Separator for secondary battery and electrochemical device using the same

The high resistance and heat of the lithium secondary battery separator are solved by applying a crosslinkable composition of a self-crosslinked water-based latex adhesive with high glass transition temperature on the lithium secondary battery separator. The problem of poor stability achieves low resistance and excellent surface hardness, ensuring the safety and efficient performance of the battery.

CN111864164BActive Publication Date: 2024-11-15SK INNOVATION CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010333770.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-25
Filing Date
2020-04-24
Publication Date
2024-11-15
Estimated Expiration
2040-04-24

AI Technical Summary

Technical Problem

The existing lithium secondary battery separators have high resistance, poor thermal stability, insufficient mechanical strength and hole blockage under the trend of high capacity and high output, resulting in poor battery safety and performance.

Method used

A crosslinkable composition with a self-crosslinked water-based latex adhesive and an epoxy crosslinker coated on a porous substrate is formed to form a heat-resistant coating with low resistance and reduce the kudzu by heating curing. Erlai permeability and improve adhesive strength to prevent electrode short circuit and ignition.

Benefits of technology

The composite separator is achieved with low resistance, excellent surface hardness and penetration stability, reducing battery resistance, improving battery circulation performance and capacity, ensuring battery safety and efficient operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111864164B_ABST
    Figure CN111864164B_ABST
Patent Text Reader

Abstract

The present invention provides a separator for a secondary battery and an electrochemical device using the separator. More specifically, a composite separator is provided, which has a lower Gurley permeability after curing than before curing when a heat-resistant coating having low resistance is formed, does not have a significantly increased Gurley permeability compared to the Gurley permeability of a porous substrate itself before forming the coating, and has a generally low Gurley permeability, and has a high surface hardness to have penetration stability.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the priority benefit of Korean Patent Application No. 10-2019-0048599 filed on April 25, 2019, in the Korean Intellectual Property Office, the entire contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] The following invention relates to a separator for a secondary battery and an electrochemical device using the separator. More specifically, the following invention relates to a composite separator, when forming a heat-resistant coating having low resistance, the composite separator after curing has a lower Gurley permeability than before curing, and does not have a significantly increased Gurley permeability compared to the Gurley permeability of the porous substrate itself before forming the coating so as to have an overall low Gurley permeability, and has a high surface hardness to have penetration stability. Background Art

[0004] In recent years, according to the high capacity and high output trend of secondary batteries, there is a growing demand for high strength, high permeability and thermal stability of separators and improved characteristics of separators in terms of electrical safety during charging and discharging of secondary batteries. Lithium secondary batteries need to have high mechanical strength to improve safety during battery manufacturing and battery use, and need to have high permeability and high thermal stability to increase capacity and output.

[0005] In order to increase the output of a lithium secondary battery, it is important to achieve low resistance characteristics. In addition, it is important to make the porosity at a level at which pore clogging due to swelling of the binder in the electrolyte solution does not occur.

[0006] When a water-based ceramic coating is applied to a porous membrane, the resistance of the secondary battery increases. Specifically, when an aqueous adhesive is used, the adhesive enters the pores between the inorganic particles, causing the pores to be clogged. When the pores are clogged, the transmission channel through which lithium ions pass is disturbed, thereby increasing the resistance.

[0007] In addition, when preparing a conventional separator including an inorganic material layer, there are some problems with the coating method based on an adhesive composition soluble in an organic solvent. First, as the organic solvent evaporates during the drying process, the adhesive soluble in the organic solvent forms a gel, thereby creating a solvent-impermeable space, resulting in an unbalanced organic / inorganic coating, which may reduce the battery characteristics. In addition, explosion-proof equipment is required, and by-products harmful to the environment or the human body are generated during operation. In addition, there is the following problem: in a state where the adhesive is dissolved in an organic solvent, the pores of the porous polymer substrate are closed.

[0008] In order to solve this problem, Korean Patent Early Publication No. 10-2016-0041492 (April 18, 2016) proposed a method of using a polyvinylidene fluoride dispersion and a water-based slurry containing inorganic material particles and organic material particles to form a coating on a porous polymer substrate. It is proposed that the separator made therefrom has heat resistance, a porous substrate and excellent electrochemical properties, but still lacks battery resistance and stability levels, and therefore, improvement work is urgently needed.

[0009] In addition, when a nail or a pin penetrates a battery, it may be dangerous due to heat and fire. When a nail or a pin penetrates a battery, the separator and electrodes constituting the components of the battery are stretched along a specific portion in the penetration direction, and the stretched positive electrode or negative electrode is more likely to directly contact another electrode with a different polarity, and when direct contact occurs, a high current is caused due to a short circuit between the electrodes, which in turn may cause heating and fire of the entire battery.

[0010] [Related technical literature]

[0011] [Patent Document]

[0012] (Patent Document 1) Korean Patent Early Publication No. 10-2016-0041492 (April 18, 2016) Summary of the invention

[0013] An embodiment of the present invention is directed to providing a composite separator having low Gurley permeability, high surface hardness, and excellent resistance characteristics by coating a special coating layer on a porous substrate.

[0014] In an embodiment of the present invention, a self-crosslinking water-based latex adhesive with a high glass transition temperature and an epoxy crosslinking agent are mixed and coated, aiming to reduce Gurley permeability and improve the porosity of the inorganic material coating after heating and drying, thereby improving the resistance of the electrolyte solution. In addition, in terms of penetration stability, after crosslinking, the strength of the adhesive itself is improved to prevent fire due to short circuits between electrodes.

[0015] Another embodiment of the present invention is directed to providing a composite separator with improved safety, which has excellent surface hardness so that direct contact between electrodes does not occur in a penetration test.

[0016] Another embodiment of the present invention is directed to providing a composite membrane having increased hardness and reduced Gurley permeability.

[0017] Another embodiment of the present invention is directed to providing a composite separator which, through the above-mentioned advantages, allows the manufacture of a battery having excellent cycle performance and can achieve a desired high capacity.

[0018] Another embodiment of the present invention is directed to providing a composite separator having a coating layer having reduced battery resistance and excellent heat resistance.

