Silicon-carbon composite material, preparation method thereof, lithium battery negative electrode material and lithium battery

By using alkali metal salt as an etchant in nano-silicon composite materials, the graphene-like carbon film coating and secondary carbonization treatment are solved, and the compaction density of silicon-carbon composite materials is improved. and conductivity, achieving better cycle life and rate performance.

CN111807345BActive Publication Date: 2024-12-03GREE ALTAIRNANO NEW ENERGY INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010556446.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-17
Publication Date
2024-12-03
Estimated Expiration
2040-06-17

AI Technical Summary

Technical Problem

The problems of low compaction density and low surface load of silicon-carbon materials caused by uneven carbon coating in existing nano-silicon composite materials.

Method used

A method of preparing silicon-carbon composite material is adopted, including mixing nanosilicon, carbon source, etchant, binder and solvent, and performing a carbonization treatment to form a graphene-like carbon film-coated silicon material, and then with the carbon series The conductive agent and polymer conductive agent are mixed, compacted and molded, and undergo secondary carbonization treatment. The alkali metal salt is used as an etchant to reduce the agglomeration and volume expansion effects of nano-silicon, and enhance the interface adhesion and mechanical strength.

Benefits of technology

It improves the compaction density and conductivity of silicon-carbon composite materials, enhances cycle life and rate performance, simplifies the preparation process and is easy to produce on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111807345B_ABST
    Figure CN111807345B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon-carbon composite material, a preparation method thereof, a negative electrode material for a lithium battery and a lithium battery. The preparation method comprises: step S1, mixing nano-silicon, a carbon source, an etchant, a binder and a solvent to obtain a mixture; step S2, subjecting the mixture to a primary carbonization treatment to obtain a graphene-like carbon film-coated silicon material; step S3, mixing and compacting the graphene-like carbon film-coated silicon material, a carbon series conductive agent and a polymer conductive agent to obtain a molded blank; and step S4, subjecting the molded blank to a secondary carbonization treatment to obtain a silicon-carbon composite material; wherein the etchant is an alkali metal salt. The present application obtains a silicon-carbon composite material with better cycle life and rate performance through the synergistic effect of the above-mentioned primary carbonization treatment and secondary carbonization treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a silicon-carbon composite material, a preparation method thereof, a lithium battery negative electrode material and a lithium battery. Background Art

[0002] With the rapid development of pure electric vehicles, it is urgent to improve the energy density of power lithium-ion batteries. In terms of negative electrodes, silicon has the advantages of the highest theoretical specific capacity, low charge and discharge platform, and abundant reserves, and is the best candidate for the next generation of high-energy lithium-ion negative electrode materials. However, the huge volume expansion defects of silicon during the alloying process seriously limit its cycle performance. At the same time, the poor intrinsic conductivity and ion conductivity of silicon affect its rate performance. Therefore, researchers have conducted some related modification studies on silicon-based materials.

[0003] At present, the modification research of silicon-based materials mainly focuses on the nano-, porous and composite processing of silicon materials to improve and solve the volume expansion problem of silicon. Liu et al. found that when the particle size of silicon particles is reduced to 150nm, the volume expansion problem can be effectively reduced (ACS Nano 2012, 6, 1522-1531); Yang et al. generated a silicon dioxide layer on the silicon surface by liquid phase method, etched it with hydrofluoric acid, and synthesized a silicon-carbon shell-core structure with reserved space. The reserved space can alleviate the stress damage of the carbon shell caused by the volume expansion of silicon (Nano Energy 18 (2015) 133-142); Lee et al. used nano-silicon and graphite as the core, added a carbon coating layer on the surface to avoid direct contact between silicon and electrolyte, and effectively improved the stability of the material (J.Power Sources 176 (2008) 353-358). However, the reserved space in manufacturing leads to low material compaction density and high specific surface area. In the later electrode production, there are problems such as poor coating effect and broken shell-core structure. In addition, the hydrofluoric acid in this method is a highly toxic substance, which pollutes and damages the environment and human body, and is difficult to industrialize. Nano-sizing and composite processing are the mainstream technologies for industrialization, but the nano-silicon obtained by the existing method has a high surface energy, which makes it easy to agglomerate and difficult to disperse, resulting in uneven carbon coating, which in turn makes the coating structure easy to break, resulting in low material compaction density and low surface loading. Summary of the invention

[0004] The main purpose of the present invention is to provide a silicon-carbon composite material, a preparation method thereof, a lithium battery negative electrode material and a lithium battery, so as to solve the problems of low compaction density and low surface loading of silicon-carbon materials caused by uneven carbon coating in nano-silicon composite materials in the prior art.

