Method for producing organic microparticles and method for modifying organic microparticles
By adding surfactants to organic particles and using solvents with part of the solubility capacity, the problem of growth and necking of organic particles in solvents is solved, and fine control of particle size and crystallinity is achieved, which is suitable for a variety of industrial applications. .
Patent Information
- Application Number
- CN202010980088.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2015-12-07
- Filing Date
- 2015-12-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2035-12-15
AI Technical Summary
It is difficult to effectively control the particle size and crystallinity of organic particles with existing technology, resulting in growth, coarsening or necking in solvents, affecting their performance and application.
Surfactants are added to organic particles containing amorphous matter to allow them to act in a solvent that has some solubility, thereby controlling the particle size and crystallinity of the particles and inhibiting growth and necking.
It achieves precise control of organic particles, maintains its original performance, is suitable for various industrial applications, and reduces production costs.
Smart Images

Figure CN112094221B_ABST
Abstract
Description
[0001] This application is a divisional application of a patent application with application number "201580068325.6", application date "December 15, 2015", and invention name "Method for producing organic microparticles and method for modifying organic microparticles". Technical Field
[0002] The present invention relates to a method for producing organic microparticles and a method for modifying organic microparticles. Background Art
[0003] By making conventional organic matter into microparticles, especially nanoparticles, it is possible to make the physical properties of the organic matter exhibit new functions, and therefore the technology of nanoparticleization of organic matter has become an important theme in the entire industry.
[0004] Organic nanoparticles have a much higher specific surface area and are more reactive than solids of several μm or more. They have improved functions such as increased activity and are expected to be used in a wide range of technical fields as materials that can dramatically improve their original properties.
[0005] In order to exert expected properties as organic nanoparticles, it is necessary to control the particle size. Generally, organic nanoparticles have problems such as particle growth due to recrystallization, particle coarsening, and necking, due to their improved solubility in solvents.
[0006] Therefore, as in Patent Document 1, a method for producing a biological ingestible material in which the particle size is maintained by pulverizing the pigment in a poor solvent containing a surface modifier has been proposed, and in Patent Document 9, a method for producing an organic pigment by adding an organic solvent to a cyan organic pigment such as copper phthalocyanine and performing a dry pulverization process has been proposed.
[0007] However, when mechanical pulverization is performed as described in the document, the crystallinity of the particles is often reduced, and sometimes the particles after pulverization in a solvent are condensed and the particles become coarse. In addition, as a mechanical pulverization method, a pulverization method using a medium such as a ball mill, a sand mill, or a bead mill is often used, which is difficult to avoid the mixing of impurities from the device, and then a large amount of time and power are required to make it a target particle size.
[0008] In addition, in patent documentation 2, as the method for the nanoparticle composition that is used to make the stability of particle diameter and minimum crystal growth after long-term preservation and / or high temperature exposure, disclose adding surface stabilizer, carry out pulverization and coprecipitation.But, for crystallinity, stay on as crystal phase or as amorphous and have such record, for the control of crystallinity such as control of crystallinity, crystal form, do not show.In addition, as shown in patent documentation 10, adopting by mixing the organic matter nanometer particle that the method for separating out organic pigment particulate is made by dissolving organic pigment solution in the good solvent of soluble organic pigment and comparing with above-mentioned good solvent for the low poor solvent of solubility of above-mentioned organic pigment many contain amorphous component, exist in the problem of easy coarsening in organic solvent.
[0009] In order to exert the expected characteristics as organic nanoparticles, it is important to control not only the particle size but also the properties of particles such as crystallinity and crystal form. For example, in polymer compounds such as resins, it is known that in many cases the crystallinity of the resin strongly affects the occurrence of secondary coagulation and properties such as slip. Therefore, the following technique is disclosed in Patent Document 3: as heat-treated resin particles, the crystallinity of the resin particles is controlled by heat treatment at a temperature above the glass transition temperature and below the melting point. However, for this method, it is necessary to perform a long-term heat treatment, and a method that can more easily control the crystallinity is sought.
[0010] Therefore, in patent documents 4 and 8 proposed by the applicant of the present application, biological ingestion particles (patent document 4) or organic pigment particles (patent document 8) are precipitated in a thin film fluid between at least one of the processing surfaces that are arranged to be accessible and separable and that rotates relatively with respect to the other. According to these patent documents, it is possible to easily manufacture fine and uniform organic nanoparticles, and it is also possible to control the particle size and crystal form of the precipitated organic nanoparticles.
[0011] However, since the obtained organic nanoparticles are fine, their solubility increases with the increase in specific surface area. As a result, after the particles are precipitated, the particles may grow into coarse particles in the solvent due to the action of the amorphous part of the particles, or the particles may neck.
[0012] In addition, as a technology for changing the crystallite diameter of the precipitated particles without changing the particle size of the precipitated particles after precipitation, it is known as in Patent Document 5, that uniform and homogeneous particles are obtained by growing the nuclei or crystallites of the particles precipitated in a thin film fluid formed between at least two processing surfaces that are opposed, approachable and separable, and at least one of which rotates relative to the other. Specifically, after the fluid after the particles are precipitated is discharged from between the above-mentioned processing surfaces, the residence time and temperature of the above-mentioned fluid when passing through a tubular container are adjusted, thereby controlling the crystallite diameter of the particles.
[0013] However, in Patent Document 5, although the crystallite diameter of the particles is controlled by the residence time and the temperature, the coarsening and necking of the particles in the solvent after the above treatment are still not solved.
[0014] In addition, Patent Document 6 discloses that copper phthalocyanine powder is added to a solution of a dispersant dissolved in an organic solvent to prepare a sample for measurement, but the copper phthalocyanine particles used here are originally extremely crystalline, and the effects of the solvent and even the dispersant on the organic particles are completely different from those of the present invention. Since the dispersion treatment is performed for the purpose of measurement, it cannot be said that the particles are modified or their properties are controlled.
[0015] In organic matter, especially in the case of organic pigments, since the color characteristics of organic pigments depend on the properties of particles such as particle size and crystallinity, it is desired to precisely control the properties of organic pigments and organic pigment particles while expanding the use of organic pigments. However, there is no decisive means for controlling crystal growth, and for the commonly used method of nanoparticleizing organic pigments together with derivatives of organic pigments (Patent Document 7), since the color peculiar to the derivatives affects the color development of the organic pigments actually used, there is a problem that it is difficult to develop the desired color.
[0016] As described above, various organic substances such as biological ingestion, resins, and pigments have been used in various fields and for various purposes. However, in all applications, the properties of particles such as particle size and crystallinity have a great influence on their performance. Therefore, it is desirable to precisely control the properties of organic particles and suppress changes in their properties until the actual organic particles are used.
[0017] Prior art literature
[0018] Patent Literature
[0019] Patent Document 1: Japanese Patent Publication No. 8-501073
[0020] Patent Document 2: Japanese Patent Application No. 2002-538199
[0021] Patent Document 3: Japanese Patent Application Publication No. 2007-291168
[0022] Patent Document 4: Japanese Patent Application No. 2009-8391
[0023] Patent Document 5: Japanese Patent Application Publication No. 2014-23997
[0024] Patent Document 6: Japanese Patent Application Laid-Open No. 2010-242104
[0025] Patent Document 7: International Publication No. WO2008 / 044519 Pamphlet
[0026] Patent Document 8: Japanese Patent Application Publication No. 2009-82902
[0027] Patent Document 9: Japanese Patent Application Publication No. 2004-244563
[0028] Patent Document 10: Japanese Patent Application Publication No. 2006-193681 Summary of the invention
[0029] Problems to be solved by the invention
[0030] Therefore, the subject of the present invention is to provide a method for producing organic particles that can suppress the growth of organic particles in a solvent and improve crystallinity or cause a crystalline transformation in order to effectively utilize the original characteristics of organic particles. With regard to the above-mentioned subject, the inventors found through trial and error that a particle property control solution containing a surfactant that controls the effect of the organic particles on the organic particles in a solvent having a partial solubility for organic particles at least partially containing amorphous substances can be added to the solvent to act on the organic particles, thereby improving the crystallinity of the organic particles or causing a crystalline transformation of the organic particles without substantially changing the particle size of the organic particles, and thus completed the present invention.
[0031] Means for solving problems
[0032] That is, the present invention relates to a method for producing organic microparticles, characterized in that a surfactant is added to a solvent that has a partial solubility for organic microparticles at least a portion of which contains amorphous substances, and the solvent is allowed to act on the organic microparticles, thereby increasing the crystallinity of the organic microparticles without substantially changing the particle size of the organic microparticles.
[0033] In addition, the present invention relates to a method for producing organic microparticles, characterized in that a surfactant is added to a solvent that has a partial solubility for organic microparticles at least a portion of which is amorphous, and the above-mentioned solvent is allowed to act on the above-mentioned organic microparticles, thereby causing the above-mentioned organic microparticles to undergo crystallization transformation without substantially changing the particle size of the above-mentioned organic microparticles.
[0034] The present invention also relates to a method for producing organic microparticles, characterized in that the particle size change rate of the organic microparticles before and after the solvent to which the surfactant is added acts on the organic microparticles (after surfactant treatment (A) / before surfactant treatment (B)) is 1 to 4.
[0035] In addition, the present invention relates to a method for producing organic microparticles, characterized in that it includes: step 1: mixing a raw material solution of organic microparticles with a precipitation solvent L for precipitating at least one type of organic microparticles from the raw material solution of the organic microparticles to precipitate the organic microparticles (P1); and step 2: preparing a particle property control solution in which a surfactant that can inhibit the growth of the organic microparticles is added to a solvent that has a partial solubility for the organic microparticles, and allowing the particle property control solution to act on the organic microparticles (P1); the step 2 acts in a manner that controls the particle properties of the organic microparticles (P1).
[0036] The present invention also relates to a method for producing organic fine particles, wherein the step 2 is performed so as to change at least any one of the crystallinity, crystal form, and particle size of the organic fine particles (P1).
[0037] In addition, the present invention relates to a method for producing organic microparticles, characterized in that it includes a step c for washing and / or solvent replacement of the organic microparticles (P1) obtained in the above-mentioned step 1, and allowing the above-mentioned particle property control solution to act on the organic microparticles (P2) obtained in the above-mentioned step c.
[0038] The present invention also relates to a method for producing organic fine particles, wherein the organic fine particles contain amorphous material in at least a part thereof.
[0039] In addition, the present invention relates to a method for producing organic particles, characterized in that stirring is performed when the solvent is acted on the organic particles or when the particle property control solution is acted on the organic particles, and the properties of the organic particles, the organic particles (P1) or the organic particles (P2) are controlled by stirring energy.
[0040] The present invention also relates to a method for producing organic microparticles, wherein the organic microparticles are ingestible by a living body.
[0041] The present invention also relates to a method for producing organic fine particles, wherein the organic fine particles are resin.
[0042] The present invention also relates to a method for producing organic fine particles, wherein the organic fine particles are organic pigments such as red organic pigments and cyan organic pigments.
[0043] In addition, the present invention relates to a method for producing organic microparticles, characterized in that the above step 1 is performed using the following microreactor: at least two processed fluids, including a raw material solution containing organic microparticles and a precipitation solvent L, are introduced between a first processing surface and a second processing surface that are arranged to be approachable and detachable and opposite to each other, and at least one of them rotates relative to the other, and a separation force that acts in a direction of separating the first processing surface from the second processing surface is generated by an introduction pressure applied between the first processing surface and the second processing surface, and the above separation force allows the at least two processed fluids to merge between the first processing surface and the second processing surface maintained at the above-mentioned small interval while maintaining a small interval between the first processing surface and the second processing surface, and pass between the first processing surface and the second processing surface, thereby forming a thin film fluid, and reacting between the processed fluids in the above-mentioned thin film fluid. The above stirring can be performed using a stirrer equipped with a rotating stirring blade.
[0044] The particle size of the organic particles obtained by the manufacturing method can be modified according to the use of the particles, for example, it can be made to be 100 nm or less, or 30 nm or less. For example, the particle size of the organic particles before and after the organic particles are acted on by the solvent having a partial solubility for the organic particles to which the surfactant is added can be 100 nm or less, and the particle size of the organic particles (P1) can be 30 nm or less.
[0045] The present invention also relates to a method for producing organic fine particles, wherein the solvent contains substantially no pigment derivative.
[0046] In addition, the present invention relates to a method for modifying organic particles, which is a method for modifying organic particles without substantially changing the particle size of the organic particles, and is characterized in that it includes a step of allowing a particle property control solution prepared by adding a surfactant to a solvent having a partial solubility for the organic particles to act on the organic particles, whereby the crystallinity of the organic particles is improved, thereby modifying the organic particles into organic particles having a crystallinity that matches target set conditions.
[0047] In addition, the present invention relates to a method for modifying organic particles, which is a method for modifying organic particles without substantially changing the particle size of the organic particles, and is characterized in that it includes a step of allowing a particle property control solution prepared by adding a surfactant to a solvent having a partial solubility for the organic particles to act on the organic particles, whereby the crystal form of the organic particles is changed, thereby modifying the organic particles into organic particles having a crystal form that meets target set conditions.
[0048] The present invention also relates to a method for modifying organic particles, wherein the particle size change ratio of the organic particles before and after the treatment in the above step (after the treatment in the step (A) / before the treatment in the step (B)) is 1 to 4.
[0049] The present invention also relates to a method for modifying organic fine particles, wherein the organic fine particles before being subjected to the above-mentioned step contain amorphous matter in at least a part thereof.
[0050] Effects of the Invention
[0051] By using the manufacturing method of the present invention, the particle growth of organic particles can be suppressed, and the crystal form and crystallinity can be controlled, and organic particles that can fully exert the original performance of organic particles can be manufactured. In addition, by precisely controlling the properties of organic particles, a manufacturing method of organic particles that can meet various requirements of the industry can be provided. Furthermore, since the properties of particles can be easily controlled in a solvent that has a partial solubility for the above-mentioned organic particles, various types of organic particles with properties that match the target can be manufactured from a single organic particle, which can greatly reduce costs.
[0052] In particular, by applying the method for producing organic microparticles of the present invention to a forced thin film type microreactor that can control the crystallinity of the precipitated particles, after precipitating organic microparticles containing amorphous substances from the microreactor, the properties of the microparticles can be further controlled, and organic microparticles having a wide variety of properties can be easily produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 It is a diagram showing an example of a processing step according to an embodiment of the present invention.
[0054] Figure 2 (A) is a schematic cross-sectional view of a forced thin-film type microreactor according to an embodiment of the present invention, and (B) is a schematic cross-sectional view of a forced thin-film type microreactor according to another embodiment of the present invention.
[0055] Figure 3 for Figure 2(A) and (B) are schematic plan views of the first processing surface of the forced thin-film type microreactor.
[0056] Figure 4 This is a TEM photograph of indomethacin microparticles obtained in step c of Example A1 of the present invention.
[0057] Figure 5 These are the results of X-ray diffraction measurements of the indomethacin microparticles obtained in Example A1, Step c, and Step 2 of the present invention.
