²

[0057] Finally, the trapezoidal ribs are reduced by 20~60mm³ per linear meter.

[0058] Further, combined with Figure 1 and Figure 2 In order to facilitate the welding of the trapezoidal rib and the diaphragm 6, the thickened part of the upper Turkish head 11 of the hot-rolled trapezoidal rib web 1 is located on the inner side of the web 1, and the outer wall of the web 1 is a flat oblique line. The length of the straight section 12 of the web is much larger than the width of the splicing plate 5 used for the longitudinal extension of the trapezoidal rib, which facilitates the connection. In order to reduce the amount of weld metal deposition and improve the welding quality, and reduce the stress concentration at the weld between the end of the trapezoidal rib and the bridge deck 3, the end of the trapezoidal rib is formed into a concave arc-shaped weld groove 2 by hot cutting (see Figure 3 ). In order to increase the anti-torsion performance of the trapezoidal rib and eliminate the cracking of the weld between the trapezoidal rib and the arc-shaped incision of the transverse partition, multiple rib inner partitions 7 are arranged inside the trapezoidal rib at intervals, and the two sides of the rib inner partition 7 are welded to the inner wall of the trapezoidal rib. The trapezoidal rib is a part of the orthotropic plate, and the orthotropic plate includes the transverse partition 6. The rib inner partition 7 corresponds to the transverse partition 6 of the orthotropic plate.

[0059] The following compares the new hot-rolled trapezoidal ribs of the present embodiment with the existing cold-rolled trapezoidal ribs, and analyzes the key indicators. Figure 4 and Figure 5 As shown in the figure, the same force is constructed on the existing model of equal-thickness cold-rolled trapezoidal rib (thickness is 8mm) and ultra-deep variable-section trapezoidal rib. The following results are obtained after analysis using ABAQUS finite element analysis software:

[0060] contrast Figure 6 and Figure 7 The maximum deformation of ultra-deep variable-section trapezoidal ribs is the same as that of cold-rolled trapezoidal ribs of equal thickness, both of which are 2.3. Figure 7 and Figure 8 The maximum stress of the cold-rolled trapezoidal rib with equal thickness is reduced from 104.9 to 104.4 for the ultra-deep variable-section trapezoidal rib, and the ultra-deep variable-section trapezoidal rib is reduced by 0.5. Figure 8 and Fig. 9 as well as Fig.10 and Fig.11, as can be seen from the heat-affected zone in the figure, the stress distribution of the ultra-deep variable-section trapezoidal ribs is more uniform. The light white area of ​​the ultra-deep variable-section trapezoidal ribs at the weld is longer and has a larger range, indicating that the stress at the weld is smaller, and the maximum stress is also smaller and more uniform, thereby reducing the fatigue stress amplitude and increasing the fatigue life. The strength damage and fatigue damage of steel structures both start from the weakest part. After the cross-section is optimized, not only materials are saved, but also better effects are achieved in various technical indicators, and the fatigue resistance of the trapezoidal ribs is improved. This is something that technicians in this field cannot imagine based on the existing technology. At the same time, the trapezoidal ribs processed by hot rolling reduce stress concentration. Therefore, this product solves the problem that the industry has always wanted to solve but has not solved, and fills the domestic gap.

[0061] Example 2: A hot rolling production process for hot-rolled thin-bellied, ultra-deep variable-section trapezoidal ribs, taking the trapezoidal rib of model 1 in Example 1 as an example, includes the following processing steps:

[0062] The production and processing technology is divided into three main steps: initial rolling of slab, secondary rough rolling and finishing rolling. The initial rolling of slab adopts two hole types: M hole and K hole, with a total of 5 passes; the secondary rough rolling adopts three hole types: J, I, H holes, with a total of three passes; the finishing rolling adopts 7 hole types: G, F, E, D, C, B, A holes (corresponding to finishing rolling 1-7), with a total of 7 passes for continuous rolling.

[0063] The rough rolling of the slab is carried out by a two-roll reversible BD1 mill, the secondary rough rolling is carried out by a BDU mill (a two-roll reversible hole-type BD2 mill with an anti-stuck device and automatic roll changing), and the finishing rolling is carried out by a universal mill.