[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing a silicon-carbon composite material is provided, the preparation method comprising step S1, mixing nano-silicon, a carbon source, an etchant, a binder and a solvent to obtain a mixture; step S2, subjecting the mixture to a primary carbonization treatment to obtain a graphene-like carbon film-coated silicon material; step S3, mixing and compacting the graphene-like carbon film-coated silicon material, a carbon series conductive agent and a polymer conductive agent to obtain a molded blank; and step S4, subjecting the molded blank to a secondary carbonization treatment to obtain a silicon-carbon composite material; wherein the etchant is an alkali metal salt.

[0006] Furthermore, the mass ratio of the alkali metal salt to the carbon source is 1:5 to 1:20, calculated as alkali metal atoms, and the alkali metal salt is preferably selected from any one or more of potassium chloride, sodium chloride, sodium carbonate, potassium carbonate, sodium nitrate, and potassium nitrate.

[0007] Furthermore, the mass ratio of the above-mentioned nano-silicon to the carbon source is 1:4 to 5:3, and the carbon source is preferably selected from any one or more of polyvinylidene fluoride, glucose, sucrose, fructose, cellulose, soluble starch, citric acid, phenolic resin, sodium hydroxymethyl cellulose, polyvinyl pyrrolidone, ascorbic acid, chitosan, sodium alginate, polyaniline, polythiophene, and polyacrylonitrile.

[0008] Furthermore, in the above step S1, the particle size of nano-silicon is 80 to 120 nm, the solvent is preferably any one or more of ethanol, isopropanol, and acetone, the mass ratio of the binder to the carbon source is preferably 1:5 to 1:10, and the binder is preferably selected from one or two of polyvinyl alcohol and polyvinyl butyral. The mixture is preferably dried before being subjected to a carbonization treatment, and the drying is preferably spray drying.

[0009] Furthermore, in the above step S3, the mass ratio of the graphene-like carbon film-coated silicon material, the carbon series conductive agent and the polymer conductive agent is 2:2~10:1~4, preferably the carbon series conductive agent is selected from one or more of carbon black, graphene, and graphite, and preferably the polymer conductive agent is selected from one or more of polyaniline, polypyrrole, polyvinyl pyrrolidone, and polyvinyl amide.

[0010] Furthermore, the above step S3 also includes crushing the mixed and compacted materials to obtain a molding blank with a diameter in the range of 6≤D50≤20μm.

[0011] Furthermore, the above-mentioned step S2 also includes washing and drying the material after the mixture is carbonized once, preferably using a hydrochloric acid solution with a mass concentration of 2 to 8% to wash the material after the mixture is carbonized once, and the washing time is preferably 0.5 to 4 hours to obtain an acid-washed silicon-carbon material, washing the acid-washed silicon-carbon material with water to obtain a water-washed silicon-carbon material, preferably drying the water-washed silicon-carbon material at a temperature of 80 to 120°C to obtain a graphene-like carbon film-coated silicon material, preferably spray drying time is 10 to 24 hours, and preferably drying is spray drying.

[0012] Furthermore, the primary carbonization treatment and the secondary carbonization treatment are each independently carried out in a hydrogen or inert gas atmosphere, at a reaction temperature of 500 to 1000° C. and for a reaction time of 0.5 to 4 h.

[0013] According to another aspect of the present invention, a silicon-carbon composite material is provided. The silicon-carbon composite material is prepared by the aforementioned preparation method.

[0014] According to another aspect of the present invention, there is provided a negative electrode material for a lithium battery, the negative electrode material for a lithium battery comprising any one of the aforementioned silicon-carbon composite materials.

[0015] According to another aspect of the present invention, there is provided a lithium battery, comprising a negative electrode and a positive electrode, wherein the negative electrode is the above-mentioned negative electrode material for the lithium battery.

[0016] By applying the technical solution of the present invention, the nano-silicon in the above-mentioned mixture of the present application is diluted by the carbon source, etchant, binder and solvent, and the temporary agglomeration between the nano-silicon is reduced to a certain extent. Then, a layer of carbon film with a graphite-like structure is coated around the nano-silicon by using the etchant, which not only fundamentally solves the problem of nano-silicon agglomeration, but also alleviates the volume expansion effect of nano-silicon and promotes electron transmission. At the same time, the carbon film is used as a bridge to avoid direct contact between the nano-silicon and the carbon series conductive agent. Because the defect sites on the carbon film interact with the defect sites on the surface of the carbon series conductive agent, the interface adhesion between the carbon series conductive agent and the nano-silicon in the secondary carbonization treatment is indirectly enhanced, so that the carbon series conductive agent is easy to be coated on the nano-silicon, and the silicon is more evenly distributed on the graphite surface. After the first carbonization treatment, the graphene-like carbon film-coated silicon material is compacted, which reduces the pore structure produced by the first carbonization treatment, improves the compaction density of the silicon-carbon composite material, and can withstand the stress caused by the volume expansion of silicon, enhances the stability of the silicon-carbon composite material while reducing the specific surface area of ​​the silicon-carbon composite material, so that if it is applied to the battery, it is conducive to the formation of a solid electrolyte membrane, increases the surface load of the battery core, and then improves the Coulomb efficiency and cycle life of the battery core. The secondary carbonization treatment further reduces the possibility of direct contact between silicon and the silicon-carbon electrolyte, enhances the mechanical strength of the silicon-carbon composite material, and improves the compaction density of the silicon-carbon composite material. At the same time, the polymer conductive agent is selected to improve the conductivity of the silicon-carbon composite material and the rate performance of the battery. Therefore, the present application obtains a silicon-carbon composite material with better cycle life and rate performance through the synergistic effect of the above-mentioned first carbonization treatment and the secondary carbonization treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0018] Figure 1 A TEM image of a graphene-like carbon film-coated silicon material provided according to Example 1 of the present invention is shown;