[0058] Figure 6 This is a TEM photograph of indomethacin microparticles obtained in step 2 of Example A1 of the present invention.
[0059] Figure 7 This is a TEM photograph of indomethacin microparticles obtained in step 2 of Example A2 of the present invention.
[0060] Figure 8 This is a TEM photograph of indomethacin microparticles obtained in step 2 of Comparative Example A1 of the present invention.
[0061] Fig. 9 These are the X-ray diffraction measurement results of the indomethacin microparticles obtained in Example A3, Step c, and Step 2 of the present invention.
[0062] Fig.10 This is a TEM photograph of indomethacin microparticles obtained in step 2 of Example A3 of the present invention.
[0063] Fig.11 This is a TEM photograph of indomethacin microparticles obtained in step 2 of Comparative Example A2 of the present invention.
[0064] Fig.12 This is a TEM photograph of indomethacin microparticles obtained in step c of Example A4 of the present invention.
[0065] Fig.13 These are the X-ray diffraction measurement results of the indomethacin microparticles obtained in Example A4, Step c, and Step 2 of the present invention.
[0066] Fig.14 This is a TEM photograph of indomethacin microparticles obtained in step 2 of Example A4 of the present invention.
[0067] Fig.15 This is a TEM photograph of indomethacin microparticles obtained in step 2 of Comparative Example A3 of the present invention.
[0068] Fig.16 This is a TEM photograph of the curcumin microparticles obtained in step c of Example A5 of the present invention.
[0069] Fig.17 These are the X-ray diffraction measurement results of the curcumin microparticles obtained in step c and step 2 of Examples A5 and A6 of the present invention.
[0070] Fig.18 This is a TEM photograph of the curcumin microparticles obtained in step 2 of Example A5 of the present invention.
[0071] Fig.19 This is a TEM photograph of the curcumin microparticles obtained in step 2 of Comparative Example A4 of the present invention.
[0072] Fig. 20 This is a TEM photograph of the curcumin microparticles obtained in step 2 of Example A6 of the present invention.
[0073] Fig.21 This is a TEM photograph of the curcumin microparticles obtained in step 2 of Comparative Example A5 of the present invention.
[0074] Fig. 22 This is a SEM photograph of the polypropylene microparticles obtained in step c of Example A7 of the present invention.
[0075] Fig.23 These are the results of X-ray diffraction measurements of the polypropylene microparticles obtained in Example A7, Step c, and Step 2 of the present invention.
[0076] Fig.24 This is a SEM photograph of the polypropylene microparticles obtained in step 2 of Example A7 of the present invention.
[0077] Fig.25 This is a SEM photograph of the polypropylene microparticles obtained in step 2 of Comparative Example A6 of the present invention.
[0078] Fig.26 This is a TEM photograph of the pirenoxine microparticles obtained in step 1 of Example A8 of the present invention.
[0079] Fig. 27 This is a TEM photograph of the pirenoxine microparticles obtained in step 2 of Example A8 of the present invention.
[0080] Fig.28 These are the results of X-ray diffraction measurements of the pirenoxine microparticles obtained in Example A8, step 1 (before treatment in step 2), and step 2 of the present invention.
[0081] Fig.29 This is a transmission electron microscope (TEM) observation photograph of the red pigment nanoparticles of the present invention produced in step 1 of experiment number 1-1 of Example B.
[0082] Fig.30This is a transmission electron microscope (TEM) observation photograph of the red pigment nanoparticles of the present invention produced in step 2 of Experiment No. 1-2 of Example B.
[0083] Fig.31 This is a transmission electron microscope (TEM) observation photograph of the red pigment nanoparticles of the present invention produced in step 2 of experiment number 1-1 of Example B.
[0084] Fig.32 This is a transmission electron microscope (TEM) observation photograph of the cyan organic pigment fine particles of the present invention obtained after step 1 (cleaning) of Experiment No. 1-7 of Example C.
[0085] Fig.33 This is a transmission electron microscope (TEM) observation photograph of the cyan organic pigment fine particles of the present invention obtained after step 1 (cleaning) of Experiment No. 1-7 of Example C.
[0086] Fig.34 This is a transmission electron microscope (TEM) observation photograph of the cyan organic pigment fine particles of the present invention obtained after step 2 (action) of Experiment No. 1-7 of Example C.
[0087] Fig.35 This is a transmission electron microscope (TEM) observation photograph of the cyan organic pigment fine particles of the present invention obtained after step 2 (action) of Experiment No. 1-7 of Example C.
[0088] Fig.36 This is a transmission electron microscope (TEM) observation photograph of the cyan organic pigment particles produced in Experiment No. 4-4 of Example C.
[0089] Fig.37 This is a transmission electron microscope (TEM) observation photograph of the cyan organic pigment particles produced in Experiment No. 3-1 of Example C. DETAILED DESCRIPTION
[0090] The embodiments of the present invention are described in detail below. However, the embodiments of the present invention are not limited to the embodiments described below.
[0091] In the present invention, organic matter is a carbon-containing compound, mainly composed of carbon and oxygen, and may be an artificially synthesized organic matter or an organic matter extracted from natural matter, and is not particularly limited. Examples thereof include pharmaceutical compositions, foods, food additives, health foods and other biological ingestions, synthetic resins, synthetic fibers, rubber and other polymer compounds, pigment compounds including dyes, pigments, coatings and the like, fragrances, pesticides and the like. In addition, in the present invention, organic microparticles are microparticles of the above-mentioned organic matter.
[0092] The so-called biological ingestible is not particularly limited as long as it is intended for ingestion by the organism, and examples thereof include substances that are absorbed in the organism and intended to exhibit effects in the organism, such as drugs in pharmaceuticals; substances that pass through the body and are then excreted; substances used to transport drug components in drug delivery systems; or substances that are applied to the skin of the organism, such as cosmetics, and intermediates between foods and the above substances. Specifically, it refers to organic substances used in medicines, quasi-drugs, cosmetics, foods, food additives, health foods, etc. As the biological ingestible of the present invention, commercially available products can be used, and newly synthesized products can also be used.
[0093] Specific examples of the above-mentioned biological ingestion substances include analgesics, anti-inflammatory drugs, anthelmintics, antiarrhythmic drugs, antibiotics, anticoagulants, antihypertensive drugs, antidiabetic drugs, antiepileptic drugs, antihistamines, anti-malignant tumor drugs, appetite suppressants, anti-obesity drugs, antimuscarinics, antimycobacterial drugs, anti-neoplastic drugs, immunosuppressants, antithyroid drugs, antibacterial drugs, antiviral drugs, anxiety-relieving drugs, astringents, adrenergic beta-blockers, blood products, plasma substitutes, myocardial inotropes, contrast media, corticosteroids, cough suppressants, diagnostic drugs, diagnostic imaging drugs, diuretics, dopamine-acting drugs, hemostatic drugs, immunosuppressants, lipid-regulating drugs, muscle relaxants, parasympathetic nerve stimulants, parathyroid calcitonin, bisphosphonates, prostaglandins, radiopharmaceuticals, sexual Hormones, antiallergic drugs, stimulants, anorexigenic substances, sympathetic stimulants, thyroid drugs, vasodilators and xanthines, cataract therapeutic agents, adrenocortical hormone agents, allergic rhinitis therapeutic drugs and other pharmaceutical compositions, nutritional and pharmacological substances, food supplements, vitamins, minerals, food nutritional supplements such as herbs, folic acid, fatty acids, fruit and vegetable extracts, vitamin supplements, mineral supplements, phosphatidylserine, lipoic acid, melatonin, glucosamine / chondroitin, aloe, glucur, glutamine, amino acids, green tea, lycopene and other foods or food additives, herbs, phytonutrients, antioxidants, flavonoid components of fruits, and collagen, hyaluronic acid, amino acids, vitamin C derivatives, hydroquinones and other beauty supplements, but are not limited thereto. As preferred properties, biological ingestibles that can be orally administered with low solubility in water and biological ingestibles that can be used as injections can be listed.
[0094] Examples of the drug include danazol, tacrolimus hydrate, progesterone, indomethacin, curcumin, tranilast, benzbromarone, naproxen, phenytoin, carotene, perthiazide, piposulfan, camptothecin, paracetamol, acetylsalicylic acid, amiodarone, cholinesterol, choridene, sodium cromoglycate, salbutamol, sucralfate, sulfasalazine, minoxidil, temazepam, alprazolam, propoxyphene, and kinone. Fen, erythromycin, cyclosporine, acyclovir, ganciclovir, etoposide, melphalan, methotrexate, mitoxantrone, daunorubicin, doxorubicin, megestrol acetate, tamoxifen, medroxyprogesterone, nystatin, terbutaline, amphotericin B, aspirin, ibuprofen, diclofenac, ketoprofen, flurbiprofen, diflunisal, diosgenin, cilostazol, toluidine, peptide, sodium cromoglycate, pirenoxine, etc.
[0095] Examples of quasi-drugs include toothbrushes, cosmeceuticals, hair growth enhancers, mouth fresheners, and oral halitosis preventives.
[0096] Examples of the cosmetics include basic cosmetics such as lotions, emulsions, and serums, sunscreen cosmetics, makeup cosmetics, hair cosmetics, cleansing cosmetics, lip cosmetics, oral cosmetics, nail cosmetics, eyeliner cosmetics, and shower cosmetics.
[0097] Examples of the food or food additive include vitamins such as vitamin A, B, C, and E and their derivatives, amino acids, carotenoids, and fruit and plant extracts.
[0098] Examples of health foods include coenzyme Q10, vitamins such as vitamins A, B, C, and E, and derivatives thereof, etc. These may be used alone or in combination of two or more.
[0099] In the present invention, there is no particular limitation on the resin, and the resin includes thermoplastic resins [condensation-type thermoplastic resins such as polyester resins, polyamide resins, polyurethane resins, poly(sulfide)ether resins, polycarbonate resins, polysulfone resins, polyimide resins, etc., vinyl polymerization-type thermoplastic resins such as polyolefin resins, (meth)acrylic resins, styrene resins, vinyl resins, thermoplastic elastomers, resins from natural materials such as cellulose derivatives, thermoplastic silicone resins, etc.], thermosetting resins [e.g., epoxy resins, unsaturated polyester resins, diallyl phthalate resins, silicone resins (silicone rubber, silicone varnish)], etc. These resins can be used alone or in combination of two or more. Usually, thermoplastic resins and water-insoluble resins (or hydrophobic resins, water-insoluble thermoplastic resins, etc.) can be preferably used.
[0100] Examples of the polyester resin include various resins using dicarboxylic acid components, glycol components, hydroxycarboxylic acids, and lactones, for example, poly (C2-6) alkylene-aryl ester resins such as polyethylene terephthalate, poly (1,3-trimethylene terephthalate), poly (1,2-trimethylene terephthalate), poly (butylene terephthalate), poly (1,4-cyclohexanedimethanol terephthalate), polyethylene naphthalate, and poly (butylene naphthalate), and copolyesters containing C2-6 alkylene-aryl ester units as main components (e.g., 50% by weight or more) (e.g., copolymer components are polyoxy C2-4 alkylene glycols having oxyalkylene units, C6-1 2 aliphatic dicarboxylic acids, copolyesters of asymmetric aromatic dicarboxylic acids such as isophthalic acid and phthalic acid), aromatic polyester resins such as polyarylate resins and liquid crystal polyesters, poly-C2-6 alkylene glycol-C2-10 aliphatic dicarboxylates such as poly-C2-6 alkylene-oxalate, poly-C2-6 alkylene-succinate, and poly-C2-6 alkylene-adipate, poly-hydroxycarboxylic acid resins (e.g., polyglycolic acid, polylactic acid, glycolic acid-lactic acid copolymers, etc.), polylactone resins (e.g., poly-C3-12 lactone resins such as polycaprolactone, etc.), and their copolyesters (e.g., polycaprolactone-polybutylene succinate copolymer resins, etc.). The polyester resin may contain a urethane bond. Furthermore, the polyester resin may be biodegradable.
[0101] Examples of the polyamide resin include aliphatic polyamide resins, alicyclic polyamide resins, and aromatic polyamide resins, and aliphatic polyamide resins are generally used. These polyamide resins may be used alone or in combination of two or more. Examples of the aliphatic polyamide-based resins include condensates of an aliphatic diamine component (C4-10 alkylenediamine such as tetramethylenediamine and hexamethylenediamine) and an aliphatic dicarboxylic acid component (C4-20 alkylenedicarboxylic acids such as adipic acid, sebacic acid, and dodecanedioic acid) (e.g., polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 1010, polyamide 1012, polyamide 1212, etc.), homopolymers or copolymers of lactams (C4-20 lactams such as ε-caprolactam and ω-laurolactam), or aminocarboxylic acids (C4-20 aminocarboxylic acids such as ω-aminoundecanoic acid), such as polyamide 6, polyamide 11, polyamide 12, polyamide 6 / 11, polyamide 6 / 12, etc.), and copolyamides obtained by copolymerization of these polyamide components (e.g., polyamide 66 / 11, polyamide 66 / 12, etc.). The dicarboxylic acid component of the polyamide resin may contain a dimer acid unit. Furthermore, the polyamide resin may have biodegradability.
[0102] Ether resins, particularly poly(thio)ether resins, include, for example, polyoxyalkylene resins (stabilized polyoxymethylene glycol or homo- or copolymeric acetal resins, polyoxypropylene glycol, polyoxytetramethylene glycol, polyoxyethylene-polyoxypropylene block copolymers and other polyoxy C2-4 olefin glycols), polyphenylene ether resins, polyphenylene ether ketone resins, polythioether resins (polythioether resins such as polyphenylene sulfide or its copolymers), polyetherketone resins (including polyetheretherketone resins), and the like.
[0103] Among the polyolefin resins, homopolymers or copolymers of α-C2-6 olefins, for example, homopolymers or copolymers of olefins such as polyethylene, polypropylene, ethylene-propylene copolymers, polymethylpentene-1, and copolymers of olefins and copolymerizable monomers [ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylate copolymers, etc.] can be cited. These polyolefin resins can be used alone or in combination of two or more.
[0104] Among vinyl resins, examples of halogen-containing vinyl resins containing halogen include polyvinyl chloride resins, vinyl chloride-vinyl acetate copolymers, vinylidene chloride resins, and fluororesins.
[0105] In addition, as other vinyl resins or their derivatives, for example, homopolymers or copolymers of vinyl carboxylate (polyvinyl acetate, ethylene-vinyl acetate copolymer, etc.), saponified products thereof (vinyl alcohol resins such as polyvinyl alcohol and ethylene-vinyl alcohol copolymer), derivatives derived from saponified products (vinyl alcohol resins) (for example, polyvinyl formal, polyvinyl butyral, etc. polyvinyl acetal resins, etc.), etc. In ethylene-vinyl alcohol copolymers, the ethylene content can be about 5 to 40% by weight.
[0106] The present invention can be applied to various pigments that can be provided and produced as organic pigments.
