Explosion-proof boiler tube with double protection and preparation method thereof

By adopting double protection measures on the boiler pipes, we ensure that the life of the inner and outer wall coatings is the same. The coating and substrate are synchronized by using high-frequency induction remelting heat source, which solves the problems of short life of the boiler pipe and explosive pipes, and achieves efficient corrosion protection and Improved durability.

CN111520702BActive Publication Date: 2024-12-06JIANGSU KEHUAN INNOVATIVE MATERIAL CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010503426.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-05
Publication Date
2024-12-06
Estimated Expiration
2040-06-05

AI Technical Summary

Technical Problem

The average service life of the four boiler pipes in harsh environments is short, and it is prone to pipe bursting. The existing coating protection technology is not effective and cannot effectively extend the life of the pipe.

Method used

Using double protection measures, the outer wall and inner wall of the boiler pipe are covered with alloy anticorrosion coating. The remelting of the inner and outer wall coatings and normalizing treatment of the pipe matrix through high-frequency induction remelting heat source are achieved simultaneously to ensure the same life of the inner and outer wall coatings. Avoid shortcomings.

Benefits of technology

It significantly improves the comprehensive anti-corrosion performance and service life of the pipeline, reduces costs, reduces the risk of pipe bursting, and improves the high-temperature fatigue and creep resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111520702B_ABST
    Figure CN111520702B_ABST
Patent Text Reader

Abstract

The present invention relates to an explosion-proof boiler tube with double protection and a preparation method thereof. The explosion-proof boiler tube comprises a boiler tube, an outer wall anti-corrosion coating coated on the outer wall of the boiler tube, and an inner wall anti-corrosion coating coated on the inner wall of the boiler tube, wherein the anti-corrosion coating is an alloy anti-corrosion coating; the thickness of the outer wall anti-corrosion coating is 0.5±0.1mm, the thickness of the inner wall anti-corrosion coating is 0.2±0.1mm, and the substrate of the boiler tube has been normalized. As a result, the explosion-proof boiler tube in the present invention becomes a "double-protected medium-strong" explosion-proof boiler tube with double protection, and the service life of the inner wall and outer wall anti-corrosion coatings can reach more than 6 years. The present invention utilizes a set of high-frequency induction remelting heat sources used for the outer wall coating of the tube, and can simultaneously achieve the triple effects of remelting treatment of the inner wall and outer wall coatings of the tube and normalizing treatment of the substrate with only one process, thereby achieving a significant improvement in the comprehensive anti-corrosion performance and service life of the pipeline at a relatively low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal pipeline protection, and relates to an explosion-proof boiler pipe with double protection and a preparation method thereof. Background Art

[0002] Since the beginning of the 21st century, with the implementation of the country's major circular economy policies, my country's waste incineration power generation has entered a rapid development track, with a blowout in the scale of installed power generation capacity and power generation, and has now jumped to the first place in the world. In recent years, with the continuous increase in high-parameter garbage power plants, the average service life of the four boiler tubes, especially the water-cooled wall, superheater, and reheater tubes, is only 1-3 years in harsh working environments. In severe cases, pipe bursts may occur after only more than half a year of use. Although a variety of coating protection technologies have been developed in recent years, and the life of the pipeline can be greater than 3 years, the effect is still unsatisfactory, and the wall thickness is thinned to the point of bursting. Therefore, preventing the wall thickness of the four boiler tubes from thinning to the point of bursting and effectively extending the life of the pipeline has become a technical problem that has always been wanted to be solved in this field but has not been solved. Summary of the invention

[0003] One of the purposes of the present invention is to provide an explosion-proof boiler tube with double protection. The outer wall and the inner wall of the boiler tube are both covered with alloy anti-corrosion coatings, and the service life of the two is the same without any shortcomings.

[0004] The second object of the present invention is to provide a method for preparing the above-mentioned explosion-proof boiler tube with double protection. The method uses a high-frequency induction remelting heat source on the outer wall coating of the boiler tube to fully tap the potential of the heat source, and can simultaneously achieve the triple effects of remelting the inner and outer wall coatings and normalizing the tube matrix in only one process. Without spending special preparation time and additional cost, the comprehensive anti-corrosion performance and service life of the pipeline can be greatly improved.

[0005] To this end, the first aspect of the present invention provides an explosion-proof boiler tube with double protection, which includes a boiler tube, an outer wall anti-corrosion coating coated on the outer wall of the boiler tube, and an inner wall anti-corrosion coating coated on the inner wall of the boiler tube, wherein the anti-corrosion coating is a self-fluxing alloy anti-corrosion coating.

[0006] In some embodiments of the present invention, the thickness of the outer wall anti-corrosion coating is 0.5±0.1 mm, and the thickness of the inner wall anti-corrosion coating is 0.2±0.1 mm.

[0007] In some embodiments of the present invention, the base of the boiler tube is normalized.

[0008] In the present invention, the anti-corrosion coating is a nickel-based alloy corrosion-resistant coating.

[0009] In some embodiments of the present invention, the nickel-based alloy corrosion-resistant coating contains nickel, chromium, molybdenum, iron, copper, silicon and boron.

[0010] In some preferred embodiments of the present invention, the nickel-based alloy corrosion-resistant coating contains Ni 60wt%-70wt%, Cr 17wt%-18wt%, Mo 11wt%-13wt%, Cu 1.7wt%-2wt%, B 1.7wt%-2wt%, Si2.5wt%-3wt%, and Fe 3wt%-5wt%.

[0011] In the present invention, the outer wall and inner wall of the boiler tube are independently metallurgically bonded to the self-fluxing alloy anti-corrosion coating. Preferably, the alloy anti-corrosion coating on the outer wall and inner wall of the boiler tube has no pores inside.

[0012] According to the present invention, the anti-corrosion time of the inner wall and the outer wall anti-corrosion coating of the explosion-proof boiler tube with double protection is the same.

[0013] In the present invention, the boiler tubes include water-cooled wall tubes, superheater tubes, reheater tubes or economizer tubes.