[0019] Figure 2 A SEM image of a silicon-carbon composite material provided according to Example 1 of the present invention is shown;

[0020] Figure 3 Shows Figure 2 SEM image of a cross section of the silicon-carbon composite material shown;

[0021] Figure 4 A schematic diagram showing the cycle performance of a soft-pack battery cell made of silicon-carbon composite materials obtained in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention and NCM811 at a current density of 1C is shown; and

[0022] Figure 5 A schematic diagram showing the cycle performance of soft-pack batteries made of silicon-carbon composite materials obtained according to Example 1, Comparative Example 1 and Comparative Example 2 of the present invention and NCM811 at current densities of 1C / 2C / 3C respectively. DETAILED DESCRIPTION

[0023] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0024] As analyzed in the background technology, the prior art has the problem of low compaction density and low surface loading of silicon-carbon materials due to uneven carbon coating in nano-silicon composite materials. To solve this problem, the present invention provides a silicon-carbon composite material, a preparation method thereof, a lithium battery negative electrode material and a lithium battery.

[0025] In a typical embodiment of the present application, a method for preparing a silicon-carbon composite material is provided, and the preparation method comprises: step S1, mixing nano-silicon, a carbon source, an etchant, a binder and a solvent to obtain a mixture; step S2, subjecting the mixture to a primary carbonization treatment to obtain a graphene-like carbon film-coated silicon material; step S3, mixing and compacting the graphene-like carbon film-coated silicon material, a carbon series conductive agent and a polymer conductive agent to obtain a molded blank; and step S4, subjecting the molded blank to a secondary carbonization treatment to obtain a silicon-carbon composite material; wherein the etchant is an alkali metal salt.

[0026] The nano-silicon in the above-mentioned mixture of the present application is diluted by the carbon source, etchant, binder and solvent, which reduces the temporary agglomeration of the nano-silicon to a certain extent. Then, a layer of carbon film with a graphite-like structure is coated around the nano-silicon by using the etchant, which not only fundamentally solves the problem of nano-silicon agglomeration, but also alleviates the volume expansion effect of nano-silicon and promotes electron transmission. At the same time, the carbon film is used as a bridge to avoid direct contact between the nano-silicon and the carbon series conductive agent. In addition, due to the interaction between the defect sites on the carbon film and the defect sites on the surface of the carbon series conductive agent, the interface adhesion between the carbon series conductive agent and the nano-silicon in the secondary carbonization treatment is indirectly enhanced, so that the carbon series conductive agent is easy to be coated on the nano-silicon, and the silicon is more evenly distributed on the graphite surface. After the first carbonization treatment, the graphene-like carbon film-coated silicon material is compacted, which reduces the pore structure produced by the first carbonization treatment, improves the compaction density of the silicon-carbon composite material, and can withstand the stress caused by the volume expansion of silicon, enhances the stability of the silicon-carbon composite material while reducing the specific surface area of ​​the silicon-carbon composite material, so that if it is applied to the battery, it is conducive to the formation of the solid electrolyte membrane, increases the surface load of the battery core, and then improves the Coulomb efficiency and cycle life of the battery core. The secondary carbonization treatment further reduces the possibility of direct contact between silicon and the silicon-carbon electrolyte, enhances the mechanical strength of the silicon-carbon composite material, and improves the compaction density of the silicon-carbon composite material. At the same time, the polymer conductive agent is selected to improve the conductivity of the silicon-carbon composite material and the rate performance of the battery. Therefore, the present application obtains a silicon-carbon composite material with better cycle life and rate performance through the synergistic effect of the above-mentioned first carbonization treatment and the secondary carbonization treatment, and the above-mentioned silicon-carbon composite material preparation process is simple and easy to scale production.

[0027] In order to enhance the etching effect of alkali metal salts on graphene-like carbon films and obtain a graphene-like carbon film coating layer with richer defect sites, the mass ratio of alkali metal salts to carbon source is preferably 1:5 to 1:20, calculated as alkali metal atoms, and the alkali metal salt is preferably selected from any one or more of potassium chloride, sodium chloride, sodium carbonate, potassium carbonate, sodium nitrate, and potassium nitrate.