[0107] For example, as the red pigment of the present invention, a commercially available product may be used, or a newly synthesized product may be used. As an example, a part of the pigments classified as CI Pigment Red, CI Pigment Violet, and CI Pigment Orange in the color index may be cited. More specifically, quinacridone pigments such as CI Pigment Red 122 and CI Pigment Violet 19, diketopyrrolopyrrole pigments such as CI Pigment Red 254 and CI Pigment Orange 73, naphthol pigments such as CI Pigment Red 150 and CI Pigment Red 170, perylene pigments such as CI Pigment Red 123, and azo pigments such as CI Pigment Red 144 may be cited.
[0108] Furthermore, the present invention is also applicable to cyan organic pigments, which include cyan organic pigments such as cyan, navy blue, and cyan.
[0109] As the cyan organic pigment of the present invention, commercially available products can be used, or newly synthesized products can be used. As an example, pigments classified as CI pigment blue in the color index can be listed. More specifically, CI pigment blue-1, CI pigment blue-2, CI pigment blue-3, CI pigment blue-15, CI pigment blue-15:2, CI pigment blue-15:3, CI pigment blue-15:4, CI pigment blue-16, CI pigment blue-22, CI pigment blue-60, CI pigment blue-75, etc. can be listed. These can be used alone, or two or more can be mixed and used.
[0110] As the organic pigment of the present invention, composite phthalocyanine fine particles can also be used. Various composite phthalocyanine fine particles have been provided and commercially available so far, and these can also be used, or newly synthesized.
[0111] In particular, the applicant of the present application has developed composite phthalocyanine particles such as copper-oxytitanium phthalocyanine particles, copper-cobalt phthalocyanine particles, and copper-oxytitanium-cobalt phthalocyanine particles at the nano level, preferably below 100 nm, which can inhibit crystal growth, meet the required properties, and are most suitable as colorants such as pigments. The composite phthalocyanine particles obtained by the manufacturing method can also be used.
[0112] The novel composite phthalocyanine microparticles are described. The method for producing the composite phthalocyanine microparticles is characterized in that it includes: step 0 of preparing a solution by dissolving at least copper phthalocyanine and oxytitanium phthalocyanine and / or cobalt phthalocyanine as raw materials in a first solvent; step 1 of mixing the solution obtained in the above step 0 with a second solvent that is a poor solvent for the above raw materials to precipitate the composite phthalocyanine; and step 2 of allowing an organic solvent to act on the composite phthalocyanine obtained in the above step 1.
[0113] The organic solvent is preferably an aromatic compound solvent or a heterocyclic compound solvent, for example, the organic solvent is preferably at least one selected from styrene, xylene, toluene, benzene, cresol, cumene, and tetrahydrofuran. By using an aromatic compound solvent or an alicyclic compound solvent that generally induces and promotes a crystal transformation to a more stable β-type crystal structure, surprisingly, it is possible to suppress the crystal transformation of α-type copper phthalocyanine to a more stable β-type crystal structure, and also to suppress the growth of crystals.
[0114] The step 0 may be implemented with a mixing weight ratio of the raw materials (copper phthalocyanine / oxytitanium phthalocyanine and / or copper phthalocyanine / cobalt phthalocyanine) of 1 or more and less than 20. In the step 0, oxytitanium phthalocyanine and cobalt phthalocyanine may be dissolved simultaneously or sequentially.
[0115] The above step 1 can be performed similarly to the above step 1 of the present invention by using a microreactor for reacting at least two types of fluids to be processed.
[0116] Alternatively, the composite phthalocyanine obtained in step 1 may be implemented in the same crystal form as the composite phthalocyanine obtained in step 2. That is, in step 2, even when an organic solvent is allowed to act on the composite phthalocyanine obtained in step 1, no crystal transformation occurs. Alternatively, a surfactant or a dispersant is added to the organic solvent.
[0117] It is appropriate that the aspect ratio of the above-mentioned composite phthalocyanine particles is greater than 1.1 and less than 2.5, and the particle size is greater than 5nm and less than 100nm. The above-mentioned aspect ratio refers to the ratio of the long side to the short side in each composite phthalocyanine particle such as copper-oxytitanium phthalocyanine particles. For example, when its shape can be captured as a rectangular parallelepiped or a rectangular parallelepiped-like body, it refers to the ratio of the longest side to the shortest side among the three sides. Alternatively, when its shape can be captured as a sphere or a roughly spherical shape, it refers to the ratio of its longest diameter to its shortest diameter. In addition, for example, the above-mentioned aspect ratio refers to the value obtained by observing by a transmission electron microscope (TEM) and measuring the long diameter and short diameter of 100 particles The average value of the result.
[0118] The method can be implemented as a scheme in which the relative value ([Abs(a)] / [Abs(b)]) of the peak Abs(a) at 655 to 700 nm and the peak Abs(b) at 550 to 640 nm of the absorption spectrum in the ultraviolet-visible region of the composite phthalocyanine microparticles is 0.8 or more. The Abs refers to the absorbance (Abspbance) calculated in the ultraviolet-visible absorption spectrum measurement based on the Lambert-Beer law, and the peak Abs refers to the maximum value among the Abs values within a specific wavelength range.
[0119] In this work, the surface active agents, active agents, and other products listed below are various types of commercial products and new synthetic products. Specific limitations, specific examples, different types of surface active agents, non-restrictive surface active agents, non-restrictive surface active agents, combinations of various types of surface active agents, etc. For root use, limited surface activity for use during certain periods of time. For example, biological toxicity must be considered when collecting biological organisms. Also, but not limited to, the following 12-carbon base carbonyl compounds are listed: Neogen RK (Daiichi Kogyo Pharmaceuticals), Solsperse 20000, Solsperse 24000, Solsperse 26000, Solsperse 27000, Solsperse 28000, Solsperse 41090 (all manufactured by Avecia), BYK108, Disperbyk BYK160, Disperbyk BYK161, Disperbyk BYK162, Disperbyk BYK163, Disperbyk BYK166, Disperbyk B YK170, Disperbyk BYK180, Disperbyk BYK181, Disperbyk BYK182, Disperbyk BYK183, Disperbyk BYK184, Disperbyk BYK190, Disperbyk BYK191, Disperbyk BYK192, Disperbyk BYK2000, Disperbyk BYK2001, Disperbyk BYK2163, Disperbyk BYK2164 (all manufactured by BIK Chemical Company), Aggregate 100, Aggregate 120, 150, 400, 401, 402, 403, 450, 451, 452, 453, EFKA-46, EFKA-47, EFKA-48, EFKA-49, EFKA-1 501, EFKA-1502, EFKA-4540, EFKA-4550 (manufactured by EFKA Chemical Co., Ltd.), Kaosera 2000, Perex TG, Perex TR (manufactured by Kao Corporation), Floren DOPA-158, Flow Len DOPA-22, Floren DOPA-17, Floren G-700, Floren TG-720W, Floren-730W, Floren-740W, Floren-745W (all manufactured by Kyoryosha Chemical Co., Ltd.), Ajisper PA111, Ajisper PB711, Ajisper PB811, Ajisper PB821, Ajisper PW911 (all manufactured by Ajinomoto Co., Ltd.), Johncryl 678, Johncryl 679, Johncryl 62 (all manufactured by Johnson & Johnson Compounds Co., Ltd.),Cellulose such as hydroxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, hydroxypropylmethylcellulose, carboxymethylcellulose, sodium carboxymethylcellulose, methylcellulose, ethylcellulose, etc., polymers such as polyvinyl alcohol, polyvinyl pyrrolidone, lecithin, cholesterol, etc., phospholipids, sulfonium compounds, plant resins such as gum arabic and gum gadis, gelatin, casein, phospholipids, dextran, glycerin, tragacanth gum, stearic acid, benzalkonium chloride, calcium stearate, glyceryl monostearate, cetearyl alcohol, cetostearyl emulsifying wax, Sp an80, Span60, Span20 and other sorbitan esters, polyoxyethylene alkyl ethers, polyoxyethylene castor oil derivatives, Tween80, Tween60, Tween40, Tween20 and other polyoxyethylene sorbitan fatty acid esters, polyethylene glycol, dodecyltrimethylammonium bromide, polyoxyethylene stearate, colloidal silicon dioxide, phosphate esters, sodium lauryl sulfate, 4-(1,1,3,3-tetramethylbutyl)-phenol polymers of ethylene oxide and formaldehyde, Lutrol F127, Lutrol F108, Futrol F87, Futrol F68 and other Poloxamer, Poloxamine, charged phospholipids, dioctyl sulfosuccinate, dialkyl esters of sodium sulfosuccinate, sodium dodecyl sulfate, alkyl aryl polyether sulfonate, mixture of sucrose stearate and sucrose distearate, p-isononylphenoxy polyglycidol, decanoyl-N-methylglucamide, n-decyl β-D-pyranoglucoside, n-decyl β-D-maltopyranoside, n-dodecyl β -D-glucopyranoside, n-dodecyl β-D-maltoside, heptanoyl-N-methyl gluconamide, n-heptyl β-D-glucopyranoside, n-heptyl β-D-thioglucoside, n-hexyl β-D-glucopyranoside, nonanoyl-N-methyl gluconamide, n-nonyl β-D-glucopyranoside, octanoyl-N-methyl gluconamide, n-octyl-β-D-glucopyranoside, octyl β-D-thioglucopyranoside , lysozyme, PEG-phospholipids, PEG-cholesterol, PEG-cholesterol derivatives, PEG-vitamin A, and random copolymers of vinyl acetate and vinyl pyrrolidone, quaternary ammonium compounds, benzyl-di(2-chloroethyl)ethylammonium bromide, coconut trimethylammonium chloride, coconut trimethylammonium bromide, coconut methyl dihydroxyethylammonium chloride, coconut methyl dihydroxyethylammonium bromide, decyl triethylammonium chloride, decyl dimethyl hydroxyethylammonium chloride, decyl dimethyl hydroxyethylammonium chloride bromide, C12-15 dimethyl hydroxyethylammonium chloride, C12-15 dimethyl hydroxyethylammonium chloride bromide, coconut dimethyl hydroxyethylammonium chloride, coconut dimethyl hydroxyethylammonium bromide, myristyl trimethylammonium methyl sulfate, lauryl dimethyl benzyl ammonium chloride, lauryl dimethyl benzyl ammonium bromide, lauryl dimethyl (vinyloxy) 4 ammonium chloride, lauryl dimethyl (vinyloxy) 4 ammonium bromide,N-Alkyl (C12-18) dimethyl benzyl ammonium chloride, N-alkyl (C14-18) dimethyl-benzyl ammonium chloride, N-tetradecyl methyl benzyl ammonium chloride monohydrate, dimethyl didecyl ammonium chloride, N-alkyl and (C12-14) dimethyl 1-naphthyl methyl ammonium chloride, trimethyl ammonium halide, alkyl-trimethyl ammonium salt, dialkyl-dimethyl ammonium salt, lauryl trimethyl ammonium chloride, ethoxylated alkyl amido alkyl dialkyl ammonium salt, ethoxylated trialkyl ammonium salt, dialkyl benzene dialkyl ammonium chloride, N-didecyl dimethyl ammonium chloride, N-tetradecyl dimethyl benzyl ammonium, chloride monohydrate, N-alkyl (C12-14) dimethyl 1-naphthyl methyl ammonium chloride, dodecyl dimethyl benzyl ammonium chloride, dialkyl benzene alkyl ammonium chloride, lauryl trimethyl ammonium chloride, alkyl benzyl methyl ammonium chloride, alkyl benzyl dimethyl ammonium bromide, C12 trimethyl bromide ammonium chloride, C15 trimethylammonium bromide, C17 trimethylammonium bromide, dodecylbenzyltriethylammonium chloride, poly-diallyldimethylammonium chloride (DADMAC), dimethylammonium chloride, alkyldimethylammonium halide, tricetylmethylammonium chloride, decyltrimethylammonium bromide, dodecyltriethylammonium bromide, tetradecyltrimethylammonium bromide, methyltrioctylammonium chloride, POLYQUAT10TM, tetrabutylammonium bromide, benzyltrimethylammonium bromide, choline ester, stearyldimethylbenzyl ammonium chloride compound, cetylpyridinium bromide, cetylpyridinium chloride, halide salt of quaternized polyoxyethyl alkylamine, MIRAPOLTM, ALKAQUATTM, alkylpyridinium salt, amine, amine salt, amine oxide, imidoazolinium salt, protonated quaternized acrylamide, methylated quaternized polymer, etc. These may be used alone or in combination of two or more. ,
[0120] Be not limited to this, for example, when the organic microparticles are low molecular weight organic substances such as indomethacin, curcumin, pyrenoxine shown in Example A, preferably use the macromolecular surfactants such as water-soluble nitrogen-containing vinyl polymers, nonionic cellulose derivatives. More specifically, hydroxypropyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, methylcellulose, polyvinyl alcohol, polyvinyl pyrrolidone, etc. can be listed. In addition, from the viewpoint of dispersibility, the nonionic surfactants such as Tween80, polyoxyethylene cured castor oil, etc. sometimes have an effect, and are also preferably used in conjunction with macromolecular surfactants. When the organic microparticles are the organic substances of the pigment shown in Example B and C, preferably use the macromolecular surfactants such as acrylic acid polymers, macromolecular block copolymers, surfactants such as carboxylic acid esters containing hydroxyl, dialkyl sodium sulfosuccinates, sodium dodecylbenzene sulfonates, etc. anionic surfactants, etc.
[0121] In addition, in the organic particles of the present invention, block copolymers as high molecular surfactants can also be used. In this case, as block copolymers, acrylic acid, methacrylic acid block copolymers, polystyrene and other addition polymerization or condensation polymerization block copolymers, block copolymers with polyoxyethylene, polyoxyalkylene blocks, etc. can be listed. In addition, previously known block copolymers can also be used, but the block copolymer used in the present invention is preferably amphiphilic. As a specific preferred form, a diblock copolymer consisting of a hydrophobic segment and a hydrophilic segment with an organic acid or its ionic salt unit can be listed. In addition, a triblock copolymer having a hydrophobic segment and a hydrophilic segment with an organic acid or its ionic salt unit and another segment is preferably used. In the case of three blocks, it is preferably adopted as a hydrophobic segment, a nonionic hydrophilic segment, a hydrophilic segment with an organic acid or its ionic salt unit, which is also preferred in the sense of stabilization of the inner package state. For example, if the above-mentioned triblock copolymer is used to prepare a dispersion using an organic substance such as a pigment and water as a solvent, the organic substance such as the pigment can be encapsulated in the micelle formed by the triblock copolymer. In addition, the particle size of the particles of the dispersion composition can be made very uniform. Furthermore, the dispersion state can be made extremely stable.
[0122] As solvent of the present invention, in order to dissolve the raw material of organic particles, in order to precipitate organic particles from the raw material solution of organic particles, and then in order to control the properties of organic particles by adding the surfactant described below, various solvents can be used. As an example of these solvents, water (distilled water, pure water, etc.), organic solvents (alcohol solvents, ketone solvents, ether solvents, aromatic solvents, aliphatic hydrocarbon solvents, nitrile solvents, sulfoxide solvents, halogen solvents, ester solvents, amine solvents, ionic solutions) can be listed. With regard to these solvents, one or more mixed solvents can be selected according to the purpose to implement. In addition, as required, acidic substances and alkaline substances can also be added to various solvents to adjust pH.