[0014] The second aspect of the present invention provides a method for preparing an explosion-proof boiler tube with double protection, which comprises:

[0015] Step A, performing sandblasting on the inner wall surface to remove dust, debris and sand particles on the inner wall surface of the boiler tube to obtain a boiler tube with a roughened inner wall surface;

[0016] Step B, using cold spraying to evenly spray the self-fluxing alloy coating material on the inner wall surface of the boiler tube with a roughened inner wall surface, and after drying, obtaining a boiler tube with a self-fluxing alloy pre-coating on the inner wall;

[0017] Step C, sandblasting the outer wall of the boiler tube with the self-fluxing alloy pre-coating on the inner wall to remove dust, debris and sand on the outer wall surface of the boiler tube to obtain a boiler tube with the self-fluxing alloy pre-coating on the inner wall and a roughened outer wall surface;

[0018] Step D, flame spraying the self-fluxing alloy coating material on the outer surface of the boiler tube with the self-fluxing alloy pre-coating on the inner wall and the roughened outer wall surface, to obtain a boiler tube with the self-fluxing alloy pre-coating on both the inner wall and the outer wall;

[0019] Step E, by feeding and moving high-frequency induction treatment on the boiler tube with self-fluxing alloy pre-coating on the inner wall and outer wall of the boiler tube, the self-fluxing alloy pre-coating on the inner wall and outer wall of the boiler tube is simultaneously remelted, and the substrate of the boiler tube is normalized at the same time, so as to obtain the boiler tube with self-fluxing alloy anti-corrosion coating on the inner wall and outer wall.

[0020] In the present invention, the thickness of the self-fluxing alloy pre-coating layer on the outer wall of the boiler tube is 0.5±0.1 mm, and the thickness of the self-fluxing alloy pre-coating layer on the inner wall of the boiler tube is 0.2±0.1 mm.

[0021] In some embodiments of the present invention, in step E, the high frequency induction remelting temperature is 960-1100°C.

[0022] In some other embodiments of the present invention, in step E, the speed of the feeding movement is 2-3 min / mm.

[0023] In some embodiments of the present invention, in step B, drying is performed by natural drying; preferably, the drying time is 4-6 hours.

[0024] In the present invention, the boiler tubes include water-cooled wall tubes, superheater tubes, reheater tubes or economizer tubes.

[0025] In some preferred embodiments of the present invention, step F is further included after step E, in which the thermal deformation of the boiler tube having the self-fluxing alloy anti-corrosion coating on both the inner and outer walls is corrected during the remelting process to obtain an explosion-proof boiler tube with double protection.

[0026] In some further preferred embodiments of the present invention, step G is further included after step F, for testing the quality of the self-fluxing alloy anti-corrosion coating of the explosion-proof boiler tube with double protection.

[0027] In the present invention, the self-fluxing alloy pre-coating layer on the outer wall of the boiler tube is formed of a nickel-based self-fluxing alloy base material.

[0028] In the present invention, the self-fluxing alloy pre-coating layer on the inner wall of the boiler tube is formed of a nickel-based self-fluxing alloy composite material.

[0029] Preferably, the nickel-based self-fluxing alloy composite material comprises a nickel-based self-fluxing alloy base material, a curing agent and a diluent.

[0030] Further preferably, the nickel-based self-fluxing alloy composite material comprises 40wt%-65wt% of a nickel-based self-fluxing alloy base material, 15wt%-40wt% of a curing agent, and 10wt%-20wt% of a diluent.

[0031] In some embodiments of the present invention, the nickel-based self-fluxing alloy base material includes: Ni 60wt%-70wt%, Cr17wt%-18wt%, Mo 11wt%-13wt%, Cu 1.7wt%-2wt%, B 1.7wt%-2wt%, Si 2.5wt%-3wt%, Fe 3wt%-5wt%.

[0032] The beneficial effects of the present invention are as follows:

[0033] (1) The present invention cleverly utilizes a set of high-frequency induction remelting heat sources used for the outer wall coating of the pipe, fully tapping the potential of the heat source, and can simultaneously achieve the triple effects of remelting the inner and outer wall coatings and normalizing the pipe substrate in just one process. Without spending special preparation time and additional costs, the comprehensive anti-corrosion performance and service life of the pipeline can be greatly improved.

[0034] (2) The principle of "equal life" for the inner and outer walls of the pipe proposed in the present invention is a new concept in the understanding of high-temperature corrosion protection. That is, the life of the outer wall coating and the inner wall coating should be as equal as possible, and there should be no short board. This is because as long as the coating on any side is "lost" first, it will soon begin to thin from that side until the pipe bursts. Figuratively speaking, when the fortress is breached from one side, no matter how strong the other side is, it is useless and a waste. Only when both sides are equally strong can the protection life of the pipeline be maximized.

[0035] (3) After the pipeline undergoes integrated remelting and normalizing treatment, the structure and size of the pipe matrix can be effectively stabilized and internal stress can be eliminated, which is extremely beneficial for improving the material's high-temperature fatigue strength, creep strength and other high-temperature corrosion resistance properties.

[0036] (4) At present, most superheaters and reheaters use high-quality stainless steel materials. After adopting the present invention, ordinary 20G materials can be used instead. While the protective life is increased compared with the coating prepared simply on the outer wall, the cost can also be appropriately reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The present invention will be described below with reference to the accompanying drawings.

[0038] Figure 1 This is a photo of the remaining tubes after a boiler tube (superheater tube) burst.

[0039] Figure 2 This is a photo of corrosion on the outer wall of a boiler tube (superheater tube).

[0040] Figure 3 These are metallographic photographs of the holes and cracks on the inner wall of a boiler tube (superheater tube) after it burst.

[0041] Figure 4 Schematic diagram of the water-cooled wall tube row structure.

[0042] Figure 5 The high frequency induction remelting process of the water-cooled wall tube row is shown.

[0043] Figure 6 This is a schematic diagram of the cross-sectional structure of the water-cooled wall tube row and the copper tube induction coil during the high-frequency induction remelting of the inner and outer walls of the water-cooled wall tube row and the matrix normalizing treatment.