[0028] In order to improve the mitigating effect of the obtained graphene-like carbon film coating on the volume expansion of silicon particles, the mass ratio of the above-mentioned nano-silicon to the carbon source is preferably 1:4 to 5:3, and the carbon source is preferably selected from any one or more of polyvinylidene fluoride, glucose, sucrose, fructose, cellulose, soluble starch, citric acid, phenolic resin, sodium hydroxymethyl cellulose, polyvinyl pyrrolidone, ascorbic acid, chitosan, sodium alginate, polyaniline, polythiophene, and polyacrylonitrile.

[0029] In one embodiment of the present application, in the above step S1, the particle size of nano-silicon is 80-120 nm, the solvent is preferably any one or more of ethanol, isopropanol, and acetone, the mass ratio of the binder to the carbon source is preferably 1:5-1:10, and the binder is preferably selected from one or two of polyvinyl alcohol and polyvinyl butyral. The mixture is preferably dried before being subjected to a carbonization treatment, and the drying is preferably spray drying.

[0030] The nano silicon of the above particle size is conducive to controlling the particle size of the silicon-carbon composite material, and the mass ratio of the binder to the carbon source is conducive to firmly bonding the two, thereby obtaining a relatively complete graphene-like carbon film coating layer. The nano silicon can be purchased directly or crushed by conventional crushing methods in the prior art to obtain large-particle silicon powder. For example, in the present application, large-particle silicon powder is added to an organic solvent and ground by a rod-pin type dispersion grinder to obtain nano silicon of the above particle size.

[0031] In one embodiment of the present application, in the above-mentioned step S3, the mass ratio of the graphene-like carbon film-coated silicon material, the carbon series conductive agent and the polymer conductive agent is 2:2~10:1~4, and the carbon series conductive agent is preferably selected from one or more of carbon black, graphene, and graphite, and the polymer conductive agent is preferably selected from one or more of polyaniline, polypyrrole, polyvinyl pyrrolidone, and polyvinyl amide.

[0032] In order to further improve the dispersion uniformity of nano-silicon in the silicon-carbon composite material, preferably, the above step S3 also includes crushing the mixed and compacted materials to obtain a molding blank with a diameter in the range of 6≤D50≤20μm.

[0033] The mass ratio of the graphene-like carbon film coated silicon material, the carbon series conductive agent and the polymer conductive agent is that on the one hand, a carbon coating layer is formed on the graphene-like carbon film coated silicon material, which is beneficial to improve the mechanical strength of the carbon silicon composite material. At the same time, the selection of the above carbon source is helpful to improve the conductivity of the carbon silicon composite material. The diameter of the carbon series conductive agent and the polymer conductive agent is beneficial to control the diameter of the molding blank, so as to better adapt to the application of the battery.

[0034] In one embodiment of the present application, the above-mentioned step S2 also includes washing and drying the material after the mixture is carbonized once, preferably using a hydrochloric acid solution with a mass concentration of 2 to 8% to wash the material after the mixture is carbonized once, and the washing time is preferably 0.5 to 4 hours to obtain an acid-washed silicon-carbon material, and the acid-washed silicon-carbon material is washed with water to obtain a water-washed silicon-carbon material, preferably at a temperature of 80 to 120°C, The washed silicon-carbon material is dried to obtain a graphene-like carbon film-coated silicon material, preferably the drying time is 10 to 24 hours, and the drying is preferably spray drying.

[0035] The above-mentioned washing and drying of the material after the mixture is carbonized once is helpful to remove excess alkali metal salt of the etchant, thereby reducing the influence of the etchant on subsequent reactions. The above-mentioned specific washing and drying treatment conditions are conducive to improving its efficiency and removing the etchant as much as possible. The above-mentioned spray drying is conducive to forming a uniform graphene-like carbon film-coated silicon material particles and quickly completing the drying process.

[0036] In one embodiment of the present application, the primary carbonization treatment and the secondary carbonization treatment are independently carried out in a hydrogen or inert gas atmosphere, at a reaction temperature of 500 to 1000° C. and a reaction time of 0.5 to 4 hours.

[0037] The carbonization treatment in a hydrogen or inert gas atmosphere can reduce the generation of by-products at high temperatures on the one hand, and inhibit the re-oxidation of the generated carbon on the other hand, thereby improving the stability of the carbonization product. The temperature and time of the carbonization treatment are conducive to improving the efficiency of the carbonization treatment.

[0038] In another typical embodiment of the present application, a silicon-carbon composite material is provided. The silicon-carbon composite material is prepared by the above-mentioned preparation method.