[0064] Before hot rolling of the trapezoidal ribs, the ABAQUS finite element analysis software is used to establish an elastic-plastic finite element analysis model, and the elastic-plastic thermal-mechanical coupling simulation of the hot rolling process pass system of the variable-section thin-bellied and ultra-deep trapezoidal ribs is carried out to calculate the hot rolling process, comprehensively analyze the simulated filling conditions and rolling force conditions of the rolled pieces, analyze the stress and strain distribution and heating temperature of typical passes, and the metal flow law, and optimize the pass system and rolling parameters; a special ultra-deep, thin-bellied, variable-section groove continuous casting and rolling hot rolling pass design, continuous rolling process and special equipment are used.

[0065] Initial rolling: During BD1, the F2 billet (height 230*width 350) or F3 billet (height 320*width 410) is turned 90° by the front pusher, so that the original height of the billet is fully guaranteed to be 1.2-1.5 times greater than the required height (280mm); Fig.12 As shown, the upper and lower surfaces of the M-type hole are both divided by U-shaped micro-cutting method, the "wedge" of the upper roller is sharper, and the "wedge" of the lower roller is blunter.

[0066] like Fig.13As shown, the K-hole lower roller adopts a flat rolling method, and the upper roller adopts a U-shaped large cutting method, increasing the downward pressure to continue to increase the metal amount of the web 1 and flatten the bottom of the billet. By first U-shaped micro-cutting the bottom plate 4 and then rolling it flat, the bottom plate 4 can obtain sufficient metal, and the surface oxide scale can be removed to ensure the surface quality; by high-pressure cutting on the upper surface of the billet, the web 1 part can obtain sufficient metal.

[0067] Due to the large width of the continuous casting billet, the box-type holes M and K are used for high-piece vertical rolling to make the billet size reach the required width. The box-type holes M and K are symmetrical up and down and left and right, and are configured on the BD1 billet mill. After rolling through the holes M and K, the inner fillet radius R1 of the billet is 108-112mm, the outer fillet radius R2 of the bottom is 53-57mm, and the width of the bottom of the billet is 220mm.

[0068] Secondary rough rolling: After the initial rolling of the slab, the slab with the initial outer bottom surface is put into the BDU rolling mill. Fig.14 As shown, the J-type continues to use the upper roller to cut with high pressure, and the J-type adopts the edge rolling closed-mouth type. The outer arc radius of the closed-mouth hole of the upper roller of the J-type is 120mm, and the innermost arc radius is 100mm. The rounded corners are set here to facilitate material removal, and the upper roller adopts a reasonable amount of pressure control. The inner side angle of the lower roller is close to the final trapezoidal rib web 1 angle, which can be 3 to 8 degrees larger than the final angle. In this embodiment, the inner side angle of the lower roller is 107 degrees, which is 5 degrees larger than the final trapezoidal rib web 1 angle of 102 degrees. The lower inner chamfer arc transition has a radius of 350mm; the height of the rolled piece is 220mm. Since the J-type has a large deformation amount, uneven deformation, and the rolling of the outer side of the blank must be basically finalized, it is very critical. After this pass, the outer bottom surface of the blank is basically formed, and the surface of the rolled workpiece is smooth, the amount of metal is basically fixed, and the residual stress inside the metal is small.

[0069] like Fig.15 As shown, the I-type hole is an open hole type, and the upper roller continues to press down and cut; the lower inner chamfer arc transition has a radius of 380mm; the height of the rolled piece (i.e., the height of the web 1 or the leg height) increases to 270mm.

[0070] like Fig.16 As shown, the H-type is a closed-end rolling hole type. The upper roller continues to press down and cut, and the outermost side of the closed hole of the upper roller is pressed down obliquely to change the metal volume again to ensure that the end is flush. The height of the rolled piece is reduced to 206.6mm;

[0071] For hole types J, I, and H, the upper rollers continue to use the deep arc cutting method, and the lower rollers use the flat rolling method to roll the inner fillet radius R1 to 48-52mm and the outer fillet radius R2 to 35-40mm.

[0072] After initial rolling and secondary rough rolling, the rectangular billet coming out of the heating furnace is processed into the shape required by the universal rolling mill, so that the thickness of each part of the cross-section of the rolled piece basically meets the finished product size requirements and is initially formed.

[0073] The three hole types of BDU are closed hole-open hole-closed hole in order, which can ensure that there is sufficient metal on the top of the web 1.