[0019] In one general aspect, a composite separator is provided, comprising: a porous substrate; and a heat-resistant coating having a low electrical resistance formed on the porous substrate, wherein

[0020] A heat-resistant coating having low electrical resistance is formed by curing a coating layer obtained by coating a crosslinkable composition comprising inorganic particles, acrylic latex and a crosslinking agent,

[0021] The acrylic latex is coated on the surface of the inorganic particles in the form of a film, and

[0022] When the surface hardness is measured using a nanoindenter, the heat-resistant coating having a low electrical resistance has a hardness of 0.8 GPa or more at an indentation depth of 50 to 150 nm.

[0023] In another general aspect, an electrochemical device includes a composite separator. More specifically, the electrochemical device can be a lithium secondary battery.

[0024] Other features and aspects will become apparent from the following detailed description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a SEM photograph (magnified 20K times) of a coating layer obtained by coating the crosslinkable composition according to an exemplary embodiment of the present invention.

[0026] Figure 2 is a SEM photograph (magnified 20K times) of a heat-resistant coating layer having low resistance obtained by heating and curing a coating layer obtained by coating a crosslinkable composition according to an exemplary embodiment of the present invention.

[0027] Figure 3 is a SEM photograph (magnified 20K times) of a coating layer formed by forming a coating layer using the general water-based latex according to Comparative Example 1 and heating the coating layer. DETAILED DESCRIPTION

[0028] Hereinafter, the present invention will be described in more detail with reference to specific embodiments or exemplary embodiments including the accompanying drawings. However, the following specific embodiments or exemplary embodiments are only references for describing the present invention in detail, the present invention is not limited thereto, and can be implemented in various forms.

[0029] In addition, unless otherwise defined, all technical terms and scientific terms have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. The terms used herein are only used to effectively describe certain specific embodiments and are not intended to limit the present invention.

[0030] In addition, unless the context indicates otherwise, the singular forms used in the specification and the appended claims are intended to include the plural forms as well.

[0031] An embodiment of the present invention is a composite separator comprising a porous substrate and a heat-resistant coating having a low electrical resistance formed on the porous substrate, wherein:

[0032] A heat-resistant coating having low electrical resistance is formed by curing a coating layer obtained by coating a crosslinkable composition comprising inorganic particles, acrylic latex and a crosslinking agent,

[0033] The acrylic latex is coated on the surface of the inorganic particles in the form of a film, and

[0034] When the surface hardness is measured using a nanoindenter, the heat-resistant coating with low electrical resistance has a hardness of 0.8 GPa or more at an indentation depth of 50 to 150 nm.

[0035] The acrylic latex may be coated on the surface of the inorganic particles in the form of a film. The term "coated on the surface of the inorganic particles in the form of a film" means that the spherical binder particles are coated on the entire or partial surface of the inorganic particles in the form of a film without maintaining the spherical shape of the binder particles. Therefore, the aggregate form of the acrylic latex particles or the crosslinkable composition is not substantially observed.

[0036] In an embodiment of the present invention, the composite membrane may have a Gurley permeability satisfying the following Formula 1 and Formula 2:

[0037] [Formula 1]

[0038] G2≤200

[0039] [Formula 2]

[0040] G2 <G1

[0041] Among them, G2 is the Gurley permeability of the composite membrane measured according to ASTM D726 after the coating layer obtained by coating the cross-linkable composition is cured at 120°C for 1 hour, and G1 is the Gurley permeability of the composite membrane measured after coating the cross-linkable composition but before curing, and the unit is second / 100cc.

[0042] In an embodiment of the present invention, the composite membrane may have a Gurley permeability variation satisfying the following formula 3:

[0043] [Formula 3]

[0044] G1-G2≤100

[0045] In an embodiment of the present invention, the composite membrane may have a Gurley permeability variation satisfying the following formula 4:

[0046] [Formula 4]

[0047] G2-G3≤50

[0048] Wherein, G2 is the Gurley permeability of the composite membrane measured according to ASTM D726 after the coating layer obtained by coating the crosslinkable composition is cured at 120° C. for 1 hour, and G3 is the Gurley permeability of the porous substrate itself, in seconds / 100 cc.

[0049] In an embodiment of the present invention, when the elastic modulus is measured using a nanoindenter, the heat-resistant coating layer having a low electrical resistance may have an elastic modulus of 0.3 GPa or more at an indentation depth of 50 to 150 nm.

[0050] The acrylic latex is obtained by reacting an acrylic resin with a melamine-based curing agent or a melamine-formaldehyde-based curing agent in the presence of an amine-based catalyst, and may contain a hydroxyl group at the terminal.

[0051] The heat-resistant coating layer having low resistance may include inorganic particles and acrylic latex in a weight ratio of 50-90:10-50.

[0052] The acrylic latex may have an average particle diameter of 10 to 300 nm.

[0053] The crosslinking agent may be an epoxy-based crosslinking agent.

[0054] The content of the crosslinking agent may be 1 to 30 wt % of the content of the acrylic latex.

[0055] In the embodiment of the present invention, the aggregate form of the acrylic latex particles or the crosslinkable composition is not observed in the heat-resistant coating having low electrical resistance by curing.

[0056] The aggregates can be observed by magnifying the prepared composite membrane by 20K times by SEM. In the present invention, Figure 2 As shown in FIG. 1 , voids are formed between the inorganic particles. Aggregates are Figure 3 As shown, some aggregated agglomerates were observed, but no voids were formed between the inorganic particles.

[0057] The acrylic latex may be melted at 80° C. to 150° C. and self-crosslinked with the crosslinking agent.

[0058] The inorganic particles may have an average particle diameter of 1 μm or less.

[0059] The inorganic particles may be boehmite.

[0060] The heat-resistant coating layer having low electrical resistance may have a thickness of 1 to 10 μm.

[0061] Another embodiment of the present invention is an electrochemical device including the composite separator.

[0062] In an embodiment of the present invention, the electrochemical device may be a lithium secondary battery.

[0063] Hereinafter, each constituent element of the present invention will be described in more detail.