[0044] Figure 7 This is a longitudinal cross-sectional view of the water-cooled wall tube row and the copper tube induction coil during the high-frequency induction remelting of the inner and outer walls of the water-cooled wall tube row and the matrix normalizing treatment.

[0045] Above Figure 4 , Figure 6 and Figure 7 The meanings of the reference numerals in the accompanying drawings are: 1 water-cooled wall (tube row); 12 substrate; 13 fins; 14 outer wall; 141 self-fluxing alloy pre-coating layer (cladding layer) of the outer wall; 142 self-fluxing alloy anti-corrosion coating (remelting layer) of the outer wall; 15 inner wall; 151 self-fluxing alloy pre-coating layer (cladding layer) of the inner wall; 152 self-fluxing alloy anti-corrosion coating (cladding layer) of the inner wall; 2 rectangular copper tube induction coil. DETAILED DESCRIPTION

[0046] In order to make the present invention easy to understand, the present invention will be described in detail below in conjunction with the accompanying drawings. However, before describing the present invention in detail, it should be understood that the present invention is not limited to the specific embodiments described. It should also be understood that the terms used herein are only for describing specific embodiments and are not intended to be limiting.

[0047] Unless otherwise defined, all terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. Although any methods and materials similar or equivalent to those described herein can also be used in the practice or testing of the present invention, preferred methods and materials are now described.

[0048] I. Terminology

[0049] The term "water wall" used in the present invention is also called "water wall" or "water wall tube". It is usually made of steel pipes laid vertically on the inner wall surface of the boiler furnace wall, mainly used to absorb the heat released by the flame and high-temperature flue gas in the furnace.

[0050] The term "inner surface" in the present invention refers to the side of the boiler tube facing the axis, which is also referred to as "inner wall" in the present invention.

[0051] The term "outer surface" in the present invention refers to the side of the boiler tube that faces the axis and the side that faces away from the axis, and is also referred to as the "outer wall" in the present invention.

[0052] The term "double protection" described in the present invention means that both the inner wall and the outer wall of the boiler tube have a self-fluxing alloy anti-corrosion coating, thereby forming double-sided protection on the inner wall and the outer wall of the boiler tube, that is, "double protection".

[0053] The term "pre-coating layer" mentioned in the present invention refers to the self-fluxing alloy coating on the surface of the inner wall or outer wall of the boiler tube before the remelting treatment. For the inner wall, since cold spraying does not have a cladding effect, the pre-coating layer formed by uniformly spraying the self-fluxing alloy coating material on the inner wall surface by cold spraying before the remelting treatment is actually a cladding layer; the pre-coating layer (cladding layer) forms a self-fluxing alloy anti-corrosion coating on the inner wall surface of the boiler tube after remelting treatment (induction heating), which is actually a cladding layer. For the outer wall, since flame spraying has a cladding effect, the pre-coating layer formed by spraying the self-fluxing alloy coating material on the outer wall surface by flame spraying before the remelting treatment is actually a cladding layer; the pre-coating layer (cladding layer) forms a self-fluxing alloy anti-corrosion coating on the outer wall surface of the boiler tube after remelting treatment is actually a remelting layer, the internal porosity of the remelting layer becomes smaller, the bonding force with the outer wall is enhanced, and the anti-corrosion strength is enhanced.

[0054] The term "remelting treatment" in the present invention refers to the cladding of the pre-coating layer on the inner wall or outer wall surface of the boiler tube. For the inner wall, since its pre-coating layer has not been clad but only applied to the inner wall surface, the "remelting treatment" mainly plays a cladding role for the pre-coating layer on the inner wall surface, and the self-fluxing alloy anti-corrosion coating formed on the inner wall surface after the pre-coating layer on the inner wall surface is "remelting treatment" is actually a cladding layer. For the outer wall, since flame spraying has a cladding effect, the pre-coating layer formed on the outer wall surface by flame spraying is actually a cladding layer, and the "remelting treatment" mainly plays a remelting role for the pre-coating layer (cladding layer) on the outer wall surface, so the self-fluxing alloy anti-corrosion coating formed on the outer wall surface after the pre-coating layer (cladding layer) on the outer wall surface is "remelting treatment" is actually a remelting layer.

[0055] In the present invention, the terms "join" and "couple" can be used interchangeably.

[0056] The term "flow passage of steam turbine" mentioned in the present invention refers to the channel for the working steam flow in the steam turbine body, which is mainly composed of three parts: the steam inlet mechanism, the flow passage blades of each stage and the exhaust cylinder; specifically, the channel for the working steam flow in the steam turbine body becomes the flow passage of the steam turbine, which includes the main steam valve, the regulating steam valve, the duct, the steam inlet chamber, the nozzles and the moving blades of each stage and the steam inlet pipe of the steam turbine.

[0057] II. Implementation Plan

[0058] As mentioned above, although a variety of coating protection technologies have been developed in recent years, and the life of the pipeline can be greater than 3 years, the effect is still unsatisfactory, and the phenomenon of thinning the wall thickness until the pipe bursts occurs from time to time. Therefore, preventing the wall thickness of the four boiler tubes from thinning until the pipe bursts and effectively extending the life of the pipeline has become a technical problem that the field has always wanted to solve but has not been able to solve. In view of this, the inventor has conducted a lot of research on boiler pipe protection technology. The inventor found that in order to solve the above problems, the industry has generally focused on the protection of the outer wall of the heating surface for many years. The reason is that in addition to the relatively easy preparation of the outer wall protective coating, the inventor believes that there is a major misunderstanding in the industry: it is generally believed that the main reason for the explosion of boiler tubes is that during the incineration of garbage, high-temperature (>1000℃) corrosion mainly composed of chlorides and sulfides causes local thinning of the outer wall of the pipeline, and finally causes the pipe to burst. However, the inventor believes through long-term research that this is not the case. The burst pipe should essentially be caused by the "inside and outside" of the inner wall and the outer wall. To be more precise, the failure of the inner wall should be the main cause, and the failure of the outer wall should be secondary. This is because the inner wall is subjected to long-term high temperature (450-550℃), high pressure (4.5-6MPa) and water vapor high humidity harsh service environment, which causes fatigue cracks in the pipe wall material, hole cracks caused by high temperature creep, and the generation and shedding of oxide scale and other multiple damages. If it continues to be used under the action of high pressure steam pressure in the pipe, it is very easy to cause local swelling. The inner wall material is subjected to greater tensile stress than the outer wall, causing the micro cracks in the inner wall to continue to expand and network, resulting in patchy shedding and pitting. Therefore, the degree of damage to the inner wall, including macroscopic (oxide scale) and microscopic hidden (micro cracks and micropores and tensile stress) risks, is higher than that of the outer wall. For example, Figure 1 The inner wall of the remaining part after the pipe burst is shown in Figure 1 It can be seen that there are many evenly distributed longitudinal cracks visible to the naked eye on the inner surface of the burst pipe. The wall thickness of the burst part is obviously uneven, and the inner wall is obviously thinned. This shows that the thinned part inside the steel pipe burst because it could not withstand the steam pressure. In fact, from Figure 2 From the corrosion photos of the outer wall of the pipeline, it can be seen that the oxide scale caused by corrosion on the outer wall, including dust accumulation, is actually not easy to fall off from the surface, and the thinning is not obvious. This also proves that most of the thinning is caused by the inner wall.