[0039] The nano-silicon in the above-mentioned mixture of the present application is diluted by the carbon source, etchant, binder and solvent, which reduces the temporary agglomeration of the nano-silicon to a certain extent. Then, a layer of carbon film with a graphite-like structure is coated around the nano-silicon by using the etchant, which not only fundamentally solves the problem of nano-silicon agglomeration, but also alleviates the volume expansion effect of nano-silicon and promotes electron transmission. At the same time, the carbon film is used as a bridge to avoid direct contact between the nano-silicon and the carbon series conductive agent. In addition, due to the interaction between the defect sites on the carbon film and the defect sites on the surface of the carbon series conductive agent, the interface adhesion between the carbon series conductive agent and the nano-silicon in the secondary carbonization treatment is indirectly enhanced, so that the carbon series conductive agent is easy to be coated on the nano-silicon, and the silicon is more evenly distributed on the graphite surface. After the first carbonization treatment, the graphene-like carbon film-coated silicon material is compacted, which reduces the pore structure produced by the first carbonization treatment, improves the compaction density of the silicon-carbon composite material, and can withstand the stress caused by the volume expansion of silicon, enhances the stability of the silicon-carbon composite material while reducing the specific surface area of ​​the silicon-carbon composite material, so that if it is applied to the battery, it is conducive to the formation of a solid electrolyte membrane, increases the surface load of the battery core, and then improves the Coulomb efficiency and cycle life of the battery core. The secondary carbonization treatment further reduces the possibility of direct contact between silicon and the silicon-carbon electrolyte, enhances the mechanical strength of the silicon-carbon composite material, and improves the compaction density of the silicon-carbon composite material. At the same time, the polymer conductive agent is selected to improve the conductivity of the silicon-carbon composite material and the rate performance of the battery. Therefore, the present application obtains a silicon-carbon composite material with better cycle life and rate performance through the synergistic effect of the above-mentioned first carbonization treatment and the secondary carbonization treatment.

[0040] In another typical embodiment of the present application, a negative electrode material for a lithium battery is provided. The negative electrode material for a lithium battery includes any one of the aforementioned silicon-carbon composite materials.

[0041] The silicon-carbon composite material having the properties of high compaction density, low specific surface area and high conductivity is used as a negative electrode material for a lithium battery, so that the obtained negative electrode material for a lithium battery has a higher battery capacity, excellent cycle performance and rate performance.

[0042] In another typical embodiment of the present application, a lithium battery is provided, comprising a negative electrode and a positive electrode, wherein the negative electrode is the aforementioned negative electrode material of the lithium battery.

[0043] The above-obtained lithium battery negative electrode material with high battery capacity, excellent cycle performance and rate performance is used as the negative electrode material of the lithium ion battery, so that the lithium ion battery has a higher energy density and improves the specific capacity, compaction density, cycle performance and rate performance of the lithium ion battery.

[0044] The beneficial effects of the present application will be described below in conjunction with specific embodiments and comparative examples.

[0045] Example 1

[0046] 300g silicon powder is added to 4L isopropanol, and ground by a pin-type dispersion mill until the particle D50 is 80-100nm. The slurry is transferred to a nano-disperser, and 45g PVB, 60g KCl, and 300g PVDF are added in sequence, dispersed for 30min, and spray-dried to obtain a mixture; the mixture is subjected to a first carbonization treatment at 800°C for 2h under a nitrogen protective atmosphere to obtain a graphene-like carbon film-coated silicon material. The graphene-like carbon film-coated silicon material is dispersed in an 8% hydrochloric acid solution and stirred for 2h to remove potassium salt from the graphene-like carbon film-coated silicon material to obtain an acid-washed silicon-carbon material, and the acid-washed silicon-carbon material is washed with water and dried in an oven at 80°C for 12h to obtain a graphene-like carbon film-coated silicon material.

[0047] 100g of graphene-like carbon film coated silicon material, 150g of graphite (D50 is 5μm) and 50g of polyaniline (D50 is 6μm) are mixed evenly in a fusion machine and sent to a three-screw extruder to extrude into sheets, which are then pressed into molding blanks by a roller mill. The molding blanks are actually air flow crushed and graded to obtain molding blanks with a D50 of 10 to 16μm. A second carbonization treatment is carried out at 800°C for 2h under a nitrogen protective atmosphere to obtain a silicon-carbon composite material. The surface morphology of the graphene-like carbon film coated silicon material and the silicon-carbon composite material is detected, and the TEM image of the graphene-like carbon film coated silicon material is obtained as follows: Figure 1 , the SEM image of silicon-carbon composite material is as follows Figure 2 As shown, the SEM image of the cross section of the silicon-carbon composite material is as follows Figure 3 shown.

[0048] Example 2

[0049] The difference between Example 2 and Example 1 is that:

[0050] The amount of KCl is 115 g, and a silicon-carbon composite material is finally obtained.

[0051] Example 3

[0052] The difference between Example 3 and Example 1 is that:

[0053] The amount of KCl was 29 g, and a silicon-carbon composite material was finally obtained.