[0064] [Porous substrate]

[0065] In the embodiment of the present invention, the porous substrate is not limited as long as it is generally used as a separator for a secondary battery.

[0066] For example, the porous substrate may be formed of a woven fabric, a nonwoven fabric, a porous film, etc. The material of the porous substrate is not limited, and specifically, for example, it may be formed of any one selected from the following: polyethylene, polypropylene, polybutylene, polypentene, polymethylpentene, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, copolymers thereof, etc., or a mixture of two or more thereof.

[0067] The thickness of the porous substrate is not limited, and may be generally 1 to 100 μm, specifically 5 to 50 μm, more preferably 6 to 30 μm, which are ranges used in the art.

[0068] In an embodiment of the present invention, since a composite diaphragm having excellent air permeability and a total Gurley permeability of 200 sec / 100 cc can be provided after forming a heat-resistant coating with low resistance, the Gurley permeability of the porous substrate can be less than 200 sec / 100 cc, specifically less than 150 sec / 100 cc, and more specifically less than 100 sec / 100 cc.

[0069] [Heat-resistant coating with low electrical resistance]

[0070] The composite separator of the present invention has high heat resistance and high surface hardness by forming a heat-resistant coating with low resistance, does not cause fire in a penetration test, and has low Gurley permeability, thereby greatly reducing the resistance during battery assembly.

[0071] In embodiments of the present invention, the heat-resistant coating with low resistance can be formed by solidifying a coating layer, which is obtained by coating a crosslinkable composition comprising inorganic particles, acrylic latex and a crosslinking agent. Here, acrylic latex and a crosslinking agent are solidified and melted to have the form of a film coated and adsorbed on the surface of inorganic particles. More specifically, the heat-resistant coating with low resistance can be coated on the surface of inorganic particles in the form of a film, and the statement "coated on the surface of inorganic particles in the form of a film" refers to coating spherical adhesive particles on all or part of the surface of inorganic particles in the form of a film, without keeping the spherical shape of adhesive particles. Therefore, by solidification, the aggregate form of acrylic latex particles or crosslinkable compositions will not be observed in the heat-resistant coating with low resistance. Aggregates can be observed by measuring SEM and amplifying SEM 20K times, and it can be observed that inorganic particles do not aggregate and there are gaps between inorganic particles.

[0072] Therefore, an unprecedented phenomenon in which the Gurley permeability is further greatly reduced compared to the Gurley permeability before curing can be shown. This phenomenon is unusual and in sharp contrast to the fact that ordinary organic particles made of polymers melt when heated to form aggregates, thereby increasing the Gurley permeability after heating. That is, when the heat-resistant coating with low resistance of the present invention is formed, the composite diaphragm has a low Gurley permeability, thereby having excellent air permeability, has a high hardness, so that when measured using a nanoindenter, the surface hardness is 0.8 GPa or more, and has excellent heat resistance.

[0073] In an embodiment of the present invention, a coating layer obtained by coating a crosslinkable composition comprising inorganic particles, acrylic latex and a crosslinking agent is cured to crosslink the acrylic latex and the crosslinking agent, thereby coating a heat-resistant coating having low resistance on the surface of the inorganic particles in the form of a film.

[0074] For example, the Figure 1 and Figure 2 Provide specific examples. Figure 1 is a photograph of a coating layer obtained by coating a crosslinkable composition, such as Figure 1 As shown, it can be confirmed that the acrylic latex exists in a spherical shape. Figure 2 is a photograph of a heat-resistant coating having low electrical resistance obtained by heating and curing a coating layer obtained by coating a crosslinkable composition, such as Figure 2As shown, the acrylic latex and the cross-linking agent melt and cross-link after heating and curing, and the acrylic latex self-cross-links to coat and adsorb on the surface of the inorganic particles in the form of a film, so that the spherical particles of the acrylic latex are not seen, and there are no gaps between the inorganic particles. In this regard, Figure 3 : is a SEM photograph (magnified 20K times) of a coating layer formed by forming a coating layer using a conventional water-based latex and heating the coating layer. As shown in the portion marked with a red circle, it can be seen that aggregates are formed between the inorganic particles.

[0075] In addition, it was confirmed that when the Gurley permeability of the coating layer obtained by coating the crosslinkable composition was measured, the Gurley permeability after curing was greatly reduced compared to the Gurley permeability before curing, thus recognizing that the acrylic latex was coated and adsorbed on the surface of the inorganic particles. Therefore, the Gurley permeability after curing was further reduced compared to the Gurley permeability after coating the crosslinkable composition and before curing, thereby providing a composite separator having further improved air permeability after curing.

[0076] In an embodiment of the present invention, the composite membrane may have a Gurley permeability satisfying the following Formula 1 and Formula 2:

[0077] [Formula 1]

[0078] G2≤200

[0079] [Formula 2]

[0080] G2 <G1

[0081] Among them, G2 is the Gurley permeability of the composite membrane measured according to ASTM D726 after the coating layer obtained by coating the cross-linkable composition is cured at 120°C for 1 hour, and G1 is the Gurley permeability of the composite membrane measured after coating the cross-linkable composition but before curing, and the unit is second / 100cc.

[0082] In Formula 1 and Formula 2, G2 can be less than 200 seconds / 100cc, specifically 100 to 200 seconds / 100cc, more specifically 120 to 190 seconds / 100cc, and more specifically 150 to 180 seconds / 100cc. Within this range, the air permeability is excellent, the battery resistance is further reduced, and the electrochemical stability is excellent, so this is preferred. Specifically, the following excellent effects can be achieved: the battery resistance is less than 700mΩ, more preferably less than 690mΩ, and the 100 cycle life retention rate during the battery life characteristic evaluation is more than 90%, more preferably more than 95%.

[0083] In addition, as can be seen from Formula 2, in the composite diaphragm according to an embodiment of the present invention, the coating layer obtained by coating a cross-linkable composition comprising inorganic particles, acrylic latex and a cross-linking agent is heated and cured, so that the acrylic latex and the cross-linking agent are cured and melted, and coated on the surface of the inorganic particles, and therefore, after heating and curing, the permeability tends to be greatly reduced.