[0059] The inventors conducted further research on the failure process and principle of the inner wall of the tube, and the results showed that:

[0060] (1) Fatigue and creep of the inner wall of the pipeline, which is the most difficult problem and an important cause of pipe burst.

[0061] First, the inner wall material of the pipeline gradually suffers fatigue damage in the long-term high temperature, high pressure, and water vapor high humidity service environment, and the metallographic structure changes from ferrite + pearlite to ferrite + spherical pearlite, and the fatigue strength decreases significantly, which makes fatigue cracks very likely to occur; secondly, because the inner surface of the pipe wall serves in a long-term high temperature and high pressure environment, the pipe material suffers creep damage, forming creep holes and intergranular cracks, causing the pipeline to creep and expand, the pipe diameter increases, and the pipe wall becomes thinner. Figure 3 This is a metallographic photo of the inner wall of the tube after the tube burst. Figure 3 It can be seen that the inner wall of the pipe, which has been used for only more than one year, is full of holes and cracks. The research results show that under the continuous scouring of high-temperature steam, the inner wall of the pipe gradually develops longitudinally uniformly distributed microcracks, some of which are even deeper than 1mm. These longitudinal cracks gather and increase to form a network, and coupled with the thinning caused by high-temperature corrosion of the outer wall, the "internal and external" eventually cannot withstand the steam pressure in the pipe and burst.

[0062] (2) The generation and shedding of oxide scale on the inner wall of the pipeline. The oxide scale generated by high-temperature steam corrosion on the inner wall during service is very different from the lattice structure of the oxide scale and the matrix in a reducing atmosphere, whether compared with the 20G water-cooled wall boiler tube or the alloy steel and austenitic stainless steel commonly used in superheaters and reheaters. This leads to a large difference in the thermal expansion coefficient between the oxide scale and the matrix, resulting in a loose interface between the oxide scale and the matrix.

[0063] In addition, oxide scale is easily generated on the inner wall when the temperature is high during the preparation of the outer wall coating of the pipeline. For example, the main methods for preparing high-temperature protective coatings on the outer wall of pipelines are currently high-temperature alloy surfacing, nickel-based self-melting alloy remelting, etc. Whether it is surfacing or spray remelting, the same problem is that the heating temperature of the outer wall exceeds thousands of degrees, and due to high temperature conduction, a layer of oxide scale is generated on the inner surface material of the pipe. In other words, oxide scale is generated before the pipeline is put into use, and in the future it will be superimposed on the oxide scale generated during service. Moreover, the two oxide scales have different properties and are incompatible with each other. The thermal cycle process aggravates the sliding between the layers, and gradually falls off and thins. As a result, the risk of pipe bursting is undoubtedly increased.

[0064] The oxide scale produced on the inner wall of the pipe is easy to fall off due to the frequent start and stop of the boiler or the induction of thermal stress, resulting in a reduction in the steam flow area in the pipe, local overheating, deformation and even bursting of the pipe; secondly, the peeled oxide scale debris will be brought into the turbine by steam, damaging the nozzle, blade and other turbine flow parts, and even the peeled oxide scale may cause the steam valve to become stuck, affecting the normal closing of the valve. The above problems not only affect the life of the pipeline, but also have a significant impact on the safe operation of the garbage power plant unit.

[0065] In summary, inner wall damage and oxidation corrosion are the main causes of pipe wall burst, and high-temperature corrosion of the outer wall accelerates the speed of pipe burst. In this regard, the inventors have proposed the concept of high-frequency induction remelting and coordinated preparation of equal-life bilateral protection and explosion-proof pipe coatings for boiler four tubes for the first time at home and abroad after research and design. In short, it is "bilateral protection and central strengthening". The so-called bilateral protection means that both the inner and outer walls must be protected, which can be figuratively described as putting on "double-sided armor" for the pipeline; central strengthening means that while putting on armor, the pipeline matrix must also be normalized and strengthened, which is equivalent to enhancing the body's own immunity, so that it can naturally be "immune to the five poisons" when attacked by foreign pathogens. The so-called "double protection and medium strength" is the process of remelting the outer wall coating only with the help of the original high-frequency induction coil. Now it is completed at one time, which can be said to be "killing three birds with one stone".

[0066] Therefore, the explosion-proof boiler tube with double protection involved in the first aspect of the present invention comprises a boiler tube, an outer wall anti-corrosion coating coated on the outer wall of the boiler tube, and an inner wall anti-corrosion coating coated on the inner wall of the boiler tube, wherein the anti-corrosion coating is an alloy anti-corrosion coating. Preferably, the boiler tube substrate has been normalized. Thus, the explosion-proof boiler tube with double protection in the present invention becomes a "double-protected medium-strong" explosion-proof boiler tube with double protection.