[0123] The above-mentioned solvents are further described in detail. As alcohol solvents, for example, methanol, ethanol, isopropanol, n-propanol, 1-methoxy-2-propanol (PGME) and the like can be listed, and further, straight-chain alcohols such as n-butanol, branched alcohols such as 2-butanol and tert-butanol, polyols such as ethylene glycol and diethylene glycol and the like can be listed. As ketone solvents, for example, acetone, methyl ethyl ketone, cyclohexanone and the like can be listed. As ether solvents, for example, dimethyl ether, diethyl ether, tetrahydrofuran and the like can be listed. As aromatic solvents, for example, styrene, toluene, xylene, phenol, nitrobenzene, chlorobenzene, dichlorobenzene, tetrahydrofuran, pyridine and the like can be listed. As aliphatic solvents, for example, pentane, hexane, heptane, octane, cyclohexane and the like can be listed. As nitrile solvents, for example, acetonitrile and the like can be listed. As sulfoxide solvents, for example, dimethyl sulfoxide, diethyl sulfoxide, hexamethylene sulfoxide, cyclopentane and the like can be listed. As halogen solvents, for example, chloroform, dichloromethane, trichloroethylene, iodoform, etc. can be listed. As ester solvents, for example, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, propylene glycol monomethyl ether acetate (PGMEA), etc. can be listed. As ionic liquids, for example, benzyltrimethylammonium hydroxide (BTMA), 1-butyl-3-methylimidazolium and PF6- (hexafluorophosphate ion) salts can be listed. As amine solvents, for example, dimethylaminoethanol, ethylenediamine, methylamine, dimethylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, etc. can be listed. As amide solvents, for example, N,N-dimethylformamide, N,N-dimethylacetamide, etc. can be listed.
[0124] The "solvent having partial solubility for organic particles" in the present invention means that during the period from the reaction with the organic particles to the end of the treatment, the solvent does not show strong solubility to completely dissolve all of the organic particles, but shows solubility to the extent that the properties of the particles are "changed". Hereinafter, it is also referred to as "solvent having partial solubility". There is no particular limitation on the "change", but examples thereof include a phenomenon in which a part of the organic particles grows and becomes coarser when the solvent acts on the organic particles, a phenomenon in which necking occurs between the organic particles, and the like.
[0125] As an example of the solubility of the organic particles in the solvent having partial solubility, when measured using organic particles having an average particle size of 1000 nm, it is preferably 1 μg / g or more and 1000 μg / g or less (1 ppm or more and 1000 ppm or less), and more preferably 1 μg / g or more and 500 μg / g or less (1 ppm or more and 500 ppm or less). Even if the organic particles are not completely dissolved, if the solubility of the organic particles in the solvent is too high, the growth of the particles and the degree of coarsening of the particles become excessive, so that the application in the present invention is difficult.
[0126] It should be noted that when measuring the solubility, the above solvent is allowed to act on organic particles with an average particle size of 1000 nm, and then filtered through a filter with an opening diameter of about 0.1 to 0.2 μm, and the filtrate is subjected to UV-Vis measurement (visible ultraviolet spectrometry) to calculate the concentration of the organic matter dissolved in the solvent. When calculating the concentration, the above filtrate can be measured by other detection methods such as fluorescence and refractive index.
[0127] In addition, as an example of a combination of organic particles and a solvent having a partial solubility, when the organic particles are indomethacin, curcumin, or pyrenoxine, it is preferred to use straight-chain alkanes such as pentane, hexane, heptane, octane, nonane, decane, and undecane, cyclic alkanes such as cyclohexane, or water as the above-mentioned solvent. In addition, as an example, when the organic particles are polypropylene, it is preferred to use alcoholic solvents such as methanol and isopropanol, and aromatic solvents such as toluene and xylene as the above-mentioned solvent.
[0128] As an example, the results of Comparative Example A of the present invention were confirmed. Figure 8 , Fig.11 The particles seen in the figure grow in the solvent and shrink. In such a state, even if a dispersion treatment is performed later, the particles cannot be dispersed, and it is very difficult to exert the properties obtained by the micronization of organic matter (for example, physical property changes such as improved solubility, changes in optical properties such as improved transparency, chemical property changes such as new reactions, etc.).
[0129] As another example, the TEM observation results of the PR254 fine particles, a red pigment produced in Experiment No. 1-1 of Example B of the present invention, when put into propylene glycol monomethyl ether acetate (PGMEA) are shown in FIG. Fig.31 In addition, the TEM observation results before injection are shown in Fig.29 (dispersed in a surfactant aqueous solution). Fig.29 Compared to the PR254 nanoparticles seen in Fig.31 The PR254 nanoparticles are growing in PGMEA and are shrinking. In this state, even if a dispersion treatment is performed later, the nanoparticles cannot be dispersed, and it is very difficult to bring out the characteristics of the fine red pigment.
[0130] Furthermore, as another example, it was confirmed that Experiment No. 4-4 ( Fig.36 ) or as the copper-titanium-cobalt phthalocyanine particles of the cyan pigment prepared in Experiment No. 3-1 ( Fig.37) grows in the solvent and also shrinks. In such a state, even if a dispersion treatment is performed later, the particles cannot be dispersed, and it is very difficult to exert the characteristics of the cyan organic pigment particles.
[0131] In the present invention, it is important that at least a part of the organic particles before the particle property control solution is applied contain amorphous materials, and a solvent having partial solubility for the organic particles is selected, and the surfactant is added to the organic particles to mix, dissolve, and disperse the molecules, and the prepared particle property control solution is applied to the organic particles. This makes it possible to control the particle size, crystal form, crystallinity, and other properties of the organic particles.
[0132] The mechanism that controls the properties of particles is still unclear. The molecular arrangement of the amorphous part of the organic particles in the solid is random, and the molecules are not as close to each other as in the crystalline part, and the molecular bonding force is weaker. Therefore, it is believed that the amorphous part of the organic particles is easily dissolved by the solvent that has partial solubility for the organic particles, and is likely to become the starting point of growth and necking.
[0133] When organic particles are partially dissolved in the solvent due to the influence of the solvent and the influence of heat, although necking and particle growth are likely to occur, when stored under such conditions, an increase in crystallinity and a crystal transformation sometimes occur at the same time. However, at this time, the primary particle size of the organic particles changes by tens to hundreds of times, and as a result, the coarsened organic particles lose the expected characteristics as organic particles. One of the functions of the surfactant in the present invention is to inhibit and control the growth of the above-mentioned organic particles. The above-mentioned surfactant can inhibit the above-mentioned organic particles (especially the amorphous part thereof) from being dissolved by the above-mentioned solvent with partial solubility, and inhibit and control the effects of the above-mentioned solvent on the organic particles, such as necking and particle growth. In more detail, if in the presence of a surfactant, it is believed that the amorphous part of the organic particles is not completely dissolved by the solvent with partial solubility, the random molecular arrangement of the amorphous part changes and becomes compacted, thereby increasing the crystallinity and crystal transformation.
[0134] Furthermore, another function of the above-mentioned surfactant is to improve the solubility of the above-mentioned organic particles in the solvent. More specifically, it is to improve the wettability of the entire particle on which the surfactant acts. That is, as far as the surfactant is concerned, different properties can be shown for the organic particles by its type and the type of the above-mentioned solvent in combination. It is also possible to add a surfactant that improves the solubility of the above-mentioned organic particles in the solvent to a solvent that has a partial solubility for the above-mentioned organic particles to prepare a particle property control solution. In addition, the above-mentioned surfactant has a further function of becoming a casting mold when the above-mentioned organic particles undergo a crystal transformation, and more specifically, it can become a casting mold for the particle size of the organic particles.
[0135] It is considered that the present invention controls the growth of organic fine particles by combining the above-mentioned actions, and in particular, densifies amorphous parts to improve crystallinity, thereby controlling the transition of crystal form and crystallinity.
[0136] Thus, in the present invention, the particle properties such as particle size, crystallinity, and crystal form of the organic particles are controlled by allowing the particle property control solution to act on the organic particles. Specifically, the above-mentioned action is to mix and / or stir the organic particles with the particle property control solution, or simply contact or spray them. By changing the type, concentration, treatment temperature, stirring method, etc. of the solvent or surfactant, the properties of the organic particles can be controlled. In addition, the solvent having a partial dissolving ability can also be prepared by containing the following acidic substances, alkaline substances, or neutral substances in the solvent.
[0137] These substances are not particularly limited, and as acidic substances, inorganic acids such as aqua regia, hydrochloric acid, nitric acid, fuming nitric acid, sulfuric acid, fuming sulfuric acid, and the like, and organic acids such as formic acid, citric acid, malic acid, acetic acid, chloroacetic acid, dichloroacetic acid, oxalic acid, trifluoroacetic acid, trichloroacetic acid, and the like can be cited. As alkaline substances, metal oxides such as sodium hydroxide and potassium hydroxide, metal alkoxides such as sodium methoxide and sodium isopropoxide, and amine compounds such as triethylamine, diethylaminoethanol, and diethylamine can be cited. Furthermore, neutral substances cited as examples of salts of the above-mentioned acidic substances and alkaline substances can also be mixed.
[0138] In particular, in the case of organic pigments such as red organic pigments and cyan organic pigments, the method can be implemented even without the pigment derivatives generally used to inhibit crystal growth, so the unique color of the derivatives can be utilized without affecting the color of the organic pigment actually used. However, it does not prevent the method from being implemented by adding such derivatives.
[0139] It should be noted that the concentration of the organic particles to which the solvent having a partial solubility for the organic particles acts is not particularly limited, but is 0.001 to 90.00% by weight, preferably 0.001 to 50.00% by weight, and more preferably 0.01 to 40.00% by weight. In addition, the surfactant is 0.01 to 500% by weight, preferably 0.1 to 300% by weight, and more preferably 1.0 to 100% by weight relative to the organic particles.
[0140] In the present invention, the particle size of the organic fine particles is not particularly limited. The particle size of the organic fine particles before controlling the particle properties of the organic fine particles is preferably 1000 nm or less, more preferably 500 nm or less, and even more preferably 200 nm or less.
[0141] In addition, in the case of organic pigments such as cyan organic pigments, it is particularly preferred that the primary particle size is below 500nm, preferably below 100nm, more preferably below 30nm. The shape of the above-mentioned particles or microparticles is not particularly limited, for example, it can be granules or their aggregates in the form of roughly cylindrical, roughly spherical, roughly disc-shaped, roughly triangular prism-shaped, roughly quadrangular prism-shaped, roughly polyhedral, ellipsoidal, etc.
[0142] The particle sizes before and after the action of the present invention refer to the particle sizes before and after the above-mentioned mixing and / or stirring, or simply contacting, spraying, etc. of the above-mentioned organic fine particles and the above-mentioned particle property control solution.
[0143] In the present invention, the range in which the particle size of the organic particles is substantially unchanged means that the particle size change rate of the organic particles before and after the organic particles are acted upon by a solvent having a partial solubility for the organic particles to which a surfactant is added (after surfactant treatment (A) / before surfactant treatment (B)) is 1 to 4.
[0144] In addition, the present invention includes a step 1: mixing at least one organic particle precipitation solvent L for precipitating organic particles from a raw material solution of organic particles with a raw material solution of organic particles that dissolves or molecularly disperses the raw material of organic particles, so as to precipitate organic particles (P1). The raw material of organic particles can be the above-mentioned organic matter, or it can be newly synthesized. The above-mentioned method of mixing can be used, for example, as described in Patent Document 5, and a forced thin film type microreactor can be used for mixing, and a known method in organic particles can be appropriately used. The raw material solution of organic particles can be prepared by mixing a good solvent that can dissolve or molecularly disperse the raw material of organic particles with the raw material of organic particles, and the method is implemented by using a solvent with a lower solubility in organic matter than the above-mentioned good solvent as the precipitation solvent L for organic particles. In addition, it can also be implemented by adjusting the pH when mixing the raw material solution of organic particles and the precipitation solvent L for organic particles. It can also be prepared by combining the above-mentioned solvent with an acidic substance or an alkaline substance as needed.
[0145] In addition, the present invention may include a step c of washing and / or replacing the solvent of the organic particles (P1) obtained in the step 1 as required. The step c of washing and / or replacing the solvent can be appropriately applied by a known method. There is no particular limitation, but for the liquid containing the organic particles, the washing and / or solvent replacement of the organic particles can be performed by filtering, centrifuging, ultrafiltration, etc., by selecting a solvent that matches the purpose.
[0146] The present invention is characterized in that the properties of the organic particles (P1) are controlled by a step 2 comprising allowing the organic particles (P1) to act on the particle property control solution. Examples of the control of the properties include the particle size of the organic particles and / or the crystallinity of the organic particles. In addition, examples of the crystallinity of the organic particles include the degree of crystallinity of the organic particles. The control of the properties of the particles mentioned here is not limited to the above content as long as the growth and necking of the particles in the solvent can be suppressed, and is also applicable to the case of the crystal transformation of the organic particles. In addition, by precipitating the particles with low crystallinity in a manner including amorphous particles, the crystal form, degree of crystallinity, etc. in step 2 can be controlled with better accuracy, and thus the present invention becomes more effective.
[0147] In addition, as the action in the above step 2 in the present invention, for example, a mixing step, a contacting step, a spraying step, etc. can be listed. In addition, in the above step 2 in the present invention, the above action can be repeated once or multiple times (for example, 2 times, 3 times, 4 times, etc.).
[0148] In addition, when the above-mentioned step 2 in the present invention includes a stirring process (hereinafter also referred to as a dispersion process using stirring, a dispersion process), the properties of the above-mentioned organic particles can be controlled by stirring energy, and a method of using a known stirring device, stirring means, and appropriately controlling the stirring energy can be listed. It should be noted that the stirring energy is described in detail in Japanese Patent Publication No. 04-114725 of the applicant of the present application.
[0149] The stirring method in the present invention is not particularly limited. It can be a method using a magnetic stirrer and a stirring bar, and can be implemented using various shearing, friction, high-pressure jet, ultrasonic and other agitators, dissolvers, emulsifiers, dispersers, homogenizers, etc. Examples include ウルトラタラックス (manufactured by IKA), ポリトロン (キネマティカManufactured), TK ホモミキサー(Manufactured by プライミクス), Eバラマイルダー(Ebara Manufacturing Co., Ltd. (manufactured by TK Polytechnics), TK Polymer (manufactured by Kobelco Materials), colloid mill (Kobelco Materials Co., Ltd. (manufactured by Nippon Coke Industry Co., Ltd.), Torotron wet micro pulverizer (Mitsui Miike Chemical Co., Ltd. Industrial Machinery Manufacturing Co., Ltd., Japan Machinery Manufacturing Co., Ltd. Continuous emulsifiers such as (manufactured by), クレアミックス (manufactured by エム・テクニック), クレアミックStructural materials・Batch-type or continuous-type devices such as those manufactured by Tokulin Co., Ltd.) and Fukuro Mining Machinery Co., Ltd. In addition, it is sometimes effective to perform a part of the microwave treatment before stirring or after stirring.