[0084] More specifically, the composite membrane may have a Gurley permeability variation satisfying the following Formula 3:

[0085] [Formula 3]

[0086] G1-G2≤100

[0087] Among them, G2 is the Gurley permeability of the composite membrane measured according to ASTM D726 after the coating layer obtained by coating the cross-linkable composition is cured at 120°C for 1 hour, and G1 is the Gurley permeability of the composite membrane measured after coating the cross-linkable composition but before curing, and the unit is second / 100cc.

[0088] Specifically, in Formula 3, G1-G2 may be 100 sec / 100 cc or less, specifically, for example, 1 to 100 sec / 100 cc, 2 to 90 sec / 100 cc, more specifically 5 to 80 sec / 100 cc, and more specifically 10 to 50 sec / 100 cc.

[0089] This is completely different from the physical property of using ordinary organic particles, in which the permeability increases due to the aggregation of organic particles after heating.

[0090] In addition, the composite membrane may have a Gurley permeability variation satisfying the following formula 4:

[0091] [Formula 4]

[0092] G2-G3≤50

[0093] Wherein, G2 is the Gurley permeability of the composite membrane measured according to ASTM D726 after the coating layer obtained by coating the crosslinkable composition is cured at 120° C. for 1 hour, and G3 is the Gurley permeability of the porous substrate itself, in seconds / 100 cc.

[0094] More specifically, in Formula 4, G2-G3 may be 50 seconds / 100 cc or less, specifically 1 to 50 seconds / 100 cc or less, and more specifically 10 to 30 seconds / 100 cc or less.

[0095] In addition, the change rate of the Gurley permeability represented by the following Formula 5 may be 10% or less. More specifically, the change rate of the Gurley permeability may be 1% to 10%.

[0096] [Formula 5]

[0097] (G1-G2) / G1×100

[0098] Among them, G2 is the Gurley permeability of the composite membrane measured according to ASTM D726 after the coating layer obtained by coating the cross-linkable composition is cured at 120°C for 1 hour, and G1 is the Gurley permeability of the composite membrane measured after coating the cross-linkable composition but before curing, and the unit is second / 100cc.

[0099] In addition, in the composite diaphragm according to an embodiment of the present invention, when the hardness is measured using a nanoindenter, the heat-resistant coating with low resistance has a high hardness of more than 0.8 GPa, specifically 0.8 to 1.1 GPa, and more specifically 0.85 to 0.95 GPa at an indentation depth of 50 to 150 nm. Within this range, battery stability can be provided so that fire does not occur in the penetration test. The surface hardness is measured at points 50 to 150 nm from the coating surface in the thickness direction using a nanoindenter (MTS (USA, Nano Indenter XP)). The results at deeper indentation depths are considered to be characteristics of porous substrates or inorganic materials. In addition, in order to evaluate more accurately, it is preferred to measure the surface hardness by measuring the hardness at 9 points in an area of ​​100 μm × 100 μm, removing the noise value caused by the inorganic material, and taking the average value thereof.

[0100] The Gurley permeability and surface hardness as described above may be due to the characteristics of the acrylic latex used as the organic particles in the embodiment of the present invention.

[0101] In an embodiment of the present invention, the acrylic latex is an aqueous dispersion in which nano-sized acrylic particles are dispersed and contains a thermoplastic or heat-curable acrylic resin and a curing agent. More specifically, the acrylic latex is a one-liquid type, which can be obtained by reacting an acrylic resin with a melamine-based curing agent or a melamine-formaldehyde-based curing agent in the presence of an amine-based catalyst, and contains a hydroxyl group at the terminal. Through the hydroxyl group at the terminal, water dispersion and self-crosslinking reactions can be performed.

[0102] The melamine-based curing agent may be a melamine-based compound, a polyaldehyde compound or a paraformaldehyde compound. More specifically, a melamine-based compound may be used, such as hexamethylolmelamine, hexamethoxymethylolmelamine (a compound in which 1 to 6 methylol groups of hexamethylolmelamine are methoxymethylated) or a mixture thereof, hexamethoxyethylmelamine, hexaacyloxymethylmelamine (a compound in which 1 to 6 methylol groups of hexamethylolmelamine are acyloxymethylated) or a mixture thereof.

[0103] The acrylic latex containing a melamine-based curing agent can be self-crosslinked in the presence of a catalyst, more specifically an acid catalyst. Specifically, the temperature for self-crosslinking in the presence of a catalyst is above 120°C, and in the absence of a catalyst, the self-crosslinking reaction can be carried out at a temperature of above 150°C. As a catalyst for self-crosslinking reaction, an acid catalyst can be used, specifically, for example, p-toluenesulfonic acid (p-TSA) and the like can be used, but not limited thereto. Based on the content of the acrylic latex including the melamine-based curing agent, the content of the acid catalyst can be 0.5 wt % to 1.5 wt %. When an acid catalyst is not used, a crosslinking reaction can be carried out by increasing the reaction time at 80°C to 120°C. Specifically, for example, by carrying out a crosslinking reaction for more than 1 hour at 120°C, the unit derived from the melamine-based curing agent or the formaldehyde-based curing agent is involved in the crosslinking reaction, thereby increasing the hardness of the coating.

[0104] Commercial examples of acrylic latexes containing melamine-based curing agents may include PRIMAL® available from Rohm and Haas. TM 3208 (solid content 44 wt%), etc., but not limited thereto.

[0105] An acrylic latex containing a melamine-based curing agent is dispersed in water to maintain a spherical shape.

[0106] The acrylic latex including the melamine-based curing agent may have a glass transition temperature of 40°C to 60°C, specifically 45°C to 55°C.

[0107] The acrylic latex containing the melamine-based curing agent may have an average particle size of 10 to 300 nm, specifically 50 to 250 nm, more specifically 90 to 150 nm. Within this range, it is easy to coat on the surface of the inorganic particles when heated and cured, so this is preferred.

[0108] Acrylic latex containing melamine-based curing agent can be used at 0.8 to 5 g / m 2 , more specifically 1 to 3 g / m 2 Contained in a heat-resistant coating having low electrical resistance. When the content of the organic particles is within this range, the Gurley permeability can be the lowest, so this is preferred.