[0067] In some embodiments of the present invention, the thickness of the outer wall anticorrosion coating is 0.5±0.1 mm, and the thickness of the inner wall anticorrosion coating is 0.2±0.1 mm. Thus, the explosion-proof boiler tube of the present invention can obtain relatively ideal double protection, and the anti-corrosion time of the inner wall and outer wall anticorrosion coatings of the explosion-proof boiler tube with double protection is the same.

[0068] In the present invention, the anti-corrosion coating may be a nickel-based alloy corrosion-resistant coating.

[0069] In the present invention, the nickel-based alloy corrosion-resistant coating may contain the components of a conventional nickel-based alloy corrosion-resistant coating. For example, the nickel-based alloy corrosion-resistant coating may contain nickel, chromium, molybdenum, iron, copper, silicon and boron.

[0070] In some preferred embodiments of the present invention, the nickel-based alloy corrosion-resistant coating contains Ni 60wt%-70wt%, Cr 17wt%-18wt%, Mo 11wt%-13wt%, Cu 1.7wt%-2wt%, B 1.7wt%-2wt%, Si2.5wt%-3wt%, and Fe 3wt%-5wt%.

[0071] In the present invention, the outer wall and inner wall of the boiler tube are independently metallurgically bonded to the self-fluxing alloy anti-corrosion coating. Preferably, the alloy anti-corrosion coating on the outer wall and inner wall of the boiler tube has no pores inside. This can ensure protection of the outer wall and inner wall of the boiler tube and better heat transfer performance.

[0072] It should be understood by those skilled in the art that the boiler tubes described in the present invention include water-cooled wall tubes, superheater tubes, reheater tubes or economizer tubes.

[0073] In order to obtain the explosion-proof boiler tube with double protection involved in the first aspect of the present invention, the second aspect of the present invention provides a method for preparing the explosion-proof boiler tube with double protection, which comprises:

[0074] Step A, performing sandblasting on the inner wall surface to remove dust, debris and sand particles on the inner wall surface of the boiler tube to obtain a boiler tube with a roughened inner wall surface;

[0075] Step B, using cold spraying to evenly spray the self-fluxing alloy coating material on the inner wall surface of the boiler tube with a roughened inner wall surface, and after drying, obtaining a boiler tube with a self-fluxing alloy pre-coating on the inner wall;

[0076] Step C, sandblasting the outer wall of the boiler tube with the self-fluxing alloy pre-coating on the inner wall to remove dust, debris and sand on the outer wall surface of the boiler tube to obtain a boiler tube with the self-fluxing alloy pre-coating on the inner wall and a roughened outer wall surface;

[0077] Step D, flame spraying the self-fluxing alloy coating material on the outer surface of the boiler tube with the self-fluxing alloy pre-coating on the inner wall and the roughened outer wall surface, to obtain a boiler tube with the self-fluxing alloy pre-coating on both the inner wall and the outer wall;

[0078] Step E, by feeding and moving high-frequency induction treatment on the boiler tube with self-fluxing alloy pre-coating on the inner wall and outer wall of the boiler tube, the self-fluxing alloy pre-coating on the inner wall and outer wall of the boiler tube is simultaneously remelted, and the substrate of the boiler tube is normalized at the same time, so as to obtain the boiler tube with self-fluxing alloy anti-corrosion coating on the inner wall and outer wall.

[0079] In some preferred embodiments of the present invention, step F is further included after step E, in which the thermal deformation of the boiler tube having the self-fluxing alloy anti-corrosion coating on both the inner and outer walls is corrected during the remelting process to obtain an explosion-proof boiler tube with double protection.

[0080] In some further preferred embodiments of the present invention, step G is further included after step F, for testing the quality of the self-fluxing alloy anti-corrosion coating of the explosion-proof boiler tube with double protection, for example, testing the porosity of the alloy anti-corrosion coating on the outer surface and inner surface of the boiler tube.

[0081] In some preferred embodiments of the present invention, the feeding movement speed is 2-3 min / mm.

[0082] In the present invention, the boiler tubes include water-cooled wall tubes, superheater tubes, reheater tubes or economizer tubes.

[0083] Those skilled in the art should understand that, in step D, the self-fluxing alloy coating material is flame-sprayed on the outer wall surface of the boiler tube, and while a self-fluxing alloy pre-coating layer (cladding layer) is formed on the outer wall surface of the boiler tube, the substrate and the inner wall coating are also preheated, whereby in the subsequent step E, the self-fluxing alloy pre-coating layers on the inner and outer walls of the boiler tube are simultaneously remelted by feeding and moving the boiler tube with the self-fluxing alloy pre-coating layer on both the inner and outer walls by high-frequency induction treatment, and at the same time, the substrate of the boiler tube is normalized, which will produce better effects on the cladding of the pre-coating layer on the inner wall of the boiler and the normalizing based on the pre-coating layer.

[0084] The present invention uses a composite method combining flame spraying of self-fluxing alloy with high-frequency induction remelting to prepare the self-fluxing alloy anti-corrosion coating on the inner and outer walls of boiler tubes. Not only is the coating performance and service life not lower than or even better than cladding, but the preparation cost is much lower than cladding, which should be said to represent the development direction of high-temperature anti-corrosion coatings for water-cooled wall tubes.

[0085] Specifically, the present invention strives to combine the three into one, i.e., preparing the outer wall coating by flame spraying self-fluxing alloy + high-frequency induction remelting, and normalizing the pipe wall for the inner wall coating preparation, while minimizing the increase in process difficulty and preparation cost, thereby greatly improving the high-temperature protection performance of the pipeline and minimizing the risk of thinning and bursting of the four-tube boiler.