[0150] There are two types of particle growth: growth and coarsening caused by agglomeration between particles and dissolution of the particle surface, and the coarsening of particles caused by components dissolved in the dispersion medium. The effect of the surfactant is to protect the particle surface and inhibit growth, but if agglomerates are formed, it is sometimes not able to function effectively. Therefore, a dispersion treatment using stirring becomes effective. In this method, in order to uniformly mix and react the surfactant with the solvent that has a partial solubility for the organic particles, it is preferably stirred. In addition, when the particle property control solution is allowed to act on the organic particles, it is preferably stirred. At this time, by applying stirring energy, the surfactant and the solvent that has a partial solubility for the organic particles can act efficiently on the organic particles. As the above-mentioned step 2, when a stirring treatment is included, the properties (crystallinity, crystal form, particle size) of the organic particles can be controlled by stirring energy.
[0151] As an example, the following Figure 1 The steps of producing organic fine particles by a batch method (steps 0 to 2) will be described.
[0152] (Step 0) A precipitation solvent for organic fine particles (liquid A: corresponding to the precipitation solvent L for organic fine particles) and a raw material solution for organic fine particles (liquid B) are prepared.
[0153] (Step 1) Mixing of Liquid A and Liquid B: Liquid A is stirred using a magnetic stirrer and a stirring bar, and Liquid B is added to precipitate organic particles.
[0154] (Step 2) The slurry, wet cake or dry powder of the organic fine particles precipitated in Step 1 is added to a particle property control solution and stirred.
[0155] It should be noted that the slurry containing organic microparticles precipitated in step 1 can be filtered and then washed with a washing liquid (step c) to produce a wet cake of organic microparticles, or a dry powder of organic microparticles can be produced by drying treatment such as vacuum drying, which is then put into the particle property control solution of step 2 and stirred.
[0156] Next, follow the Figure 1 An example of the production process (processes 0 to 2) of organic microparticles using a microreactor described later will be described.
[0157] (Step 0) A solvent for precipitating organic fine particles (liquid A) and a raw material solution for organic fine particles (liquid B) are prepared.
[0158] (Process 1) Use Figure 2 The microreactor shown in (A) mixes the raw material solution of organic particles (liquid B) with the precipitation solvent of organic particles (liquid A: equivalent to the precipitation solvent L of organic particles) to precipitate the organic particles. It should be noted that, as liquid A and liquid B, in addition to the examples illustrated in the following embodiments, the examples described in patent document 8 and other known examples of mixing and precipitation can also be applied.
[0159] (Step 2) The slurry, wet cake or dry powder of the organic fine particles precipitated in Step 1 is added to a particle property control solution and stirred.
[0160] It should be noted that the slurry containing organic particles precipitated in step 1 can be filtered and then washed with a washing liquid (step c) to produce a wet cake of organic particles or a dry powder of organic particles can be produced by drying treatment such as vacuum drying, which is then added to the particle property control solution of step 2 and stirred.
[0161] It should be noted that as a microreactor, it is possible to use Figure 2 The device shown in is the same as the device described in Patent Documents 4 to 6. The microreactor is described in detail below. Figure 2(A)(B) and Figure 3 R indicates the direction of rotation.
[0162] The microreactor in this embodiment has two opposing first and second processing parts 10 and 20, and the first processing part 10 rotates. The opposing surfaces of the two processing parts 10 and 20 become processing surfaces respectively. It is a forced thin film type microreactor in which the first processing part 10 has the first processing surface 1 and the second processing part 20 has the second processing surface 2.
[0163] The two processing surfaces 1 and 2 are connected to the flow paths d1 and d2 of the processed fluid respectively, forming a part of the flow path of the processed fluid. The interval between the two processing surfaces 1 and 2 is usually adjusted to a small interval of less than 1 mm, for example, about 0.1 μm to 50 μm. As a result, the processed fluid passing between the two processing surfaces 1 and 2 becomes a forced thin film fluid forced by the two processing surfaces 1 and 2.
[0164] Furthermore, the apparatus performs fluid processing for causing the first and second processed fluids to react between the processing surfaces 1 and 2 to precipitate microparticles.
[0165] More specifically, the device comprises: a first support 11 holding the first processing part 10, a second support 21 holding the second processing part 20, a surface pressure imparting mechanism 43, a rotation driving mechanism (not shown), a first introduction part d1, a second introduction part d2, and fluid pressure imparting mechanisms p1 and p2. A compressor or other pumps can be used in the fluid pressure imparting mechanisms p1 and p2.
[0166] In the above embodiment, the first processing part 10 and the second processing part 20 are annular disks. As for the material of the first and second processing parts 10 and 20, in addition to metal, carbon, ceramics, sintered metals, wear-resistant steel, sapphire, and products obtained by hardening metals, lining, coating, plating, etc., can be used. In the above embodiment, the first and second processing surfaces 1 and 2 of the two processing parts 10 and 20 facing each other are mirror-polished, and the arithmetic mean roughness is 0.01 to 1.0 μm.
[0167] In the above-mentioned embodiment, the second support 21 is fixed to the device, and the first support 11 installed in the rotating shaft of the rotation drive mechanism also fixed to the device rotates, and the first processing part 10 supported by the first support 11 rotates relative to the second processing part 20. Of course, the second processing part 20 can also be rotated, and both can be rotated. In addition, in the present invention, the above-mentioned rotation speed can be, for example, 350 to 3600 rpm.
[0168] In the above-mentioned embodiment, the second processing part 20 is moved closer to or further away from the first processing part 10 in the direction of the rotation axis 50, so that the part on the opposite side of the processing surface 2 of the second processing part 20 is accommodated in the accommodating part 41 provided in the second support 21 so as to be retractable. However, the first processing part 10 may be moved closer to or further away from the second processing part 20 in the opposite direction, or the two processing parts 10, 20 may be moved closer to or further away from each other.
[0169] The above-mentioned receiving section 41 is a recessed portion for receiving the position on the opposite side of the processing surface 2 of the second processing usefulness part 20, and is a groove formed into an annular shape. The receiving section 41 has enough gaps for the position on the opposite side of the processing surface 2 of the second processing usefulness part 20 to appear and disappear, and the second processing usefulness part 20 is received.
[0170] The interface pressure imparting mechanism is a mechanism for generating a squeezing force (hereinafter referred to as interface pressure) in the direction in which the first processing surface 1 of the first processing part 10 and the second processing surface 2 of the second processing part 20 approach each other. By balancing the interface pressure and the force generated by the fluid pressure to separate the two processing surfaces 1 and 2, the interval between the two processing surfaces 1 and 2 is maintained at a prescribed small interval, and a thin film fluid with a small film thickness of nm or even μm is generated. In the above-mentioned embodiment, the interface pressure imparting mechanism energizes the second processing part 20 toward the first processing part 10 by utilizing the spring 43 provided on the second bracket 21, thereby imparting the interface pressure. In addition, the first processed fluid pressurized by the fluid pressure imparting mechanism p1 is introduced from the first introduction part d1 into the space inside the two processing parts 10 and 20.
[0171] On the other hand, the second processed fluid pressurized by the fluid pressure imparting mechanism p2 is introduced from the second inlet portion d2 through a passage provided inside the second processing portion 20 and from an opening d20 formed in the second processing surface into the space inside the two processing portions 10, 20.
[0172] At the opening d20, the first processed fluid and the second processed fluid merge and mix. At this time, the mixed processed fluid becomes a thin film fluid forced by the two processing surfaces 1 and 2 that maintain the above-mentioned tiny gap, and moves to the outside of the two annular processing surfaces 1 and 2. Since the first processing part 10 is rotating, the mixed processed fluid does not move linearly from the inside to the outside of the two annular processing surfaces 1 and 2, but the synthetic vector of the movement vector in the radial direction of the annular shape and the movement vector in the circumferential direction acts on the processed fluid, and moves from the inside to the outside in a roughly vortex shape.
[0173] Here, if Figure 3As shown in, a groove-shaped recess 13 extending from the center side of the first processing usefulness part 10 to the outside, i.e. in the radial direction, can be formed on the first processing usefulness face 1 of the first processing usefulness part 10. The planar shape of this recess 13 can be a shape that makes the first processing usefulness face 1 bend or extend in a spiral shape. Although not shown in the figure, it can also be a shape that extends straight in the outer direction, a shape that is bent or curved in an L-shaped shape, a continuous shape, a discontinuous shape, a branched shape. In addition, this recess 13 can also be formed on the second processing usefulness face 2 and implemented, and can also be formed on both the first and second processing usefulness faces 1, 2 and implemented. By forming such a recess 13, a micro pump effect can be obtained, which has the effect of being able to suck the processed fluid between the first and second processing usefulness faces 1, 2.
[0174] Preferably, the base end of the recess 13 reaches the inner periphery of the first processing portion 10. The front end of the recess 13 extends toward the outer peripheral surface of the first processing portion 10, so that the depth gradually decreases from the base end to the front end. A flat surface without the recess 13 is provided between the front end of the recess 13 and the outer peripheral surface of the first processing surface 1.
[0175] The opening d20 is preferably provided at a position facing the flat surface of the first processing surface 1. This allows mixing of a plurality of fluids to be processed and precipitation of fine particles to be performed under laminar flow conditions.
[0176] In addition, the fluid discharged to the outside of both processing members 10 and 20 is collected as a discharge liquid in a beaker b through a container v. In the embodiment of the present invention, as described later, the discharge liquid contains organic fine particles.
[0177] It should be noted that the types of the above-mentioned processed fluids and the number of their flow paths are Figure 2 In the example A of (A), there are 2 openings, but there may be 3 or more. In addition, there are no particular restrictions on the shape, size, and number of the openings for introduction provided in each processing unit, and they may be appropriately changed and implemented. In addition, an opening for introduction may be provided just in front of the first and second processing surfaces 1 and 2 or further on the upstream side.
[0178] In the present invention, as long as the above-mentioned treatment can be performed between the treatment surfaces 1 and 2, the second treated fluid may be introduced from the first introduction portion d1, and the first treated fluid may be introduced from the second introduction portion d2. For example, the first and second indicia of each fluid simply have the meaning of identifying the nth number of a plurality of fluids, and as described above, there may be more than a third fluid.
[0179] In the production process of organic microparticles using a microreactor (processes 0 to 2), the microreactor can be used to continuously perform process 1 and process 2. Specifically, Figure 2As shown in (B), a third introduction part d3 is provided in the microreactor in addition to the first introduction part d1 and the second introduction part d2, and for example, a raw material solution of organic particles as the first fluid is introduced into the microreactor from the first introduction part d1, a precipitation solvent of organic particles as the second fluid is introduced into the microreactor from the second introduction part d2, and a particle property control solution as the third fluid is introduced into the microreactor from the third introduction part d3. In this case, by providing the third introduction part d3 for introducing the particle property control solution on the downstream side of the first introduction part d1 and the second introduction part d2, more specifically, by providing the opening d30 of the third introduction part d3 on the downstream side of the opening d20 of the second introduction part d2, the organic particles precipitated between the processing surfaces 1 and 2 can react with the particle property control solution. The microreactor having the above three openings (d10, d20 and d30) is suitable for the case where the steps 1 and 2 are performed continuously.
[0180] However, when the present invention is implemented, when step 1 is performed in a microreactor and steps after step 1 are performed outside the microreactor, Figure 1 As shown in (A), it is sufficient to have at least two openings (d10, d20), but in the case of organic particles precipitated between the treatment surfaces 1 and 2, or in the case of surface treatment in the above-mentioned thin film fluid, it does not prevent the implementation of process 1 in a microreactor having more than three openings.
[0181] Particularly when using the above-mentioned microreactor, for the organic matter of the present invention, it is easy to manufacture as microparticles, and the size can be set to below 1000nm, preferably below 500nm, before and after processing in a solvent having a part of solubility for the organic microparticles and a surfactant that can be growth-inhibited for the organic microparticles. Furthermore, if it is the above-mentioned microreactor, the control of the crystallinity of the precipitated microparticles is relatively easy, and therefore by precipitating it under a state containing amorphous low crystallinity, the crystal form, crystallinity, etc. in the operation 2 can be controlled more accurately. As a specific example of such a microreactor, ULREA (manufactured by Em Technik) can be cited. However, for the manufacture of the organic microparticles of the present invention, it is not limited to the use of a microreactor.
[0182] Example
[0183] The present invention is further specifically described by way of examples below. However, the present invention is not limited to the following examples. In the following examples, liquid A refers to liquid Figure 2 (A) (B) refers to the first fluid to be processed introduced into the first introduction part d1 of the apparatus shown in FIG. 1 , and liquid B refers to the second fluid to be processed introduced into the apparatus from the second introduction part d2.
[0184] In the present application, the examples are divided into three groups: Example A, Example B, and Example C, and each example is shown together with a comparative example.
[0185] Example A is a combination of an ingestible substance and a resin.
[0186] Example B is a group of red organic pigments.
[0187] Example C is a group of cyan organic pigments.
[0188] It should be noted that, in the main body of the specification, group symbols A, B, and C are described after the examples, but description of the group symbol ABC is omitted in tables and drawings.
[0189] (Group of Example A)
[0190] As an example of the method for producing organic microparticles according to the present invention, indomethacin microparticles are used for illustration in Examples A1 to 4, curcumin microparticles are used for illustration in Examples A5 and 6, polypropylene microparticles are used for illustration in Example A7, and pirenoxine microparticles are used for illustration in Example A8.
[0191] In Example A, a powder X-ray diffractometer (product name: X'PertPRO MPD, manufactured by PANalytical) was used for X-ray diffraction measurement (XRD measurement). The measurement conditions were: measurement range: 10-60°, Cu counter cathode, tube voltage 45 kV, tube current 40 mA, scanning speed 16° / min.
[0192] A transmission electron microscope, JEM-2100 (manufactured by JEOL), was used for TEM observation. As observation conditions, an accelerating voltage was set to 80 kV.
[0193] A scanning electron microscope, JFM-7500F (manufactured by JEOL), was used for SEM observation. The observation condition was an acceleration voltage of 1 kV.
[0194] For particle size evaluation, a photograph at 25,000 times magnification was used in TEM observation or SEM observation, and an average value of 50 particles was used.
[0195] The crystallinity referred to here is the ratio of the crystallized component to the total of the crystallized component and the amorphous material.
[0196] (Example A1: Indomethacin Microparticles)
[0197] <Step 0: Preparation of a solvent for precipitating organic microparticles (Solution A) and a raw material solution for organic microparticles (Solution B)>
[0198] <Preparation of organic microparticle precipitation solvent (Solution A)>
[0199] As a precipitation solvent (Solution A) for organic fine particles, an indomethacin precipitation solvent of a 0.1 mol / L hydrochloric acid aqueous solution was prepared using a magnetic stirrer.