[0109] The acrylic latex containing the melamine-based curing agent may be contained at 10 to 50 wt %, more specifically 20 to 30 wt %, based on 100 wt % of the total solid content in the heat-resistant coating having low resistance. Within this range, adhesive strength and coating stability are sufficiently exhibited.

[0110] In addition, when the acrylic latex is impregnated with an electrolyte solution, the acrylic latex containing a melamine-based curing agent can satisfy a physical property of a weight change rate of less than 50%, specifically 1 to 49%, and more specifically 10 to 40% according to the following Formula 6. Therefore, when the electrolyte solution is injected after manufacturing the electrode assembly, the composite separator including the heat-resistant coating layer having low resistance according to an embodiment of the present invention can prevent swelling or decomposition caused by the electrolyte solution.

[0111] Therefore, when the composite separator according to an embodiment of the present invention is applied, the phenomenon of swelling or decomposition caused by the electrolyte solution is significantly reduced, thereby further improving the cycle characteristics and resistance characteristics of the battery.

[0112] When the weight change rate was 50% or more, it was found that the initial life was very short when the battery life characteristics were measured.

[0113] The weight change rate is measured as follows. The acrylic latex containing a melamine-based curing agent used in the heat-resistant coating having low resistance of the present invention is placed in a Teflon dish, and water is evaporated at 60° C. for 1 day to form a film. 1 g of the film is immersed in an electrolyte solution and left to stand for 3 days, the electrolyte solution is poured out, and the weight of the film is measured to calculate the weight change rate.

[0114] [Formula 6]

[0115] Weight change rate = (W2-W1) / W1×100

[0116] Here, W2 is the weight measured after the acrylic latex was impregnated with the electrolyte solution for 3 days, and W1 is the weight measured before the acrylic latex was impregnated with the electrolyte.

[0117] Here, as the electrolyte solution, any electrolyte solution can be used without restriction, as long as it is commonly used in the art, for example, it can be selected from any one of the following: organic solvents such as carbonate-based solvents, nitrile-based solvents, ester-based solvents, ether-based solvents, ketone-based solvents, glycol dimethyl ether-based solvents, alcohol-based solvents and aprotic solvents, and water, or a mixed solvent of two or more thereof. In addition, the solvent may further include a lithium salt.

[0118] The carbonate-based solvent may be any one selected from ethylene carbonate, propylene carbonate, butylene carbonate, ethyl methyl carbonate, ethyl propyl carbonate, methyl propyl carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, etc., or a mixture of two or more thereof, but is not limited thereto.

[0119] The nitrile-based solvent may be any one selected from the group consisting of acetonitrile, succinonitrile, adiponitrile, sebaconitrile, etc., or a mixture of two or more thereof, but is not limited thereto.

[0120] The ester-based solvent may be any one selected from the following: methyl acetate, ethyl acetate, n-propyl acetate, 1,1-dimethylethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, decanoic acid lactone, valerolactone, mevalonolactone, caprolactone, etc., or a mixture of two or more thereof, but is not limited thereto.

[0121] The ether-based solvent may be any one selected from dimethyl ether, dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc., or a mixture of two or more thereof, but is not limited thereto.

[0122] The ketone-based solvent may be cyclohexanone or the like.

[0123] The glyme-based solvent may be any one selected from ethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, etc., or a mixture of two or more thereof, but is not limited thereto.

[0124] The alcohol-based solvent can be ethanol, isopropanol, etc., and the aprotic solvent can be nitrile (such as R-CN (R is a linear, branched or cyclic C2 to C20 hydrocarbon group, which may include a double bond aromatic ring or an ether bond)), amide (such as dimethylformamide), dioxolane (such as 1,3-dioxolane), cyclopentane, etc.

[0125] The lithium salt can be any one selected from the following: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroantimonate (LiSbF6), lithium hexafluoroarsenate (LiAsF6), lithium difluoromethanesulfonate (LiC4F9SO3), lithium perchlorate (LiClO4), lithium aluminate (LiAlO2), lithium tetrachloroaluminate (LiAlCl4), lithium chloride (LiCl), lithium iodide (LiI), lithium bis(oxalato)borate (LiB(C2O4)2), lithium bis(trifluoromethanesulfonyl)imide (LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)) (where x and y are natural numbers), and their derivatives, or a mixture of two or more of them. The concentration of the lithium salt can be 0.1 to 10.0 M, more specifically 1 to 10 M, but is not limited thereto.

[0126] More specifically, for example, the electrolyte can be a mixture of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate in a volume ratio of 3:5:2.

[0127] In an embodiment of the present invention, as the inorganic particles, specifically, for example, boehmite, calcium carbonate, talc, clay, kaolin, silica, hydrotalcite, diatomaceous earth, magnesium carbonate, barium carbonate, calcium sulfate, magnesium sulfate, barium sulfate, aluminum hydroxide, magnesium hydroxide, calcium oxide, magnesium oxide, titanium oxide, aluminum oxide, mica, zeolite, glass, etc. can be used. Additionally, as the inorganic particles having a dielectric constant of 5 or more, any one selected from the following can be used: SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC, etc., or a mixture of two or more of them. Additionally, as the inorganic material particles having piezoelectricity, any one of the following can be used: BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x LaxZr 1-y TiyO3 (PLZT), PB(Mg3Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnium dioxide (HfO2), etc., or a mixture of two or more of them. Additionally, as the inorganic material particles having lithium ion transfer ability, any one of the following can be used: lithium phosphate (Li3PO4), lithium titanium phosphate (LixTiy(PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O ySeries of glasses (0 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitrite (Li x N y , 0 < x < 4, 0 < y < 2), SiS2 (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4) series of glasses, P2S5 (Li x P y S z , 0 < x < 3, 0 < y < 3, 0 < z < 7) series of glasses, etc., or mixtures of two or more of them. When inorganic material particles with high dielectric constant, inorganic material particles with piezoelectricity, and inorganic material particles with lithium ion transfer ability are used in combination, their synergistic effect may be doubled.