[0086] There are no special restrictions on the high-frequency induction remelting (heating) device and the induction coil configured therewith in the present invention, as long as the requirements for the self-fluxing alloy coating cladding or remelting in the present invention can be met. For example, a conventional high-frequency induction remelting device in the art and a copper tube induction coil configured therewith can be used. The shape and size of the coil are determined according to the shape and size of the boiler tube that needs to be remelted by high-frequency induction. The high-frequency induction remelting device can be purchased directly from manufacturers of such devices such as Zhengzhou Gaoshi Electromagnetic Induction Heating Equipment Co., Ltd. or customized according to specific requirements (the shape and size of the boiler tube). The high-frequency induction remelting process for the water-cooled wall tube row in the present invention is as follows: Figure 5 As shown, the schematic diagram of the cross-sectional structure of the water-cooled wall tube row and the copper tube induction coil during the high-frequency induction remelting of the inner wall and outer wall of the water-cooled wall tube row and the matrix normalizing treatment is shown in Figure 6As shown, the longitudinal section of the water-cooled wall tube row and the copper tube induction coil during the high-frequency induction remelting of the inner and outer walls of the water-cooled wall tube row and the matrix normalizing treatment is shown in Figure 7 As shown; it can be seen that the copper tube induction coil is a rectangular copper tube induction coil, which is a spiral rectangular body formed by bending and coiling a rectangular hollow copper tube. The surface of the copper tube is insulated, and its two ends are respectively connected to the two interfaces of the power supply through wires. In addition, in order to prevent the copper tube from being damaged by high temperature, cooling water is also passed through the copper tube to reduce the temperature inside the copper tube.

[0087] However, to achieve the above goals, the following key technologies must be solved:

[0088] (1) Preliminary preparation method of pipeline inner wall coating

[0089] As mentioned above, the reason why the industry generally does not consider coating the inner wall is not only because of misunderstandings, but also because the inner wall coating is difficult to make. This is indeed a difficult problem, because the pipe is a slender pipe with an inner diameter of 50-60mm and a length of 9-10mm. However, in recent years, the equipment technology of the coating industry has developed rapidly. There are mature equipment for sandblasting and painting the inner wall of slender pipes on the market, but it has not been applied to spray high-temperature alloys on the inner holes of boiler pipes in garbage power plants. The inventor added a certain proportion of curing agent and diluent to the nickel-based self-fluxing alloy in the laboratory test and sprayed it. After repeated tests, good results were obtained.

[0090] For example, in the present invention, the self-fluxing alloy coating on the outer wall of the boiler tube is formed by a nickel-based self-fluxing alloy base material, and the self-fluxing alloy coating on the inner wall of the boiler tube is formed by a nickel-based self-fluxing alloy composite material; preferably, the nickel-based self-fluxing alloy composite material includes a nickel-based self-fluxing alloy base material, a curing agent and a diluent; further preferably, the nickel-based self-fluxing alloy composite material includes 50wt%-75wt% of a nickel-based self-fluxing alloy base material, 15wt%-30wt% of a curing agent, and 10wt%-20wt% of a diluent.

[0091] There is no particular limitation on the curing agent in the present invention, as long as it can play a role in bonding and curing the self-fluxing alloy base material; for example, the curing agent includes but is not limited to epoxy resin.

[0092] There is no particular limitation on the diluent in the present invention, as long as it can play a good dispersing role on the self-fluxing alloy base material and the curing agent; for example, the diluent includes one or more of xylene, n-butanol, and propylene glycol methyl ether acetate.

[0093] (2) Pipeline inner wall coating design

[0094] 1) Material Design

[0095] As mentioned above, the self-fluxing alloy coating on the outer wall of the boiler tube is formed by a nickel-based self-fluxing alloy base material, and the nickel-based self-fluxing alloy composite material forming the self-fluxing alloy coating on the inner wall of the boiler tube includes a nickel-based self-fluxing alloy base material, a curing agent and a diluent. The first consideration in the present invention is the "equal life" principle, that is, the life of the outer wall coating and the inner wall coating should be as equal as possible, and no short board should appear. This is because as long as any side fails first, thinning and pipe bursting will soon occur, that is, if the fortress is breached from one side, it is useless to be strong on the other side, but it is a waste. Only when both sides are equally strong can the protection life of the pipeline be maximized. The second thing to consider is whether the remelting temperature of the outer wall coating can meet the requirements of the inner wall remelting. It has been tested that the temperature transmitted to the inner wall during the high-frequency remelting of the outer wall coating reaches 900-950℃. In fact, the oxide scale of a certain thickness (>1mm) generated on the inner wall during the remelting of the outer wall also proves that the temperature is >900℃. Considering that there is a temperature difference of about 100°C between this temperature and the remelting temperature of the outer wall (about 1050°C), by appropriately adjusting the amount of B and Si in the nickel-based self-fluxing alloy base material, the melting point can be slightly reduced to achieve co-remelting of the inner and outer walls.

[0096] In some embodiments of the present invention, the nickel-based self-fluxing alloy base material includes: Ni 60wt%-70wt%, Cr17wt%-18wt%, Mo 11wt%-13wt%, Cu 1.7wt%-2wt%, B 1.7wt%-2wt%, Si 2.5wt%-3wt%, Fe 3wt%-5wt%.

[0097] 2)Thickness design

[0098] The inner wall coating thickness (about 0.2±0.1mm) is designed to be thinner than the outer wall coating (about 0.5mm±0.1). First, the actual inner wall oxidation corrosion rate is considered to be slightly lower than the high-temperature corrosion rate of the outer wall mainly caused by chlorides, that is, the rate of oxide scale formation; second, it is considered that remelting is easy to melt through; third, it is considered to try not to change the steam flow area in the pipe.

[0099] In some embodiments of the present invention, during the preparation process of the inner and outer wall coatings of the boiler tube, the thickness of the self-fluxing alloy pre-coating on the inner wall of the boiler tube is 0.2±0.1 mm, and the thickness of the self-fluxing alloy pre-coating on the outer wall of the boiler tube is 0.5±0.1 mm.

[0100] Since the thickness of the inner wall and outer wall coatings of the present invention is reasonably designed, after the self-fluxing alloy pre-coatings on the inner wall and outer wall of the boiler tube are remelted, the thickness of the self-fluxing alloy anti-corrosion coatings on the inner wall and outer wall of the boiler tube formed remains basically unchanged, that is, the thickness of the self-fluxing alloy anti-corrosion coating on the inner wall of the boiler tube is 0.2±0.1mm, and the thickness of the self-fluxing alloy anti-corrosion coating on the outer wall of the boiler tube is 0.5±0.1mm.