[0200] <Preparation of organic microparticle raw material solution (Solution B)>
[0201] As the organic particle raw material solution (liquid B), a raw material solution of indomethacin having a γ (gamma) crystal form and polyvinyl pyrrolidone (Kollidon 12PF (manufactured by BASF)) was prepared by mixing 0.2 wt% of indomethacin in a 0.35 mol / L sodium bicarbonate aqueous solution. A high-speed rotary dispersing and emulsifying device, CLEAMIX (product name: CLM-2.2S, manufactured by Em Technic), was used to stir at a rotor speed of 15,000 rpm at about 35° C. for 30 minutes to prepare a homogeneous raw material solution of indomethacin. In this way, when a plurality of components are mixed or dissolved, it is preferred to use CLEAMIX (manufactured by Em Technic), which is a high-speed rotary dispersing and emulsifying device, for preparation.
[0202] <Step 1: Mixing and precipitation>
[0203] Next, use Figure 2 The microreactor ULREA shown in (A) mixes the precipitation solvent of the prepared organic microparticles with the raw material solution of the prepared organic microparticles. Figure 2 The first introduction part d1 of the microreactor shown in (A) introduces the above-prepared organic microparticle precipitation solvent (here, 0.1 mol / L hydrochloric acid aqueous solution) as the first processed fluid (liquid A) into the processing surface at 200 mL / min and 5°C, and while the processing part 10 is operated at a rotation speed of 1700 rpm, the prepared indomethacin raw material solution as the second processed fluid (liquid B) is introduced into the processing surface 1 and 2 at 30 mL / min and 25°C, and mixed in the thin film fluid. Then, the discharge liquid containing indomethacin microparticles is discharged from the fluid processing surface 1 and 2.
[0204] <Process c: Recovery and cleaning>
[0205] The above-mentioned discharge liquid was filtered to recover the indomethacin microparticles. Then, the indomethacin microparticles were repeatedly washed with a washing solvent (pure water) to obtain a wet cake of indomethacin microparticles. The above-mentioned wet cake was diluted with pure water, and the dilution was dripped onto a collodion film, and TEM observation was performed using an observation sample dried at room temperature. The TEM observation results are shown in Figure 4In addition, the wet cake was vacuum dried at -0.095 MPaG for 16 hours to obtain a dry powder. The X-ray diffraction measurement results of the obtained dry powder are shown in Figure 5 Upper section.
[0206] The results of TEM observation confirmed that the average primary particle size of the indomethacin microparticles was about 76 nm. In addition, the results of X-ray diffraction measurement confirmed that the obtained particles were amorphous.
[0207] <Step 2: Particle property control>
[0208] For the particle property control in step 2, pure water was used as a solvent having a partial solubility for organic microparticles, and hydroxyethyl cellulose (HEC) was used as a surfactant capable of inhibiting the growth of organic microparticles. Hydroxyethyl cellulose was added to pure water, and a high-speed rotary dispersing and emulsifying device, CLEAMIX DISSOLVER (product name: CLM-2.2SD, manufactured by EMU TECHNICK), was used to stir at a rotor speed of 15,000 rpm for 30 minutes to prepare a hydroxyethyl cellulose aqueous solution (particle property control solution) in which a uniform texture was mixed. The wet cake of indomethacin microparticles obtained in step c was added to the particle property control solution to perform a dispersion treatment.
[0209] Specifically, the indomethacin microparticles obtained in step c were added to a 0.1 wt % aqueous solution of hydroxyethyl cellulose (viscosity: 200-300 mPa·s, 2% in water, at 20°C, manufactured by TCI) to give a 0.2 wt % concentration, and then dispersed using an ultrasonic disperser (manufactured by Hilux: UP200S) at an output of 0.5%, a circulation of 0.5, and a treatment temperature of 37°C±3°C for 15 minutes to obtain an indomethacin microparticle dispersion. When used for TEM observation, the obtained indomethacin microparticle dispersion was dripped onto a collodion film and dried at room temperature to obtain an observation sample. The TEM observation results are shown in FIG. Figure 6 middle.
[0210] The results of TEM observation confirmed that the average primary particle size of the indomethacin microparticles treated with a 0.1 wt% hydroxyethylcellulose aqueous solution was about 98 nm. In addition, the indomethacin microparticles were filtered and recovered from the above dispersion, washed with pure water, and then vacuum dried at -0.095 MPaG at 25°C for 16 hours to obtain a dry powder. The X-ray diffraction measurement results of the obtained dry powder are shown in Figure 5 Next paragraph.
[0211] The results of X-ray diffraction measurement confirmed that the indomethacin microparticles treated with a 0.1 wt% hydroxyethylcellulose aqueous solution in step 2 were transformed into α-type crystals. Figure 5For comparison, the X-ray diffraction measurement results of the indomethacin microparticles recovered and washed in step c (before the treatment in step 2) are also shown.
[0212] (Example A2)
[0213] Indomethacin microparticles were produced under the same conditions as in Example A1 except that the concentration of hydroxyethyl cellulose in step 2 of Example A1 was changed from 0.1 wt % to 0.05 wt %. A TEM photograph of the indomethacin microparticles obtained in step 2 of Example A2 is shown in FIG. Figure 7 In. Figure 7 As can be seen in , the average primary particle size of indomethacin microparticles was confirmed to be about 126 nm.
[0214] (Comparative Example A1)
[0215] As the solvent in the particle property control in Example A1 and Step 2, no surfactant was added, and only pure water was used as a solvent having a partial solubility for indomethacin. Indomethacin microparticles were produced under the same conditions as in Example A1.
[0216] The results of TEM observation of indomethacin microparticles obtained in step 2 of Comparative Example A1 are shown in FIG. Figure 8 The TEM observation results confirmed that the particles were coarsened to about 850 nm.
[0217] (Example A3: Indomethacin Microparticles)
[0218] The process from step 0 to step c is the same as that in Example A1, except that the solvent having a partial solubility for organic microparticles in step 2 is changed from pure water in Example A1 to hexane, and the hydroxyethyl cellulose in Example A1 is changed to Span80 as a surfactant capable of inhibiting the growth of organic microparticles, thereby producing indomethacin microparticles.
[0219] Specifically, a high-speed rotary dispersing and emulsifying device, CLEAMIX DISSOLVER (product name: CLM-2.2SD, manufactured by Em Technic), was used to stir at a rotor speed of 15,000 rpm for 30 minutes to prepare a uniformly mixed 0.01 wt% hexane solution of Span 80 (manufactured by Wako) (particle property control solution). After the indomethacin microparticles obtained in step c were added to the particle property control solution to make it 0.2 wt%, a magnetic stirrer was used to stir at 150 rpm at a temperature of 27°C for 16 hours to perform a dispersion treatment to obtain an indomethacin microparticle dispersion. The indomethacin microparticles were filtered and recovered from the obtained dispersion, and vacuum dried at 25°C at -0.095 MPaG for 16 hours to obtain a dry powder for X-ray diffraction measurement. The results of the X-ray diffraction measurement are shown in Fig. 9 Next paragraph. Explain, Fig. 9 The upper part shows the X-ray diffraction measurement results of the indomethacin microparticles obtained in step c of Example A3.
[0220] As a result of X-ray diffraction measurement, it was confirmed that the indomethacin fine particles treated with a 0.01 wt % hexane solution of Span 80 were converted into γ-type crystals.
[0221] Then, the above-mentioned dry powder was dispersed in a 0.1% hydroxyethyl cellulose (0.1wt% hydroxyethyl cellulose (viscosity: 200 to 300 mPa·s, 2% in water, at 20°C, manufactured by TCI) aqueous solution to obtain a sample for TEM observation. The TEM observation results are shown in Fig.10 middle.
[0222] The results of TEM observation confirmed that the average primary particle size of the indomethacin microparticles treated with a 0.01 wt % hexane solution of Span 80 (particle property control solution) in step 2 of Example A3 was about 138 nm.
[0223] (Comparative Example A2: Indomethacin Microparticles)
[0224] As the solvent in the particle property control in Example A3, step 2, no surfactant was added, and only hexane, which is a solvent having a partial solubility for indomethacin, was used. Indomethacin microparticles were produced under the same conditions as in Example A3.
[0225] The results of TEM observation of the indomethacin microparticles obtained in Comparative Example A2 and Step 2 are shown in FIG. Fig.11 The TEM observation results confirmed that the particles were coarsened to about 1000 nm.
[0226] (Example A4: Indomethacin Microparticles)
[0227] In Example A4, the types of indomethacin precipitation solvent and indomethacin raw material solution in step 0 of Examples A1 to 3 were changed to precipitate α-type indomethacin microparticles in step 1. In addition, the surfactant capable of inhibiting the growth of organic microparticles in step 2 of Example A1 was changed.
[0228] In step 0, pure water was used as the precipitation solvent (liquid A) for the organic microparticles. Since it was a single solvent, no preparation was performed. As a raw material solution of organic microparticles (liquid B), γ-type indomethacin was mixed in ethanol to make 1.0 wt%, and polyvinyl pyrrolidone (Kollidon 12PF (manufactured by BASF)) was mixed to make 1.0 wt%, to prepare an indomethacin raw material solution. By using a high-speed rotary dispersing and emulsifying device, CLEAMIX (product name: CLM-2.2S, manufactured by Em Technik), in the same manner as in Examples A1 to 3, stirring was performed at a rotor speed of 15,000 rpm at about 35°C for 30 minutes to prepare a homogeneous indomethacin raw material solution.
[0229] The procedures of step 1: mixing and precipitation and step c: recovery and washing are the same as those of Examples A1 to 3. In step 1, indomethacin microparticles were precipitated in the same manner as in Examples A1 to 3, and a sample for TEM observation and a dry powder for X-ray diffraction measurement were obtained using the wet cake obtained in step c. The TEM observation results are shown in Fig.12 The X-ray diffraction measurement results are shown in Fig.13 Upper section.
[0230] The results of TEM observation confirmed that the average primary particle size of the indomethacin microparticles after washing in step c was about 146 nm. In addition, the results of X-ray diffraction measurement confirmed that the indomethacin microparticles were α-type crystals. The crystallinity was 50%.
[0231] <Step 2: Particle property control>
[0232] For the particle property control in step 2, pure water was used as a solvent having a partial solubility for organic microparticles, and Lutrol F127 (manufactured by BASF) was used as a surfactant capable of inhibiting the growth of organic microparticles. Lutrol F127 was added to pure water, and a high-speed rotary dispersing and emulsifying device, CLEAMIX DISSOLVER (product name: CLM-2.2SD, manufactured by Em Technic), was used to stir at a rotor speed of 15,000 rpm for 30 minutes to prepare a uniformly mixed Lutrol F127 aqueous solution (particle property control solution). The wet cake of indomethacin microparticles obtained in step c was added to the particle property control solution to perform a dispersion treatment.
[0233] Specifically, the indomethacin fine particles obtained in step c were added to a 0.1 wt % Lutrol 127 aqueous solution to a concentration of 0.2 wt %, and then dispersed using an ultrasonic disperser (manufactured by Hilux: UP200S) at an output of 0.5 %, a circulation of 0.5, and a treatment temperature of 37°C ± 3°C for 15 minutes to obtain an indomethacin dispersion. The obtained indomethacin dispersion was dripped onto a collodion film and dried at room temperature to obtain a sample for TEM observation. The TEM observation results are shown in FIG. Fig.14 middle.
[0234] The results of TEM observation confirmed that the average primary particle size of indomethacin microparticles treated with 0.1 wt% Lutrol F 127 aqueous solution was about 168 nm. In addition, the above dispersion was filtered and recovered, washed with water, and then vacuum dried at -0.095 MPaG at 25°C for 16 hours to obtain a dry powder for X-ray diffraction measurement. The results of X-ray diffraction measurement are shown in Fig.13 Next paragraph.
[0235] The results of X-ray diffraction measurement confirmed that the indomethacin microparticles treated with a 0.1 wt% hydroxyethylcellulose aqueous solution were the same α-type as the indomethacin microparticles obtained in step c. In addition, it was confirmed that the crystallinity was 62.5%, which was higher than that of the indomethacin microparticles obtained in step c. This is considered to be because the amorphous parts contained in the indomethacin microparticles obtained in steps 1 and 2 were crystallized.
[0236] (Comparative Example A3: Indomethacin Microparticles)
[0237] As the solvent in the particle property control in Example A4, step 2, no surfactant was added, and only pure water was used as a solvent having a partial solubility for indomethacin. Indomethacin microparticles were produced under the same conditions as in Example A4.
[0238] The TEM observation results are shown in Fig.15 The TEM observation results confirmed that the particles were coarsened to about 1160 nm.
[0239] (Example A5: Curcumin microparticles)
[0240] <Step 0: Preparation of a precipitation solvent (liquid A) and a raw material solution (liquid B) of organic particles> In step 0, pure water was used for the precipitation solvent (liquid A) of the organic particles. Since it was a single solvent, no preparation was performed. As a raw material solution (liquid B) of organic particles, curcumin having a crystal form of type 1 was mixed in ethanol to a concentration of 0.5 wt%, and polyvinyl pyrrolidone (Kollidon 12PF (manufactured by BASF)) was mixed to a concentration of 0.5 wt%, to prepare a curcumin raw material solution. By using a high-speed rotary dispersing and emulsifying device, CLEAMIX (product name: CLM-2.2S, manufactured by Em Technic), in the same manner as in Examples A1 to 4, a homogeneous curcumin raw material solution was prepared by stirring at a rotor speed of 15,000 rpm at about 35°C for 30 minutes.
[0241] <Step 1: Mixing and precipitation>
[0242] Next, use Figure 2 The microreactor shown in (A) mixes the precipitation solvent of the organic microparticles and the raw material solution of the prepared organic microparticles. Figure 2 The first introduction part d1 of the microreactor shown in (A) introduces the above-prepared organic microparticle precipitation solvent (here pure water) as the first processed fluid (liquid A) into the processing surface at 500 mL / min at 5°C, and while the processing part 10 is operated at a rotation speed of 1700 rpm, the raw material solution of the prepared organic microparticles as the second processed fluid (liquid B) is introduced into the processing surface 1 and 2 at 30 mL / min at 25°C, and mixed in the thin film fluid. Then, the discharge liquid containing curcumin microparticles is discharged from the fluid processing surface 1 and 2.
[0243] <Process c: Recovery and cleaning>
[0244] The curcumin microparticles were recovered by filtering the above-mentioned discharge liquid and removing the supernatant. Then, the curcumin microparticles were repeatedly washed three times with a cleaning solvent (pure water) to obtain a wet cake of curcumin microparticles. The above-mentioned wet cake was diluted with pure water, and the dilution was dripped onto a collodion film, and a sample for observation dried at room temperature was used for TEM observation.
[0245] The wet cake was vacuum dried at -0.095 MPaG for 16 hours to obtain a dry powder for X-ray diffraction measurement. The TEM observation results are shown in Fig.16 The X-ray diffraction measurement results are shown in Fig.17 Upper section.
[0246] The results of TEM observation confirmed that the average primary particle size of the curcumin microparticles was about 88 nm. In addition, the results of X-ray diffraction measurement confirmed that the obtained particles were amorphous.