[0054] Example 4

[0055] The difference between Example 4 and Example 1 is that,

[0056] The amount of silicon powder is 75 g, and a silicon-carbon composite material is finally obtained.

[0057] Example 5

[0058] The difference between Example 5 and Example 1 is that

[0059] The amount of silicon powder is 500 g, and a silicon-carbon composite material is finally obtained.

[0060] Example 6

[0061] The difference between Example 6 and Example 1 is that

[0062] The amount of silicon powder is 60 g, and a silicon-carbon composite material is finally obtained.

[0063] Example 7

[0064] The difference between Example 7 and Example 1 is that

[0065] The amount of PVB is 30 g, and a silicon-carbon composite material is finally obtained.

[0066] Example 8

[0067] The difference between Example 8 and Example 1 is that,

[0068] The amount of PVB is 60 g, and a silicon-carbon composite material is finally obtained.

[0069] Example 9

[0070] The difference between Example 9 and Example 1 is that

[0071] The amount of PVB is 20 g, and a silicon-carbon composite material is finally obtained.

[0072] Example 10

[0073] The difference between Example 10 and Example 1 is that

[0074] 100g of graphene-like carbon film-coated silicon material, 500g of graphite and 200g of polyaniline were mixed evenly in a fusion machine and then sent to a three-screw extruder for extrusion into sheets, and finally a silicon-carbon composite material was obtained.

[0075] Embodiment 11

[0076] The difference between Example 11 and Example 1 is that

[0077] 100 g of graphene-like carbon film-coated silicon material, 300 g of graphite and 150 g of polyaniline were mixed evenly in a fusion machine and then sent to a three-screw extruder for extrusion into sheets, and finally a silicon-carbon composite material was obtained.

[0078] Example 12

[0079] The difference between Example 12 and Example 1 is that

[0080] 100 g of graphene-like carbon film-coated silicon material, 50 g of graphite and 250 g of polyaniline were mixed evenly in a fusion machine and then sent to a three-screw extruder for extrusion into sheets, and finally a silicon-carbon composite material was obtained.

[0081] Example 13

[0082] The difference between Example 13 and Example 1 is that

[0083] The diameter of the molding blank is 6 to 10 μm, and a silicon-carbon composite material is finally obtained.

[0084] Embodiment 14

[0085] The difference between Example 14 and Example 1 is that

[0086] The diameter of the molding blank is 16 to 20 μm, and a silicon-carbon composite material is finally obtained.

[0087] Embodiment 15

[0088] The difference between Example 15 and Example 1 is that

[0089] The diameter of the molding blank is 3 to 5 μm, and a silicon-carbon composite material is finally obtained.

[0090] Example 16

[0091] The difference between Example 16 and Example 1 is that

[0092] The graphene-like carbon film coated silicon material is dispersed in a 2% hydrochloric acid solution and stirred for 4 hours to remove potassium salt in the graphene-like carbon film coated silicon material to obtain an acid-washed silicon-carbon material. The acid-washed silicon-carbon material is washed with water and then dried in an oven at 120°C for 10 hours to finally obtain a graphene-like carbon film coated silicon material.

[0093] Embodiment 17

[0094] The difference between Example 17 and Example 1 is that

[0095] The graphene-like carbon film coated silicon material is dispersed in a 5% hydrochloric acid solution and stirred for 0.5 h to remove potassium salt in the graphene-like carbon film coated silicon material to obtain an acid-washed silicon-carbon material. The acid-washed silicon-carbon material is washed with water and then dried in an oven at 100° C. for 24 h to finally obtain a graphene-like carbon film coated silicon material.

[0096] Embodiment 18

[0097] The difference between Example 18 and Example 1 is that

[0098] The temperature of the first carbonization treatment and the second carbonization treatment are both 500°C, and the time of the first carbonization treatment and the second carbonization treatment are both 4 hours, and finally a graphene-like carbon film-coated silicon material is obtained.

[0099] Embodiment 19

[0100] The difference between Example 19 and Example 1 is that

[0101] The temperature of the first carbonization treatment and the second carbonization treatment are both 1000°C, and the time of the first carbonization treatment and the second carbonization treatment are both 0.5h, and finally a graphene-like carbon film-coated silicon material is obtained.

[0102] Embodiment 20

[0103] The difference between Example 20 and Example 1 is that

[0104] The temperature of the first carbonization treatment and the second carbonization treatment are both 1100°C, and the time of the first carbonization treatment and the second carbonization treatment are both 0.5h, and finally a graphene-like carbon film-coated silicon material is obtained.

[0105] Embodiment 21

[0106] The difference between Example 21 and Example 1 is that

[0107] 300 g of silicon powder was added to 4 L of isopropanol and ground by a pin-type dispersing grinder until the particle D50 was 100-120 nm. The carbon source was soluble starch, the carbon series conductive agent was graphene, and the polymer conductive agent was polyvinyl pyrrolidone, and finally a graphene-like carbon film-coated silicon material was obtained.