[0074] Finishing rolling: 1 / 3 / 4 / 5 / 7 of finishing rolling are open pass types, 2 / 6 are closed edge rolling pass types, and finishing rolling adopts continuous rolling process. Through reasonable configuration, it can not only achieve smooth rolling but also obtain accurate size and surface quality, and realize the rolling of variable cross-section ultra-deep thin belly and ultra-deep trapezoidal rib;

[0075] like Fig.17 As shown, the first stand of the finishing rolling presses down the gap of the rollers by 9.6mm, so that the bottom thickness is reduced from 50mm to 41.4mm, and the leg height is increased from 206.6mm to 270mm; the hole compression is continued in the first stand of the finishing rolling, so that the inner fillet radius R1 is changed to 36-40mm, and the outer fillet radius R2 is changed to 43-47mm; that is, the smooth transition of the inner and outer fillets is rolled into a preliminary shape. The inner side angle of the lower roller is the same as the angle of the final trapezoidal rib web 1, which is 102 degrees in this embodiment. The first stand reduces the inner fillet radius R1 of the rolled piece, increases the outer fillet radius R2, and reduces the inner side angle of the lower roller, so that the cross-section of the web 1 is formed into an inverted trapezoidal structure, providing favorable conditions for the formation of the final turkey head 11 of the trapezoidal rib.

[0076] The second to seventh stands are used to release the rolling heat stress inside the rolled piece during multiple rolling processes, which not only achieves a perfect transition in weight reduction and aesthetics, but also reduces the internal stress caused by the rolling process.

[0077] like Fig.18 As shown, the second stand presses down the roll gap by 8.6mm, so that the bottom thickness is reduced from 41.4mm to 32.8mm. At the same time, by reducing the roll groove depth, the height of the web 1 (i.e., the leg height) is reduced by 7%-20%. Specifically, the leg height can be reduced from 270mm to 239.8mm. This process is a forced extension process, the purpose of which is to reduce the metal amount of the web 1 part to further obtain the final reasonable metal amount, and it mainly plays the role of rolling edge;

[0078] like Fig.19 As shown, the third stand presses down the roller gap by 7.5mm, so that the bottom thickness is reduced from 32.8mm to 25.3mm, and the leg height is increased from 239.8mm to 282.8mm. This process is a joint process of extension and leg lengthening, and the main purpose is to increase the leg height of this thin-bellied, ultra-deep trapezoidal rib to the final height and obtain the final height dimension.

[0079] like Fig. 20 and 21 As shown, the fourth and fifth finishing stands continue to press down the roll gap, so that the thickness of the bottom plate 4 continues to become thinner; the hole design of the fifth stand makes the web 1 become an inverted trapezoidal cross section (wedge-shaped cross section).

[0080] Combination Fig. 22 and 23 After the fifth stand of finishing rolling adopts natural filling, the sixth stand of finishing rolling adopts the design of closed-mouth hole profile with edge rolling, combined with the inverted trapezoidal cross-section design of the fifth stand, to ensure that there is sufficient metal on the upper end of the web 1, which is convenient for the precise forming of the Turkey head 11 of the rolled piece and improves the forming accuracy of the end. At the same time, the end of the rolled piece is hot-cut by edge rolling to form the final arc-shaped weld groove 2. The hole profile of the sixth stand of finishing rolling realizes the thickening of the end of the web 1, the fixed thickness of the straight section 12 (thin wall) of the web, and the smooth transition between the inner side of the straight section 12 of the web and the double R angle of the thickened section; Fig.23 As shown, the welding groove is formed by pressing down the closed hole and hot cutting. Its nodes are controlled by the size of the innermost arc radius of the closed hole of the upper roller and the reasonable reduction amount of the rolling process, so as to achieve precise control of the nodes of the welding groove of the Turkish head 11. In this embodiment, the fillet radius is 15-20mm, the rolling process is given by a reduction of 2-3mm, the rolling temperature is 800-880℃, and a single-pass hot cutting is formed in one time. The height of the trapezoidal rib after the sixth frame is rolled is 261.1mm, and the inner fillet radius R1 is changed to 38.4mm and the outer fillet radius R2 is changed to 48.5mm.

[0081] like Fig.24 As shown, the seventh stand makes corrections to the hot-rolled trapezoidal ribs, mainly increasing the height of the trapezoidal ribs to 280 mm, rolling the outer surface of the web 1 flush, and changing the inner fillet radius R1 to 38 mm and the outer fillet radius R2 to 46 mm.

[0082] The hot rolling process is designed to consist of 12 links and 15 rolling passes, including five passes for BD1, three passes for BD2, and seven passes for the universal rolling mill. The pass distribution is 3+2-3-6+1.