[0247] <Step 2: Particle property control>
[0248] For the particle property control in step 2, pure water was used as a solvent having a partial solubility for organic particles, and polyvinyl alcohol was used as a surfactant that can inhibit the growth of organic particles. Polyvinyl alcohol (PVA) was added to pure water, and a high-speed rotary dispersing and emulsifying device, CLEAMIX DISSOLVER (product name: CLM-2.2SD, manufactured by EMU TECHNICK), was used to stir at a rotor speed of 15000 rpm for 30 minutes, thereby preparing a homogeneously mixed polyvinyl alcohol aqueous solution (particle property control solution). The wet cake of curcumin particles obtained in step c was added to the particle property control solution and dispersed.
[0249] Specifically, the curcumin microparticles obtained in step c were added to a 0.2wt% aqueous solution of polyvinyl alcohol 500 (completely saponified type) as a particle property control solution to obtain a 0.2wt% solution, and then an ultrasonic disperser (manufactured by Hilux: UP200S) was used to perform a dispersion treatment at an output of 0.5%, a circulation of 0.5, and a treatment temperature of 30°C ± 3°C for 30 minutes to obtain a curcumin microparticle dispersion. The obtained dispersion was dripped onto a collodion film and dried at room temperature to obtain a sample for TEM observation. The TEM observation results are shown in Fig.18 middle.
[0250] The results of TEM observation confirmed that the average primary particle size of the curcumin microparticles treated with a 0.2wt% polyvinyl alcohol 500 (completely saponified) aqueous solution was about 108nm. In addition, the liquid after the above dispersion treatment was filtered and recovered, washed with water, and then vacuum dried at -0.095MPaG at 25°C for 12 hours to obtain a dry powder for X-ray diffraction measurement. The X-ray diffraction measurement results are shown in Fig.17 Middle section.
[0251] As a result of X-ray diffraction measurement, it was confirmed that the curcumin fine particles treated with a 0.2 wt % aqueous solution of polyvinyl alcohol 500 (completely saponified type) were transformed from amorphous to type 3 crystals.
[0252] (Comparative Example A4)
[0253] As the solvent in the particle property control in Example A5, step 2, no surfactant was added, and only pure water was used as a solvent having a partial solubility for curcumin. Curcumin microparticles were produced under the same conditions as in Example A5.
[0254] The TEM observation results are shown in Fig.19The TEM observation results confirmed that the curcumin fine particles were transformed into Type 3 crystals, but the average particle size was about 980 nm, and the particles were coarsened.
[0255] (Example A6)
[0256] Steps 0 to c were the same as those in Example A5, except that the solvent having a partial solubility for the organic fine particles in step 2 was changed from pure water in Example A5 to hexane, thereby producing curcumin fine particles.
[0257] As a surfactant that can inhibit the growth of organic particles, Span 80 (manufactured by Wako) was used. Span 80 was added to hexane, and a high-speed rotary dispersing and emulsifying device, CLEAMIX DISSOLVER (product name: CLM-2.2SD, manufactured by Em Technic), was used, and the mixture was stirred at a rotor speed of 15,000 rpm for 30 minutes to prepare a homogeneously mixed solution (particle property control solution). The dry powder of the curcumin particles obtained in step c was added to the particle property control solution and dispersed.
[0258] Specifically, the curcumin microparticles obtained in step c were added to a 0.01wt% hexane solution of Span80 as a particle property control solution to a concentration of 0.2wt%, and then dispersed under the same conditions as in Example A5 to obtain curcumin microparticles. The curcumin microparticles were filtered and recovered from the obtained dispersion, and vacuum dried at 25°C for 16 hours at -0.095MPaG to obtain a dry powder for X-ray diffraction measurement. The X-ray diffraction measurement results are shown in Fig.17 Next paragraph.
[0259] The results of X-ray diffraction measurement confirmed that the curcumin microparticles treated with a 0.1 wt % Span 80 hexane solution were transformed from amorphous to type 2 crystals.
[0260] Then, the above-mentioned dry powder was dispersed in a 0.1% hydroxyethyl cellulose (0.1wt% hydroxyethyl cellulose (viscosity: 200-300mPa·s in water 2% at 20°C, manufactured by TCI) aqueous solution to obtain a sample for TEM observation. The TEM observation results are shown in Fig. 20 As a result of TEM observation, it was confirmed that the primary particle size of the curcumin microparticles treated with a 0.1 wt % hexane solution of Span 80 was about 97 nm.
[0261] (Comparative Example A5)
[0262] As the solvent in the particle property control in Example A6, step 2, no surfactant was added, and only hexane, which is a solvent having a partial solubility for curcumin, was used. Curcumin microparticles were produced under the same conditions as in Example A6.
[0263] The TEM observation results of the curcumin microparticles obtained in Comparative Example A5 and Step 2 are shown in FIG. Fig.21 The TEM observation results confirmed that the crystals were transformed into Type 3, but the particles were coarsened to 1000 nm or more.
[0264] (Example A7: Polypropylene microparticles)
[0265] <Step 0: Preparation of a solvent for precipitating organic microparticles (Solution A) and a raw material solution for organic microparticles (Solution B)>
[0266] In step 0, acetone was used as the precipitation solvent (liquid A) for the organic microparticles. Since it was a single solvent, no preparation was performed. As a raw material solution (liquid B) for the organic microparticles, polypropylene with an α-type crystal form was mixed with toluene to prepare a 1wt% polypropylene raw material solution. By using a high-speed rotary dispersing and emulsifying device, CLEAMIX (product name: CLM-2.2S, manufactured by Em Technik), in the same manner as in Examples A1 to 6, stirring at about 85°C for 30 minutes at a rotor speed of 15,000 rpm, a homogeneous polypropylene raw material solution was prepared.
[0267] <Step 1: Mixing and precipitation>
[0268] In Example A7, as Example A of Step 1 using an intermittent method, a precipitation solvent for organic microparticles and a raw material solution for organic microparticles were mixed using a cleamex. Specifically, 500 mL of acetone (liquid A) cooled to 5° C. was stirred at 15,000 rpm, and 30 mL of the prepared raw material solution for organic microparticles (liquid B) was slowly dripped and mixed at 80° C. Then, a liquid containing polypropylene microparticles was recovered from the cleamex.
[0269] <Process c: Recovery and cleaning>
[0270] The liquid containing the polypropylene microparticles was filtered to remove the supernatant, thereby recovering the polypropylene microparticles, and then repeatedly washed with a washing solvent (acetone) to obtain a wet cake of the polypropylene microparticles.
[0271] The wet cake was vacuum dried at -0.095 MPaG for 16 hours to obtain a dry powder for SEM observation and X-ray diffraction measurement. The SEM observation results are shown in Fig. 22 The X-ray diffraction measurement results are shown in Fig.23 In the above paragraph.
[0272] The results of SEM observation confirmed that the average primary particle size of the polypropylene microparticles was about 124 nm. In addition, the results of X-ray diffraction measurement confirmed that the obtained particles were α-type crystals. The crystallinity was 85.6%.
[0273] <Step 2: Particle property control>
[0274] For the particle property control in step 2, an isopropyl alcohol aqueous solution (IPA + pure water) was used as a solvent having a partial solubility for organic particles, and Tween 80 (manufactured by Wako) was used as a surfactant that can inhibit the growth of organic particles. Tween 80 was added to the isopropyl alcohol aqueous solution, and a high-speed rotary dispersing and emulsifying device, CLEAMIX DISSOLVER (product name: CLM-2.2SD, manufactured by Em Technic), was used to stir at a rotor speed of 15,000 rpm for 30 minutes to prepare a homogeneously mixed aqueous solution (particle property control solution). The wet cake of polypropylene particles obtained in step c was added to the particle property control solution and dispersed.
[0275] Specifically, the polypropylene microparticles obtained in step c were added to a 0.1wt% Tween80 / 2.0wt% isopropanol / 97.9wt% aqueous solution as a particle property control solution so as to be 0.2wt%, and then an ultrasonic disperser (manufactured by Hilux: UP200S) was used to perform a dispersion treatment at an output of 0.5%, a circulation of 0.5, and a treatment temperature of 70°C±3°C for 15 minutes to obtain a polypropylene microparticle dispersion. The polypropylene microparticles were filtered and recovered from the obtained dispersion, washed with pure water, and then vacuum dried at 25°C for 16 hours at -0.095MPaG to obtain a dry powder for SEM observation and X-ray diffraction measurement. The SEM observation results are shown in Fig.24 The X-ray diffraction measurement results are shown in Fig.23 In the next paragraph.
[0276] The results of SEM observation confirmed that the average primary particle size of the polypropylene microparticles was about 197 nm. In addition, the results of X-ray diffraction measurement confirmed that the obtained particles were α-type crystals, the same as the polypropylene microparticles obtained in step c. It was confirmed that the crystallinity was 93.5%, which was higher than that of the polypropylene microparticles obtained in step c. It is believed that the reason is that the amorphous parts contained in the polypropylene microparticles obtained in steps 1 and 2 are crystallized.
[0277] (Comparative Example A6)
[0278] As the solvent for controlling the particle properties in Example A7, Step 2, no surfactant was added, and only an isopropyl alcohol aqueous solution (2.0 wt% isopropyl alcohol / 98.0 wt% aqueous solution) was used as a solvent having a partial solubility for polypropylene. In addition, polypropylene microparticles were produced under the same conditions as in Example A7.
[0279] The SEM observation results are shown in Fig.25 From the SEM observation results, it was confirmed that the average primary particle size was about 512 nm.
[0280] (Example A8: Pirenoxine Microparticles)
[0281] <Step 0: Preparation of a solvent for precipitating organic microparticles (Solution A) and a raw material solution for organic microparticles (Solution B)>
[0282] <Preparation of organic microparticle precipitation solvent (Solution A)>
[0283] As a precipitation solvent (liquid A) for organic microparticles, citric acid was mixed with pure water in a manner of 1.9 wt % to prepare a pirenoxine precipitation solvent. A homogeneous pirenoxine precipitation solvent was prepared by stirring at about 35° C. for 30 minutes at a rotor speed of 15000 rpm using a high-speed rotary dispersing and emulsifying device, and the pirenoxine precipitation solvent was prepared. The pH of the prepared pirenoxine precipitation solvent was 2.1.
[0284] <Preparation of raw material solution (Solution B) of organic microparticles>
[0285] As a raw material solution of organic microparticles (liquid B), 0.01 mol / L sodium hydroxide aqueous solution was mixed so that 0.2 wt% of pirenoxine was obtained, thereby preparing a pirenoxine raw material solution. A homogeneous pirenoxine raw material solution was prepared by stirring at about 35° C. for 30 minutes at a rotor speed of 15000 rpm using a CLEAMIX (product name: CLM-2.2S, manufactured by Em Technik) as a high-speed rotary dispersing emulsifier. The pH of the prepared pirenoxine raw material solution was 12.0.
[0286] <Step 1: Mixing and precipitation>
[0287] Next, use Figure 2 The microreactor shown in (A) mixes the prepared organic microparticle precipitation solvent and the prepared organic microparticle raw material solution. Figure 2The first introduction part d1 of the microreactor shown in (A) introduces the prepared pirenoxine precipitation solvent (here, 1.9wt% citric acid aqueous solution) as the first processed fluid (liquid A) into the processing surface at 300mL / min at 25°C, and while the processing part 10 is operated at a rotation speed of 1700rpm, the prepared pirenoxine raw material solution as the second processed fluid (liquid B) is introduced into the processing surface 1 and 2 at 20mL / min at 25°C, and mixed in the thin film fluid. Then, the discharge liquid containing pirenoxine particles is discharged from the fluid processing surface 1 and 2. The pH of the discharge liquid containing pirenoxine particles is 2.48.
[0288] The discharged liquid containing pirenoxine microparticles was dripped onto a collodion film and dried at room temperature to prepare a sample for observation, and TEM observation was performed. The TEM observation results confirmed that the average primary particle size of the pirenoxine microparticles was about 42 nm. The TEM observation results are shown in Fig.26 middle.
[0289] <Step 2: Particle property control>
[0290] For the particle property control in step 2, pure water was used as a solvent having a partial solubility for organic particles, and Tween 80 and benzalkonium chloride were used as surfactants capable of inhibiting the growth of organic particles. Tween 80 and benzalkonium chloride were added to pure water, and stirred at a rotor speed of 15000 rpm for 15 minutes using a high-speed rotary dispersing and emulsifying device, CLEAMIX DISSOLVER (product name: CLM-2.2SD, manufactured by EMU TECHNICK), thereby preparing a uniformly mixed Tween 80 and benzalkonium chloride aqueous solution (particle property control solution), and the pirenoxine particle dispersion obtained in step 1 was added to the particle property control solution to perform a dispersion treatment.
[0291] Specifically, 500 g of the pirenoxine microparticle dispersion obtained in step 1 was added to 500 g of 0.03 wt% Tween 80-0.01 wt% benzalkonium chloride-99.96 wt% pure water. Then, using a CLEAMIX DUBLE MOTION (manufactured by Em Technic: CLM-2.2 / 3.7W), a dispersion treatment was carried out for 30 minutes at a rotor speed of 20,000 rpm, a screen speed of 18,000 rpm, and a treatment temperature of 42°C ± 3°C to obtain a pirenoxine microparticle dispersion. When used for TEM observation, the obtained pirenoxine microparticle dispersion was dripped onto a collodion film and dried at room temperature to obtain an observation sample. The TEM observation results are shown in Fig. 27 middle.
[0292] The results of TEM observation confirmed that the average primary particle size of the pirenoxine microparticles treated in an aqueous solution containing Tween 80 was about 48 nm. In addition, the pirenoxine microparticles were filtered and recovered from the above-mentioned dispersion, washed with pure water, and then vacuum dried at -0.095 MPaG at 25°C for 16 hours to obtain a dry powder. The X-ray diffraction measurement results of the obtained dry powder are shown in Fig.28 The following paragraphs. It is to be noted that, for comparison of crystallinity, the pirenoxine microparticle dispersion (the discharge liquid from step 1) before the dispersion treatment in step 2 was filtered and recovered in the same manner as above, and after washing with pure water, the powder dried under the same conditions was subjected to XRD diffraction measurement. These results are shown in Fig.28 The results of XRD diffraction measurement confirmed that the crystallinity before the dispersion treatment in step 2 was 58.1%, while the crystallinity after the dispersion treatment in step 2 increased to 63.2%. In addition, the results of X-ray diffraction measurement confirmed that the crystal form of the obtained particles did not change before and after the treatment.
[0293] Table 1 shows the results of Examples A1 to 8 and Comparative Examples A1 to 6 described above.
[0294] [Table 1]
[0295]
[0296] It should be noted that the "--" recorded in the column of crystallinity in Table 1 indicates amorphous. In addition, the crystallinity is measured using XRD as described above, and the ratio (Xa / Xb) of the average primary particle size value (Xa) before and after the treatment with the particle property control solution using organic microparticles in step 2 and after the treatment in step 2 to the average primary particle size value (Xb) before the treatment in step 2, that is, after the end of step c (only in Example A8, after the end of step 1) is set as the crystallinity change rate. Furthermore, regarding pyrenoxine, since the name of the crystal form is generally not used, the column of the crystal form of Example A8 in Table 1 is recorded as "×", indicating that there is no change in the crystal form before and after the treatment in step 2.