[0101] (3) Normalizing the tube substrate while remelting the pre-coating on the inner and outer walls of the boiler tube

[0102] 1) The waste incineration boiler pipes were not strengthened before leaving the factory, such as normalizing or annealing, resulting in poor high-temperature fatigue performance of the boiler tubes, which is the main reason for the high-temperature fatigue, creep and other failure behaviors mentioned above during service. After normalizing, the organization and size can be effectively stabilized, and the internal stress can be eliminated, which is extremely beneficial to improving the high-temperature fatigue strength and creep resistance of the material.

[0103] 2) The remelting temperature and time of the outer wall pre-coating can meet the normalizing requirements of the pipeline substrate

[0104] The high-frequency induction remelting temperature of the pre-coating on the outer wall of the boiler is 960-1100℃, while the temperature transmitted from the outer coating to the tube substrate is 950-1000℃. All high-frequency induction remelting temperatures are basically the same as the normalizing temperature. The remelting time depends on the pipeline feed speed, that is, the remelting effect. Theoretically, the normalizing and stress relief annealing holding time is about 2-3min / mm, which is close to the actual remelting time. Even if the actual time is slightly longer than the theoretical normalizing time, the segregated structure of the tube matrix will gradually melt and the structure will become more and more uniform. In addition, natural cooling in the air is the same as the cooling method of normalizing. It can be seen that it is completely possible to achieve the simultaneous operation of coating remelting and pipeline substrate normalizing.

[0105] Those skilled in the art should understand that when making the self-fluxing alloy anti-corrosion coating of the tube bank, since it is difficult to make the coating on the inner wall, the present invention chooses to make the anti-corrosion coating on the entire surface of the inner wall of the tube bank, and in order to save costs, the anti-corrosion coating is only made on the surface of the heating surface of the outer wall of the tube bank; for other boiler tubes, such as superheater tubes, reheater tubes or economizer tubes, the anti-corrosion coating is made on all surfaces of the outer wall and the inner wall.

[0106] III. Detection Method

[0107] The porosity of the alloy anti-corrosion coating on the outer and inner surfaces of the boiler tubes in the present invention is monitored according to GB / T 17721-1999 (metal coating porosity test).

[0108] Example

[0109] Example 1: Preparation of explosion-proof water-cooled wall tubes (tube rows) with double protection

[0110] Schematic diagram of water-cooled wall tube row Figure 4 shown.

[0111] (1) Sandblasting the inner wall of the tube row;

[0112] (2) preparing a nickel-based self-fluxing alloy pre-coating layer (about 0.2 mm thick);

[0113] 1) Nickel-based self-fluxing alloy composite material formula:

[0114] The nickel-based self-fluxing alloy composite material is made of the following raw materials in the following weight proportions, wherein the nickel-based self-fluxing alloy base material is 40wt%-65wt%, the curing agent is 15wt%-40wt%, and the diluent is 10%-20%; wherein the curing agent is epoxy resin, and the diluent includes one or more of xylene, n-butanol, and propylene glycol methyl ether acetate.

[0115] 2) Construction technology:

[0116] ① Preparation of nickel-based self-fluxing alloy composite material for the inner wall of the tube row: put the base material and curing agent into a heating furnace or a water bath device for preheating, stir them evenly after preheating, add them into a feed barrel equipped with a heating and heat preservation device, add a diluent, continue stirring and keep warm, and set aside;

[0117] ②Pretreatment of the inner wall surface of the tube row: Use an inner tube sandblasting machine to sandblast the inner wall surface of the tube row; Use a vacuum cleaner to remove all dust, debris and sand particles on the inner wall surface of the tube row;

[0118] ③ Cold spraying of the inner wall surface of the tube row; use an inner tube sprayer to evenly spray the nickel-based self-fluxing alloy composite material onto the inner wall surface of the tube row and dry it naturally for 4-6 hours.

[0119] (3) Sandblast the outer wall of the tube row; use a sandblasting machine to sandblast the outer wall surface (heating surface) of the tube row; use a vacuum cleaner to remove all dust, debris and sand particles on the outer wall surface of the tube row;

[0120] (4) The outer wall surface (heating surface) of the tube row is flame-sprayed with a nickel-based self-fluxing alloy base material to form a self-fluxing alloy pre-coating layer (about 0.5 mm thick), which is equivalent to preheating the base and the inner wall coating at the same time;

[0121] (5) High frequency induction remelting treatment of the inner and outer wall surfaces and pre-coating and normalizing of the substrate (see Figure 5-7 );

[0122] (6) After the pre-coating layer of the tube bank is remelted, it continues to move forward (the moving speed is determined by the time required for the inner wall cladding, the outer wall pre-coating layer remelting and the normalizing of the pipe substrate), and is also naturally cooled to room temperature. The subsequent tube banks are continuously put into the remelting process until all the tube banks are remelted and stopped, obtaining boiler tubes with self-fluxing alloy anti-corrosion coatings on both the inner and outer walls (explosion-proof tube banks with double protection);

[0123] (7) Correction of thermal deformation during the remelting process;

[0124] (8) Test the coating quality.

[0125] The porosity of the coating in this embodiment was monitored according to GB / T 17721-1999 (metal coating porosity test), and the test showed that the internal pores of the self-fluxing alloy anti-corrosion coating on the outer and inner walls of the water-cooled wall tube were very small and could be basically ignored.

[0126] The actual consumption rate in production is directly used to test the corrosion resistance of the double-protected explosion-proof water-cooled wall tubes in this embodiment. The results show that the double-protected explosion-proof water-cooled wall tubes in this embodiment have good double corrosion resistance and truly achieve equal lifespan. The lifespan of the inner and outer wall anti-corrosion coatings can reach more than 6 years.

[0127] The explosion-proof pipe bank with double protection prepared in this embodiment includes the pipe bank, an outer wall anti-corrosion coating coated on the pipe bank, and an inner wall anti-corrosion coating coated on the inner wall of the pipe bank, and the anti-corrosion coating is a self-fluxing alloy anti-corrosion coating.