[0083] The thickness of the bottom plate 4 and the Turkey head 11 of the finished size of the hot-rolled variable-section thin belly and ultra-deep trapezoidal rib is 10 mm, and the thickness of the web 1 connected to the two is 7 mm. Therefore, only by matching the inner and outer fillet radii gradually during the rolling process can a smooth transition fillet be obtained, making the inner and outer fillets smooth and beautiful.

[0084] In the present application, parameters such as temperature control in the hot rolling process are well-known technologies in the art and are not the improvement direction of the present application. For details, please refer to the production process of hot-rolled Larsen steel sheet piles, which will not be repeated here.

[0085] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A hot rolling production process for hot-rolled thin-web, ultra-deep variable-section trapezoidal ribs, wherein the produced trapezoidal ribs adopt the U-2 equal-thickness U-shaped ribs in the industry standard YB / T4624-2017 as the basic cross-section structure, wherein the trapezoidal ribs include a bottom plate (4) and a web (1), wherein the upper end of the web (1) is thickened to form a Turkish head (11), and the thickness of the straight section (12) of the web is thinned, wherein the trapezoidal ribs are characterized by: The processing steps include: Blooming and initial rolling: the billet is placed vertically, and the billet height is greater than the final depth of the trapezoidal rib; the billet enters the initial rolling mill, and the upper and lower surfaces of the billet are U-cut in the first pass; the upper surface of the billet is further U-cut in the second pass, and the lower surface of the billet is flattened; after blooming and initial rolling, the height of the billet is less than the designed depth of the trapezoidal rib; Secondary rough rolling: in the first pass, the angle between the bottom surface and the outer side surface of the blank is basically the same as the angle between the designed trapezoidal rib bottom plate (4) and the web plate (1), and the outer bottom surface of the blank is basically formed after this pass; multiple passes continue to cut the upper surface into a U-shape with high pressure, and the hole shape of the last pass makes the height of the blank smaller than the designed depth of the trapezoidal rib; Finishing rolling: In the first pass, the upper surface is continuously U-shaped cut, and the height of the web (1) is increased to a height close to the designed web (1); in the second pass, the thickness of the bottom plate (4) and the web (1) is continuously thinned, and the height of the web (1) is reduced by 7%-20%; in the third pass, the thickness of the bottom plate (4) and the web (1) is continuously thinned, and the height of the web (1) is increased to the designed web (1) height; in the subsequent passes, the thickness of the bottom plate (4) and the web (1) is continuously thinned, and a Turkish head (11) is pressed out at the top of the web (1) through a closed die, and then the end of the rolled piece is hot-cut to form a welding groove; in each pass of the finishing rolling, each variable section of the trapezoidal rib is simultaneously subjected to a smooth transition process, and finally a hot-rolled thin-webbed, ultra-deep variable-section trapezoidal rib is formed.

2. The hot rolling production process of hot-rolled thin-bellied, ultra-deep variable-section trapezoidal ribs according to claim 1 is characterized by: The rough rolling and finish rolling steps also include 1-2 passes of closed-mouth die to press down the upper end surface of the web (1) of the rolled piece.

3. The hot rolling production process of hot-rolled thin-bellied, ultra-deep variable-section trapezoidal ribs according to claim 1 is characterized by: During the finishing rolling process, the web (1) is first formed into an inverted trapezoidal cross section, and then a Turkish head (11) at the top of the web (1) is pressed out through a closed die, and a smooth transition is made between the web straight section (12) and the Turkish head (11).

4. The hot rolling production process of hot-rolled thin-bellied, ultra-deep variable-section trapezoidal ribs according to claim 1 is characterized by: Before the initial rolling of the slab, the finite element analysis software is used to establish an elastic-plastic finite element analysis model, and the elastic-plastic thermal-mechanical coupling simulation of the hot rolling process hole system of the variable-section thin belly and ultra-deep trapezoidal rib is carried out. The hot rolling process is calculated, the simulated filling condition and rolling force of the rolled piece are comprehensively analyzed, the stress and strain distribution, heating temperature and metal flow law of typical passes are analyzed, and the hole system and rolling parameters are optimized.

5. A hot-rolled thin-web, ultra-deep variable-section trapezoidal rib, characterized in that The trapezoidal rib is formed by the hot continuous rolling production process of the trapezoidal rib described in any one of claims 1 to 4.