[0108] Embodiment 22

[0109] The difference between Example 22 and Example 1 is that

[0110] 300 g of silicon powder was added into 4 L of acetone and ground by a pin-type dispersion grinder until the particle D50 was 100-120 nm, and finally a graphene-like carbon film-coated silicon material was obtained.

[0111] Embodiment 23

[0112] The difference between Example 23 and Example 1 is that the carbon source is soluble starch, and a graphene-like carbon film-coated silicon material is finally obtained.

[0113] Embodiment 24

[0114] The difference between Example 24 and Example 1 is that the polymer conductive agent is polyvinyl pyrrolidone, and a graphene-like carbon film-coated silicon material is finally obtained.

[0115] Embodiment 25

[0116] The difference between Example 25 and Example 1 is that the carbon series conductive agent is graphene, and a graphene-like carbon film-coated silicon material is finally obtained.

[0117] Embodiment 26

[0118] The difference between Example 26 and Example 1 is that the alkali metal salt is sodium carbonate, and a graphene-like carbon film-coated silicon material is finally obtained.

[0119] Comparative Example 1

[0120] The difference between Comparative Example 1 and Example 1 is that

[0121] 100g of a mixture consisting of silicon powder, potassium chloride, and PVDF, 150g of graphite, and 50g of polyaniline were mixed evenly in a fusion machine and sent to a three-screw extruder for extrusion into sheets, which were then pressed into a molding blank by a roller mill. The molding blank was air flow crushed and graded to obtain a molding blank with D50 = 16-20μm. The carbonization treatment was carried out at 800℃ for 2h under a nitrogen protective atmosphere to obtain a silicon-carbon composite material.

[0122] Comparative Example 2

[0123] The difference between Comparative Example 2 and Example 1 is that

[0124] The mixture was carbonized at 800° C. for 2 h under a nitrogen protective atmosphere to obtain a silicon-carbon composite material.

[0125] The silicon-carbon composite materials prepared in Examples 1 to 26, Comparative Example 1, and Comparative Example 2 were respectively combined with NCM811 to prepare soft-pack batteries, and their initial discharge capacities at a current density of 0.5C were tested at room temperature, and their discharge capacity retention rates at a current density of 1C after 200 cycles were tested at room temperature, and the results are listed in Table 1. The cycle performance of the soft-pack batteries prepared by combining the silicon-carbon composite materials obtained in Example 1, Comparative Example 1, and Comparative Example 2 with NCM811 at a current density of 1C is shown in Table 1. Figure 4 As shown, the rate performance diagram of the soft-pack battery made of the silicon-carbon composite material obtained in Example 1, Comparative Example 1 and Comparative Example 2 and NCM811 at 1C / 2C / 3C current density is as follows Figure 5 As shown, from Figure 4 , Figure 5 It can be seen that the silicon-carbon composite materials obtained in Example 1, Comparative Example 1 and Comparative Example 2 are combined with NCM811 to make soft-pack batteries. When cycled for 200 cycles at a current density of 1C, the battery discharge capacity retention rates are 94.9%, 86.1% and 70.8%, respectively. At a current density of 3C, the battery discharge capacity retention rates are 93.7%, 71.9% and 61.2%, respectively. It can be seen that the silicon-carbon composite materials of the present application exhibit excellent cycle performance and rate performance.

[0126] Table 1

[0127]

[0128]

[0129] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0130] The nano-silicon in the above-mentioned mixture of the present application is diluted by the carbon source, etchant, binder and solvent, which reduces the temporary agglomeration of the nano-silicon to a certain extent. Then, a layer of carbon film with a graphite-like structure is coated around the nano-silicon by using the etchant, which not only fundamentally solves the problem of nano-silicon agglomeration, but also alleviates the volume expansion effect of nano-silicon and promotes electron transmission. At the same time, the carbon film is used as a bridge to avoid direct contact between the nano-silicon and the carbon series conductive agent. In addition, due to the interaction between the defect sites on the carbon film and the defect sites on the surface of the carbon series conductive agent, the interface adhesion between the carbon series conductive agent and the nano-silicon in the secondary carbonization treatment is indirectly enhanced, so that the carbon series conductive agent is easy to be coated on the nano-silicon, and the silicon is more evenly distributed on the graphite surface. After the first carbonization treatment, the graphene-like carbon film-coated silicon material is compacted, which reduces the pore structure produced by the first carbonization treatment, improves the compaction density of the silicon-carbon composite material, and can withstand the stress caused by the volume expansion of silicon, enhances the stability of the silicon-carbon composite material while reducing the specific surface area of ​​the silicon-carbon composite material, so that if it is applied to the battery, it is conducive to the formation of the solid electrolyte membrane, increases the surface load of the battery core, and then improves the Coulomb efficiency and cycle life of the battery core. The secondary carbonization treatment further reduces the possibility of direct contact between silicon and the silicon-carbon electrolyte, enhances the mechanical strength of the silicon-carbon composite material, and improves the compaction density of the silicon-carbon composite material. At the same time, the polymer conductive agent is selected to improve the conductivity of the silicon-carbon composite material and the rate performance of the battery. Therefore, the present application obtains a silicon-carbon composite material with better cycle life and rate performance through the synergistic effect of the above-mentioned first carbonization treatment and the secondary carbonization treatment, and the above-mentioned silicon-carbon composite material preparation process is simple and easy to scale production.