[0128] The thickness of the outer wall anti-corrosion coating is 0.5±0.1 mm, the thickness of the inner wall anti-corrosion coating is 0.2±0.1 mm, and the boiler tube substrate has been normalized.

[0129] The outer wall and inner wall of the boiler tube are independently metallurgically bonded to the self-fluxing alloy anti-corrosion coating, and there are basically no pores inside the alloy anti-corrosion coating on the outer wall and inner wall of the boiler tube.

[0130] The anti-corrosion coating is a nickel-based alloy corrosion-resistant coating, and the nickel-based alloy corrosion-resistant coating contains nickel, chromium, molybdenum, iron, copper, silicon and boron.

[0131] The nickel-based alloy corrosion-resistant coating contains Ni 60wt%-70wt%, Cr 17wt%-18wt%, Mo11wt%-13wt%, Cu 1.7wt%-2wt%, B 1.7wt%-2wt%, Si 2.5wt%-3wt%, and Fe 3wt%-5wt%.

[0132] The anti-corrosion time of the inner wall and outer wall anti-corrosion coatings of the double-protected explosion-proof boiler tube is the same, and the service life of the inner wall and outer wall anti-corrosion coatings can reach more than 6 years.

[0133] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. An explosion-proof boiler tube with double protection, comprising a boiler tube, an outer wall anti-corrosion coating coated on the outer wall of the boiler tube, and an inner wall anti-corrosion coating coated on the inner wall of the boiler tube, wherein the anti-corrosion coating is a self-fluxing alloy anti-corrosion coating; The thickness of the outer wall anti-corrosion coating is 0.5±0.1mm, and the thickness of the inner wall anti-corrosion coating is 0.2±0.1mm; the substrate of the boiler tube has been normalized; the anti-corrosion coating is a nickel-based alloy corrosion-resistant coating; the nickel-based alloy corrosion-resistant coating contains Ni 60wt%-70wt%, Cr 17wt%-18wt%, Mo 11wt%-13wt%, Cu1.7wt%-2wt%, B 1.7wt%-2wt%, Si 2.5wt%-3wt%, and Fe 3wt%-5wt%.

2. The boiler tube according to claim 1, It is characterized in that The outer wall and inner wall of the boiler tube are independently metallurgically bonded to the self-fluxing alloy anti-corrosion coating; the alloy anti-corrosion coating on the outer wall and inner wall of the boiler tube has no pores inside.

3. The boiler tube according to claim 1, It is characterized in that The anti-corrosion time of the inner wall and the outer wall anti-corrosion coating of the double-protected explosion-proof boiler tube is the same.

4. The boiler tube according to any one of claims 1 to 3, It is characterized in that The boiler tubes include water-cooled wall tubes, superheater tubes, reheater tubes or economizer tubes.

5. A method for preparing a double-protected explosion-proof boiler tube as claimed in any one of claims 1 to 4, wherein include: Step A, performing sandblasting on the inner wall surface to remove dust, debris and sand particles on the inner wall surface of the boiler tube to obtain a boiler tube with a roughened inner wall surface; Step B, using cold spraying to evenly spray the self-fluxing alloy coating material on the inner wall surface of the boiler tube with a roughened inner wall surface, and after drying, obtaining a boiler tube with a self-fluxing alloy pre-coating on the inner wall; Step C, sandblasting the outer wall of the boiler tube with the self-fluxing alloy pre-coating on the inner wall to remove dust, debris and sand on the outer wall surface of the boiler tube to obtain a boiler tube with the self-fluxing alloy pre-coating on the inner wall and a roughened outer wall surface; Step D, flame spraying the self-fluxing alloy coating material on the outer surface of the boiler tube with the self-fluxing alloy pre-coating on the inner wall and the roughened outer wall surface, to obtain a boiler tube with the self-fluxing alloy pre-coating on both the inner wall and the outer wall; Step E, by feeding and moving high frequency induction treatment on the boiler tube with self-fluxing alloy pre-coating on both the inner wall and the outer wall to simultaneously remelt the self-fluxing alloy pre-coating on the inner wall and the outer wall of the boiler tube, and at the same time normalizing the base of the boiler tube to obtain the boiler tube with self-fluxing alloy anti-corrosion coating on both the inner wall and the outer wall; The thickness of the self-fluxing alloy pre-coating layer on the outer wall of the boiler tube is 0.5±0.1 mm, and the thickness of the self-fluxing alloy pre-coating layer on the inner wall of the boiler tube is 0.2±0.1 mm; The self-fluxing alloy pre-coating layer on the outer wall of the boiler tube is formed by a nickel-based self-fluxing alloy base material; the self-fluxing alloy pre-coating layer on the inner wall of the boiler tube is formed by a nickel-based self-fluxing alloy composite material; the nickel-based self-fluxing alloy composite material comprises a nickel-based self-fluxing alloy base material, a curing agent and a diluent; the nickel-based self-fluxing alloy composite material comprises 40wt%-65wt% of the nickel-based self-fluxing alloy base material, 15wt%-40wt% of the curing agent, and 10wt%-20wt% of the diluent; The nickel-based self-fluxing alloy base material comprises: Ni 60wt%-70wt%, Cr 17wt%-18wt%, Mo 11wt%-13wt%, Cu 1.7wt%-2wt%, B 1.7wt%-2wt%, Si 2.5wt%-3wt%, and Fe 3wt%-5wt%.

6. The preparation method according to claim 5, It is characterized in that In step E, the high frequency induction remelting temperature is 960-1100° C.; and / or, the feeding speed is 2-3 min / mm; And / or, in step B, drying is performed by natural drying; the drying time is 4-6 hours.

7. The preparation method according to claim 5 or 6, It is characterized in that After step E, the method further includes step F, in which the thermal deformation of the boiler tube having the self-fluxing alloy anti-corrosion coating on both the inner and outer walls is corrected during the remelting process to obtain an explosion-proof boiler tube with double protection.

8. The preparation method according to claim 7, It is characterized in that After step F, the method further includes step G, which is to detect the quality of the self-fluxing alloy anti-corrosion coating of the explosion-proof boiler tube with double protection.