[0128] More preferably, boehmite can be used, and when boehmite is used, the phenomena of battery swelling and separator release caused by surface friction are significantly improved, so this is further preferred. In addition, boehmite is more economical than alumina and is preferred in reducing the wear of coating equipment.

[0129] The size of the inorganic particles is not limited, and the average particle size can be 1 μm or less, more specifically 0.001 to 1 μm, more specifically 0.01 to 0.9 μm, more specifically 0.1 to 0.85 μm, and still more preferably 0.5 to 0.8 μm. Within this range, an appropriate porosity can be adopted, so this is preferred.

[0130] The content of the inorganic particles is not limited. Based on the total solid content of 100% by weight used in the heat-resistant coating with low resistance, the content of the inorganic particles can be 50 to 90% by weight, more specifically 60 to 80% by weight. Within this range, the required heat resistance is fully achieved.

[0131] The inorganic particles can be contained in the heat-resistant coating with low resistance at 0.8 to 10 g / m 2 , more specifically at 2 to 8 g / m 2 . When the content of the inorganic particles is within this range, the change in Gurley permeability can be minimized.

[0132] In the embodiment of the present invention, there is no limitation on the crosslinking agent as long as it crosslinks the acrylic latex, and the crosslinking agent may be a thermal crosslinking agent. In addition to the self-crosslinking of the acrylic latex, the crosslinking agent further crosslinks, thereby providing a separator having a higher surface hardness and a lower Gurley permeability, and thus can exhibit the effects of low battery resistance, stability in a nail penetration test, and excellent battery life characteristics.

[0133] Specifically, for example, an epoxy crosslinking agent can be used. The epoxy crosslinking agent can be any one selected from the following: ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, diglycerol polyglycidyl ether and sorbitol polyglycidyl ether, or a mixture of two or more thereof. In addition, the content of the crosslinking agent can be 1% to 30% by weight of the content of the acrylic latex comprising a melamine-based curing agent. More specifically, the crosslinking agent can be used with 5% to 25% by weight. Within this range, a coating with excellent hardness can be formed, so this is preferred.

[0134] In an embodiment of the present invention, a heat-resistant coating having low resistance is formed by forming a coating layer, heating and curing the coating layer, the coating layer being obtained by coating a crosslinkable composition, the crosslinkable composition being a water-based slurry including inorganic particles, an acrylic latex containing a melamine-based curing agent, a crosslinking agent and water, and the solid content of the particles in the water-based slurry may be 1 wt % to 30 wt %. That is, the particles may be contained in the water-based slurry at 10 wt % to 50 wt %, in which the inorganic particles and the acrylic latex containing a melamine-based curing agent are mixed at a weight ratio of 50 to 90:10 to 50.

[0135] In an embodiment of the present invention, an acrylic latex containing a melamine-based curing agent is cross-linked with a cross-linking agent at 80°C to 120°C and melted, self-cross-linked, and coated on the surface of the inorganic particles in the form of a film. Therefore, after the cross-linkable composition is applied to form a coating layer, heating and curing can be performed at 80°C to 120°C. In this temperature range, a heat-resistant coating with low resistance having a better hardness can be formed, so it is preferred. Although not limited thereto, heating and curing can be preferably performed at 80°C to 120°C for 30 minutes to 2 hours.

[0136] In the embodiment of the present invention, the heat-resistant coating layer having low electrical resistance may be formed on the porous substrate, specifically, for example, may be formed on one surface or both surfaces of the porous substrate.

[0137] In an embodiment of the present invention, the heat-resistant coating with low resistance may have a thickness of 1 to 10 μm, more specifically 2 to 8 μm, more specifically 3 to 5 μm. Although not limited thereto, within this range, it is suitable to achieve the desired rate of change of Gurley permeability.

[0138] In an embodiment of the present invention, when the surface hardness is measured using a nanoindenter, the composite diaphragm has a hardness of more than 0.8 GPa, more specifically 0.8 to 1.1 GPa, and more specifically 0.8 to 1.0 GPa at an indentation depth of 50 to 150 nm. The indentation depth refers to a point 50 to 150 nm away from the surface in the thickness direction, at which the hardness is measured, and the reason why the point is 50 to 150 nm away from the surface is that there is a serious deviation on the surface due to surface roughness. Within the range of satisfying the hardness, for a diaphragm with improved stability and a secondary battery including the diaphragm, more specifically, at a higher hardness, the resistance to penetration by nails is increased, thereby ensuring the internal short circuit safety of the secondary battery, so this is preferred.

[0139] In the penetration evaluation, the secondary battery is fixed to a test device to measure the temperature and voltage of the secondary battery, a sharp metal nail with a diameter of 3 mm (SK3-JIS, Japan) is passed through the battery at a speed of 80 m / s to deliberately cause an internal short circuit in the secondary battery, and the temperature or voltage change is measured. Whether the secondary battery is on fire can be visually confirmed.

[0140] In addition, when the elastic modulus is measured using a nanoindenter, the elastic modulus at an indentation depth of 50 to 150 nm can be 0.3 GPa or more, specifically 0.3 to 1.0 GPa. Within this range, it can be more clearly confirmed that the penetration is significantly different. The high elastic modulus is caused by the high cross-linking density. However, since too high a cross-linking density will increase resistance, penetration stability, reduced battery resistance, and an elastic modulus increased by increasing the cross-linking density are optimal conditions and are therefore preferred.

[0141] [Manufacturing method]

[0142] In an embodiment of the present invention, a method for forming a heat-resistant coating having low resistance may be to apply a crosslinkable composition including inorganic particles, acrylic latex and a crosslinking agent on a porous substrate to form a coating layer, and to cure the coating layer to cure and melt the acrylic latex and the crosslinking agent, thereby forming a heat-resistant coating having low resistance on the surface of the inorganic particles. More specifically, the curing may be thermal curing.

[0143] The coating method is not limited, and specifically, for example, it may be a common coating method such as rod coating, dip coating, and spray coating.