[0131] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a silicon-carbon composite material, characterized in that: The preparation method comprises: Step S1, mixing nano-silicon, a carbon source, an etchant, a binder and a solvent to obtain a mixture; Step S2, subjecting the mixture to a carbonization treatment to obtain a graphene-like carbon film-coated silicon material; Step S3, mixing and compacting the graphene-like carbon film-coated silicon material, the carbon series conductive agent and the polymer conductive agent to obtain a molding blank; and Step S4, performing secondary carbonization treatment on the molding blank to obtain a silicon-carbon composite material; Wherein, the etchant is an alkali metal salt; The mass ratio of the graphene-like carbon film-coated silicon material, the carbon series conductive agent and the polymer conductive agent is 2:2-10:1-4; The polymer conductive agent is selected from one or more of polyaniline, polypyrrole, polyvinyl pyrrolidone and polyvinyl amide; The mass ratio of the nano-silicon to the carbon source is 1:4 to 5:3; The step S3 also includes crushing the mixed and compacted materials to obtain a molding blank with a diameter in the range of 6≤D50≤20μm.

2. The preparation method according to claim 1, characterized in that: Calculated in terms of alkali metal atoms, the mass ratio of the alkali metal salt to the carbon source is 1:5 to 1:

20.

3. The preparation method according to claim 1 or 2, characterized in that: The alkali metal salt is selected from any one or more of potassium chloride, sodium chloride, sodium carbonate, potassium carbonate, sodium nitrate and potassium nitrate.

4. The preparation method according to claim 1, characterized in that: The carbon source is selected from any one or more of polyvinylidene fluoride, glucose, sucrose, fructose, cellulose, soluble starch, citric acid, phenolic resin, sodium hydroxymethyl cellulose, polyvinyl pyrrolidone, ascorbic acid, chitosan, sodium alginate, polyaniline, polythiophene, and polyacrylonitrile.

5. The preparation method according to claim 1, characterized in that: In the step S1, the particle size of the nano-silicon is 80-120 nm.

6. The preparation method according to claim 1, characterized in that: The solvent is any one or more of ethanol, isopropanol and acetone.

7. The preparation method according to claim 1, characterized in that: The mass ratio of the binder to the carbon source is 1:5 to 1:

10.

8. The preparation method according to claim 1, characterized in that: The binder is selected from one or both of polyvinyl alcohol and polyvinyl butyral.

9. The preparation method according to claim 1, characterized in that: The mixture is dried before being subjected to the primary carbonization treatment.

10. The preparation method according to claim 9, characterized in that: The drying is spray drying.

11. The preparation method according to claim 1, characterized in that: In step S3, the carbon series conductive agent is selected from one or more of carbon black, graphene, and graphite.

12. The preparation method according to claim 1, characterized in that: The step S2 further comprises washing the material after the carbonization treatment of the mixture with a hydrochloric acid solution having a mass concentration of 2 to 8%, the washing time being 0.5 to 4 hours, to obtain a silicon-carbon material after acid washing; The acid-washed silicon-carbon material is washed with water to obtain a water-washed silicon-carbon material.

13. The preparation method according to claim 12, characterized in that: The washed silicon-carbon material is dried at a temperature of 80 to 120° C. to obtain a graphene-like carbon film-coated silicon material.

14. The preparation method according to claim 13, characterized in that: The drying time is 10 to 24 hours.

15. The preparation method according to claim 13, characterized in that: The drying is spray drying.

16. The preparation method according to claim 1, characterized in that: The primary carbonization treatment and the secondary carbonization treatment are independently performed in a hydrogen or inert gas atmosphere, at a reaction temperature of 500 to 1000° C., and for a reaction time of 0.5 to 4 hours.

17. A silicon-carbon composite material, characterized in that: The silicon-carbon composite material is prepared by the preparation method according to any one of claims 1 to 16.

18. A negative electrode material for a lithium battery, characterized in that: The lithium battery negative electrode material comprises any one of the silicon-carbon composite materials described in claim 17.

19. A lithium battery comprising a negative electrode and a positive electrode, characterized in that: The negative electrode is the lithium battery negative electrode material according to claim 18.