[0144] In the process of heating and curing after coating, the temperature may be a temperature at which the acrylic latex and the crosslinking agent are crosslinked and self-crosslinked to be coated on the surface of the inorganic particles in the form of a film, specifically 80° C. to 150° C., preferably 80° C. to 120° C. In addition, as the curing time increases, the surface hardness may be further improved, and without being limited thereto, by performing curing for 30 minutes to 2 hours, a coating having excellent surface hardness may be formed.

[0145] Heat curing may be performed after drying, or heat curing may be performed alone. When heat curing is performed within this range, the coating is uniformly cured without affecting the physical properties of the porous substrate, thereby preventing poor coating, and thus this is preferred. The heat curing step is a step of drying the water of the water-based slurry formed on the porous substrate and inducing a curing reaction of the heat curing agent to finally form a coating.

[0146] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples. However, the following Examples and Comparative Examples are merely examples for describing the present invention in detail, and do not limit the present invention in any way.

[0147] 1. Gurley penetration

[0148] Gurley permeability was measured as air permeability. Gurley permeability was measured using a Densometer available from Toyoseiki according to ASTM D726. The time required for 100 cc of air to pass through a membrane having an area of ​​1 square inch was recorded in seconds and compared.

[0149] 2. Surface hardness and elastic modulus

[0150] The surface hardness of the composite membrane was measured using a nanoindenter (MTS (USA, Nano Indenter XP)).

[0151] More precisely, for the same sample, an average value is compared as the surface hardness, which is obtained by measuring the hardness at 9 points in an area of ​​100 μm×100 μm, removing noise values ​​due to inorganic materials, and averaging them.

[0152] The elastic modulus was measured at a point 50 to 150 nm from the surface.

[0153] 3. Battery resistance

[0154] 1) Preparation of positive electrode

[0155] 94 wt% of LiCoO2 as a positive electrode active material, 2.5 wt% of polyvinylidene fluoride as a binder (fusing agent), and 3.5 wt% of carbon black as a conductive agent were added to N-methylpyrrolidone as a solvent so that the solid content was 50 wt%, and the solution was stirred to prepare a uniform positive electrode slurry. The positive electrode slurry was coated on an aluminum foil with a thickness of 30 μm, dried and pressed to prepare a positive plate with a thickness of 150 μm.

[0156] 2) Preparation of negative electrode

[0157] 95 wt% of artificial graphite as a negative electrode active material, 3 wt% of acrylic latex with a Tg of -52°C as a binder, and 2 wt% of carboxymethyl cellulose as a thickener were added to water as a solvent so that the solid content was 48 wt%, and the solution was stirred to prepare a uniform negative electrode slurry. The negative electrode slurry was coated on a copper foil with a thickness of 20 μm, dried and pressed to prepare a negative electrode plate with a thickness of 150 μm.

[0158] The composite separator manufactured in the embodiment and the comparative example is used between the positive electrode and the negative electrode manufactured as above, the pouch-type batteries are assembled in a stacked manner, and the electrolyte solution (6 g) is injected to manufacture a lithium secondary battery, wherein lithium hexafluorophosphate (LiPF6) is dissolved at 1 M in a mixed solution of ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 25:45:30.

[0159] 4. Battery life characteristics

[0160] Each battery manufactured in the above-mentioned assembly process was charged and discharged 500 times at a discharge rate of 1C, and then the discharge capacity was measured and cycle evaluation was performed to measure the degree of reduction in capacity relative to the initial capacity.

[0161] The initial battery life decline means that the capacity retention rate drops by more than 20% within 50 cycles.

[0162] 5. Penetration Testing

[0163] Batteries were assembled using the composite separators prepared in the examples and comparative examples, charged to 80% at a voltage of 4.2 V, and a nail with a diameter of 3 mm was used to penetrate the center of the battery at a speed of 80 m / sec to observe whether the battery caught fire. A total of three samples were prepared, and the number of batteries that exploded was evaluated.

[0164] L1: no change, L2: slight heat, L3: leakage, L4: smoke, L5: fire, among which L1 to L3 are judged as qualified, and L4 and L5 are judged as unqualified.

[0165] Although charged to SOC 80% (temperature 49.4° C.), in the example, as a result of the penetration test, there was no ignition, and thus, penetration safety (L3) was confirmed.

[0166] [Example 1]

[0167] <Preparation of slurry for heat-resistant coating having low resistance (crosslinkable composition)>

[0168] A mixture of boehmite particles having an average particle size of 0.7 μm and acrylic latex (ROHM & HASS, PRIMAL™ 3208, solid content of 44 wt %) in a weight ratio of 90:10 was used, an epoxy-based crosslinking agent (Nagase Chemtech, DENACOL EX-614B) was added at 20 wt % of the content of the latex binder, and then the mixture was diluted with water to a total solid content of 32 wt %, thereby preparing a crosslinkable composition.

[0169] As the acrylic latex, a melamine-based curing agent containing an average particle size of 120 nm and a glass transition temperature of 48° C. (ROHM & HASS, PRIMAL TM 3208, 44 wt% solids).

[0170] <Preparation of composite diaphragm>

[0171] The crosslinkable composition was coated on both surfaces of a polyethylene-based porous substrate having a Gurley permeability of 150 seconds / 100cc and a thickness of 9 μm (SK Innovation, ENPASS) using a slit coating die to form a coating layer. The coating was carried out at a speed of 10 m / min, and the coating layer was passed through a dryer with a length of 6 m and hot air blown out at 50°C, and wound into a roll. After winding, the layer was thermally cured at 120°C for 1 hour, and the total thickness of the composite diaphragm including the heat-resistant coating with low resistance formed by curing the coating layer was 11 μm. The physical properties of the prepared composite diaphragm were measured and are shown in Table 1 below.

[0172] like Figure 1 As shown, before curing, there is an acrylic latex including a spherical melamine-based curing agent on the coating layer, but as shown in FIG. Figure 2 As shown, after curing, it can be confirmed that the acrylic latex containing the melamine-based curing agent and the crosslinking agent melts and self-crosslinks on the inorganic particles and is coated on the surface of the inorganic particles in the form of a film, so that no spherical particles are seen.

[0173] In addition, the Gurley permeability before curing was 182 sec / 100 cc, but further decreased to 170 sec / 100 cc after curing. The rate of change in the Gurley permeability was -6.6%.

[0174] [Example 2 and Example 3]

[0175] This process was performed in the same manner as in Example 1, except that the contents of the inorganic particles and the acrylic latex were changed as shown in Table 1 below.

[0176] [Comparative Example 1]

[0177] The process was performed in the same manner as in Example 1, except that an acrylic latex that was not reacted with a melamine-based curing agent (acrylic latex prepared using acrylate, the acrylic latex having a glass transition temperature of 45° C. and a particle size of 120 nm) was used instead of the acrylic latex containing a melamine-based curing agent, and no epoxy cross-linking agent was used.

[0178] [Comparative Example 2]

[0179] This process was performed in the same manner as in Example 1, except that the acrylic latex and polyvinyl alcohol (PVA) adhesive used in Comparative Example 1 were mixed in the same amounts and used.

[0180] [Comparative Example 3]

[0181] The process was carried out in the same manner as in Example 1, except that the same adhesive as in Example 1 was used and no epoxy crosslinking agent was used.

[0182] The crosslinkable compositions used in the above Examples and Comparative Examples are summarized and shown in Table 1, and the physical properties of the composite separators prepared in the Examples and Comparative Examples are evaluated and shown in Table 2 below.

[0183] [Table 1]

[0184]

[0185] [Table 2]

[0186]

[0187]

[0188] According to an embodiment of the present invention, a composite separator for a secondary battery having excellent surface hardness and excellent stability so that ignition does not occur in a penetration test can be provided.

[0189] Furthermore, the separator has a low Gurley permeability to have excellent gas permeability, and a battery manufactured therefrom has greatly reduced resistance.

[0190] In addition, according to an embodiment of the present invention, a composite separator can be provided that allows the manufacture of a battery having excellent cycle characteristics and that can achieve a desired high capacity.

[0191] In addition, according to the embodiments of the present invention, a composite separator having excellent heat resistance can be provided.

[0192] In the above, although the present invention has been described by specific matters, and limited exemplary embodiments and drawings, they are provided only to help fully understand the present invention. Therefore, the present invention is not limited to the exemplary embodiments, and those skilled in the art to which this specification belongs can make various modifications and changes based on this specification.

[0193] Therefore, the spirit of the present invention should not be limited to the above-described exemplary embodiments, and the appended claims and all claims modified equivalent to or equivalent to the claims are intended to fall within the scope and spirit of the present invention.

Claims

1. A composite diaphragm comprising a porous substrate and a heat-resistant coating having a low electrical resistance formed on the porous substrate, wherein: The heat-resistant coating having low electrical resistance is formed by curing a coating layer obtained by coating a crosslinkable composition comprising inorganic particles, acrylic latex, and a crosslinking agent, The acrylic latex is coated on the surface of the inorganic particles in the form of a film, and When the surface hardness is measured using a nanoindenter, the heat-resistant coating having low electrical resistance has a hardness of 0.8 GPa or more at an indentation depth of 50 to 150 nm. Herein, the acrylic latex is obtained by reacting an acrylic resin with a melamine-based curing agent or a melamine-formaldehyde-based curing agent, and the acrylic latex includes a hydroxyl group at a terminal.

2. The composite diaphragm according to claim 1, wherein: The composite membrane has a Gurley permeability satisfying the following formula 1 and formula 2: [Formula 1] G2≤200 [Formula 2] G2 <G1 Among them, G2 is the Gurley permeability of the composite membrane measured according to ASTM D726 after the coating layer obtained by coating the cross-linkable composition is cured at 120°C for 1 hour, and G1 is the Gurley permeability of the composite membrane measured after coating the cross-linkable composition but before curing, in units of seconds / 100cc.

3. The composite diaphragm according to claim 2, wherein: The composite membrane has a Gurley permeability variation satisfying the following formula 3: [Formula 3] G1-G2≤100.

4. The composite diaphragm according to claim 2, wherein: The composite membrane has a Gurley permeability variation satisfying the following formula 4: [Formula 4] G2-G3≤50 Wherein, G2 is the Gurley permeability of the composite membrane measured according to ASTM D726 after the coating layer obtained by coating the crosslinkable composition is cured at 120° C. for 1 hour, and G3 is the Gurley permeability of the porous substrate itself, in seconds / 100 cc.

5. The composite diaphragm according to claim 1, wherein: When the elastic modulus is measured using the nanoindenter, the heat-resistant coating layer having low electrical resistance has an elastic modulus of 0.3 GPa or more at an indentation depth of 50 to 150 nm.

6. The composite diaphragm according to claim 1, wherein: The reaction of the acrylic resin with the melamine-based curing agent or the melamine-formaldehyde-based curing agent is carried out in the presence of an amine-based catalyst.

7. The composite diaphragm according to claim 1, wherein: The heat-resistant coating layer having low resistance includes the inorganic particles and the acrylic latex in a weight ratio of 50 to 90:10 to 50.

8. The composite diaphragm according to claim 1, wherein: The acrylic latex has an average particle diameter of 10 to 300 nm.

9. The composite diaphragm according to claim 1, wherein: The crosslinking agent is an epoxy crosslinking agent. 10 . The composite separator according to claim 1 , wherein the content of the crosslinking agent is 1 to 30 wt % based on the content of the acrylic latex.

11. The composite diaphragm according to claim 1, wherein: By the curing, no particles of the acrylic latex or aggregate forms of the crosslinkable composition were observed in the heat-resistant coating having low electrical resistance.

12. The composite diaphragm according to claim 1, wherein: The acrylic latex melts at 80° C. to 150° C. and self-crosslinks with the crosslinking agent.

13. The composite diaphragm according to claim 1, wherein: The inorganic particles have an average particle size of 1 μm or less. The composite separator according to claim 13 , wherein the inorganic particles are boehmite.

15. The composite diaphragm according to claim 1, wherein: The heat-resistant coating layer having low electrical resistance has a thickness of 1 to 10 μm.

16. An electrochemical device comprising the composite separator according to any one of claims 1 to 15.