[0297] From the results of Examples A1 and 2 and Comparative Example A1, it can be seen that in pure water, which is a solvent that partially dissolves indomethacin, indomethacin microparticles are coarsened, but by performing particle property control in step 2 of adding a surfactant that can inhibit the growth of organic microparticles to the above solvent, the particle size of indomethacin microparticles is substantially unchanged, and coarsening can be suppressed. It can also be seen that by performing particle property control in step 2, amorphous particles can be transformed into α-type crystals.
[0298] Furthermore, from the results of Examples A1, 2 and A3, it was confirmed that the effect of controlling the particle properties in step 2 was obtained even when the type of the solvent having a partial solubility for indomethacin or the surfactant capable of inhibiting the growth of indomethacin was changed.
[0299] The results of Examples A1 to 4 show that the effect of the particle shape control in step 2 does not depend on the crystal form of indomethacin. In addition, it is known that the particle shape control in step 2 not only causes the crystal transformation but also improves the crystallinity.
[0300] As shown in Examples A5 to 8 and Comparative Examples A4 to 6, the above effects are not limited to indomethacin of Examples A1 to 4, but are also effective for other organic fine particles.
[0301] Furthermore, from the results of Example A8, it was confirmed that even if step c of washing and / or replacing the solvent of the organic fine particles obtained in step 1 is omitted, the effect of controlling the particle properties in step 2 can be obtained.
[0302] (Group of Example B)
[0303] Hereinafter, the group (red organic pigment) of Example B will be described.
[0304] A powder X-ray diffractometer (product name: X'PertPROMPD, manufactured by PANalytical) was used for the XRD measurement in Example B. The measurement conditions were: measurement range: 6-60°, Cu counter cathode, tube voltage 45 kV, tube current 40 mA, scanning speed 16° / min.
[0305] In addition, a transmission electron microscope, JEM-2100 (manufactured by JEOL) was used for TEM observation. As observation conditions, an acceleration voltage was set to 80 kV and an observation magnification was set to 25000 times.
[0306] (In the case of intermittent method)
[0307] As in Example A, Figure 1 Pigment particles were produced by following steps 0 to 2 shown in FIG.
[0308] (Process 0)
[0309] The pigment particle precipitation solvent (liquid A) and the pigment particle raw material solution (liquid B) shown in the following Table 2 were prepared: both liquid A and liquid B were set at a liquid temperature of 40°C, and each was stirred at 300 rpm for 30 minutes using a magnetic stirrer and a stirring bar to obtain each prepared liquid.
[0310] (Process 1)
[0311] Mixing of liquid A and liquid B: As shown in Table 2 below, liquid A is stirred at 300 rpm using a magnetic stirrer and a stirrer, and liquid B is added to precipitate organic pigment particles. It is noted that the slurry containing organic pigment particles obtained in step 1 is filtered, and the organic pigment particles are washed with pure water (step c) to obtain a wet cake of organic pigment particles. Alternatively, a dry powder of organic pigment particles is obtained by drying such as vacuum drying.
[0312] (Process 2)
[0313] The wet cake or dry powder of the organic pigment is put into a solvent (particle property control solution) to which a surfactant or dispersant is added and partially soluble in organic particles, and stirred for a certain period of time using a CLEAMIX CLM-2.2S stirrer with a rotating stirring blade.
[0314] [Table 2]
[0315]
[0316] Explanation of abbreviations: DMSO: dimethyl sulfoxide, BTMA: benzyltrimethylammonium hydroxide, MeOH: methanol, soln: solution, PR254: CI Pigment Red 254, PR122: CI Pigment Red 122
[0317] The average primary particle size of the pigment particles after washing in step c and after stirring in step 2 was calculated by TEM observation, and the crystallinity was measured and compared by XRD measurement (see Table 3 below). Among them, the crystallinity is the proportion of the crystallized component relative to the whole of the crystallized component and the amorphous component. The higher the crystallinity of the pigment, the higher the durability against light, heat, moisture, etc. It should be noted that the definitions of ◎, ○, △, and × are as follows.
[0318] When Da is the average primary particle size of the particles after the action of step 2, and Db is the average primary particle size before step 2 and after washing,
[0319] "◎" means the following situations:
[0320] Da / Db is in the range of 1.0 to 4.0, and
[0321] When Xa is the crystallinity of the particles after the action of step 2 and Xb is the crystallinity before step 2 and after washing, Xa / Xb is 1.05 or more, and
[0322] Da is 80nm or less, and
[0323] From the viewpoint of uniformity of the microparticles, when TEM observation of three fields was performed at 25,000 times, no particles having a Db exceeding 8.0 times were confirmed in the pigment microparticles in step 2 (after the action).
[0324] "○" means the following situations:
[0325] Da / Db is in the range of 1.0 to 4.0, and
[0326] Xa / Xb is 1.05 or more, and
[0327] Da is larger than 80nm, and
[0328] From the viewpoint of uniformity of the microparticles, when TEM observation of three fields was performed at 25,000 times, no particles having a Db exceeding 8.0 times were confirmed in the pigment microparticles in step 2 (after the action).
[0329] "△" is the following situation:
[0330] Da / Db is in the range of 1.0 to 4.0, and
[0331] Xa / Xb is 1.05 or more, and
[0332] From the viewpoint of uniformity of the microparticles, when TEM observation of three fields was performed at 25,000 times, it was confirmed that among the pigment microparticles in step 2 (after the action), a maximum of one particle whose Db exceeded 8.0 times was found.
[0333] "×" indicates a case where the condition does not correspond to any of the above "◎", "○", and "△".
[0334] The average primary particle size is measured by averaging a total of 100 particles observed in a plurality of fields of view at 25,000 times magnification in TEM observation.
[0335] [Table 3]
[0336]
[0337] (When using a microreactor)
[0338] In Example B, Liquid A is equivalent to Figure 2 The first fluid to be processed introduced into the first inlet d1 of the microreactor shown in (A), and the B liquid is equivalent to the second fluid to be processed introduced from the second inlet d2. The replacement of the two is arbitrary. It should be noted that in Example B, ULREA (manufactured by Em Technik) was used as the microreactor.
[0339] Liquid A and Liquid B were mixed in a microreactor operated under the conditions shown in Table 4 below, and the mixture was stirred as in Example A. Figure 1 Pigment particles were produced by following steps 0 to 2 shown in FIG.
[0340] (Process 0) As shown in Table 5, the pigment particle precipitation solvent (liquid A) and the pigment particle raw material solution (liquid B) are prepared: the liquid temperature of both liquid A and liquid B is set to 40°C, and the above-mentioned CLEAMIX CLM-2.2S is used. Liquid A is stirred at 10,000 rpm and liquid B is stirred at 20,000 rpm for 30 minutes to obtain each prepared liquid.
[0341] (Process 1) Use Figure 1 In the microreactor shown in the figure, the organic pigment solution (liquid B) and the poor solvent (liquid A) are mixed to precipitate the organic pigment particles. It is explained that the slurry containing the organic pigment particles obtained in (step 1) is filtered, and the organic pigment particles are washed with pure water (step c) to obtain a wet cake of the organic pigment particles or a dry powder of the organic pigment particles is obtained by drying treatment such as vacuum drying.
[0342] (Step 2) The wet cake or dry powder of the organic pigment is placed in a solvent (particle property control solution) to which a surfactant or dispersant is added and partially soluble in organic particles, and stirred for a certain period of time using the CLEAMIX CLM-2.2S.
[0343] [Table 4]
[0344]
[0345] Table 5
[0346]
[0347] Next, similarly to the case of the intermittent method, the average primary particle size of the pigment particles obtained in step 1 and step 2 was calculated by TEM observation, and the crystallinity was measured and compared by XRD measurement (see Table 6 below). The meanings of symbols and abbreviations are the same as those in the case of the intermittent method. The definitions of ◎, ○, △, and × are also the same as those in the case of the intermittent method.
[0348] [Table 6]
[0349]
[0350] As shown in the TEM observation photograph of the red pigment nanoparticles of the present invention obtained from Experiment No. 1-2 of Example B ( Fig.30), when the manufacturing method of the present invention is applied to Example B, it can be seen that due to the effect of the particle property controlling solution, the obtained red organic pigment particles can inhibit necking and growth.
[0351] In Experiment No. 2-1, when the above-mentioned TEM observation was performed, two or more particles having a Db exceeding 8.0 times were confirmed in each pigment fine particle in step 2 (after the action), and this was used as a comparative example.
[0352] (Group of Example C)
[0353] Next, the group (cyan organic pigment) of Example C will be described.
[0354] A powder X-ray diffractometer (product name: X'PertPRO MPD, manufactured by PANalytical) was used for the XRD measurement in Example C. The measurement conditions were: measurement range: 6 to 60°, Cu counter cathode, tube voltage 45 kV, tube current 40 mA, scanning speed 16° / min.
[0355] In addition, a transmission electron microscope, JEM-2100 (manufactured by JEOL) was used for TEM observation. As observation conditions, an acceleration voltage was set to 80 kV and an observation magnification was set to 25000 times.
[0356] (When using a microreactor)
[0357] Liquid A and liquid B were mixed under the following conditions, and cyan organic pigment particles were produced by the following procedure.
[0358] In Example C, ULREA (manufactured by Em Tech) was used as the microreactor. In this case, liquid A is equivalent to liquid Figure 2 The first fluid to be processed introduced into the first introduction part d1 of the microreactor shown in (A) corresponds to the first fluid to be processed introduced from the second introduction part d2. The first introduction part d1 and the second introduction part d2 may be replaced arbitrarily.
[0359] The experimental formulation in Example C is shown in Table 7.
[0360] [Table 7]
[0361]
[0362] Among them, CuPc: copper phthalocyanine, TiOPc: oxytitanium phthalocyanine, CoPc: cobalt phthalocyanine, H2SO4: concentrated sulfuric acid.
[0363] In Example C, as in Example A, Figure 1Pigment particles were produced by following steps 0 to 2 shown in FIG.
[0364] (Process 0)
[0365] When mixing and precipitation were carried out using ULREA using the above experimental formulation, liquid A and liquid B were prepared as follows.
[0366] Preparation conditions of organic pigment particle precipitation solvent (liquid A):
[0367] In the case of a single solvent as described in the above experimental formula, preparation is not necessary, but when applying the experimental formula described in Patent Document 8, it is desirable to use CLEAMIX for stirring. For example, in Example C, CLM-2.2S was used for stirring at 10,000 rpm for 30 minutes.
[0368] Preparation conditions of the raw material solution (Solution B) of organic pigment particles:
[0369] The mixture was stirred at 20,000 rpm for 30 minutes using a CLEAMIX CLM-2.2S. The preparation temperature of both liquid A and liquid B was 40°C.
[0370] (Process 1)
[0371] Using ULREA under the operating conditions shown in Table 8 below, an organic pigment particle precipitation solvent (liquid A) and a raw material solution of organic pigment particles (liquid B) were mixed to precipitate cyan organic pigment fine particles.
[0372] The slurry containing the cyan organic pigment particles obtained in step 1 is filtered, and the cyan organic pigment particles are washed with pure water (step c) to obtain a wet cake of cyan organic pigment particles (or a dry powder of cyan organic pigment particles obtained by drying such as vacuum drying).
[0373] (Process 2)
[0374] The wet cake (or dry powder) of the cyan organic pigment particles obtained in step 1 is added to a solvent having partial solubility for organic particles, or a solvent having partial solubility for organic particles to which a surfactant and / or a dispersant are added (particle property control solution). After the addition, a stirring treatment is performed for a certain period of time using a cleamix.
[0375] [Table 8]
[0376]
[0377] Table 9 below shows changes in particle size and crystallinity of the cyan organic pigment fine particles before and after the stirring treatment in the case of using a microreactor.
[0378] [Table 9]
[0379]
[0380] In addition, the definitions of abbreviations and terms related to the above-mentioned Example C are as shown in the following Table 10.
[0381] [Table 10]
[0382]
[0383] It should be noted that the definition of the evaluation results in Table 9 is the same as that of Example B regarding the red organic pigment.
[0384] The average primary particle size of the cyan organic pigment particles after step c (cleaning) and step 2 (action) was calculated by TEM observation, and the crystallinity was measured and compared by XRD measurement (Table 9). In addition, the TEM images obtained in the experiment number 1-7 of the above-mentioned Example C are shown ( Figure 32 to Figure 35 ). In addition, the TEM image of the comparative example obtained in the experiment number 3-1 of the above-mentioned Example C is shown ( Fig.37 ).
[0385] According to the above experimental results, in step 2, in the comparative example experiment in which a surfactant and a dispersant were not contained in a solvent having a partial solubility for cyan organic pigment particles (simply described as a solvent in Table 9), particle growth and necking occurred. Fig.37 On the other hand, when the production method of the present invention is applied to Example C, it is found that the obtained cyan organic pigment fine particles can suppress necking and growth.
[0386] (In the case of intermittent method)
[0387] In the same manner as in the case of using a microreactor, cyan organic pigment fine particles were produced by mixing liquid A and liquid B prepared using the formulation shown in Table 11 below.
[0388] [Table 11]
[0389]
[0390] Among them, CuPc: copper phthalocyanine, TiOPc: oxytitanium phthalocyanine, CoPc: cobalt phthalocyanine, H2SO4: concentrated sulfuric acid.
[0391] The processing contents in Example C are as follows.
[0392] (Process 0)
[0393] When mixing and precipitation were carried out by a batch method using the above experimental recipe, liquid A and liquid B were prepared as follows.
[0394] Preparation conditions of organic pigment particle precipitation solvent (liquid A):
[0395] In the case of a single solvent as described in the experimental formulation, preparation is not necessary, but when applying the experimental formulation described in Patent Document 8, it is desirable to use CLEAMIX for stirring. For example, in Example C, CLM-2.2S was used for stirring at 10,000 rpm for 30 minutes.
[0396] Preparation conditions of the raw material solution (Solution B) of organic pigment particles:
[0397] The mixture was stirred at 20,000 rpm for 30 minutes using a CLEAMIX CLM-2.2S.
[0398] In addition, both liquid A and liquid B were prepared at a temperature of 40°C.
[0399] (Process 1)
[0400] The organic pigment particle precipitation solvent (liquid A) in the beaker is stirred at 300 rpm using a magnetic stirrer and a stirring bar, and a raw material solution of organic pigment particles (liquid B) is added to mix liquid A and liquid B to precipitate cyan organic pigment particles. The slurry containing cyan organic pigment particles obtained in step 1 is filtered, and the cyan organic pigment particles are washed with pure water (step c) to obtain a wet cake of cyan organic pigment particles (or a dry powder of cyan organic pigment particles obtained by drying such as vacuum drying).
[0401] (Process 2)
[0402] The wet cake (or dry powder) of the cyan organic pigment particles obtained in step 1 is added to a solvent having partial solubility for organic particles, or a solvent having partial solubility for organic particles to which a surfactant and / or a dispersant are added (particle property control solution). After the addition, a stirring treatment is performed for a certain period of time using a cleamix.
[0403] The changes in particle size and crystallinity of the cyan organic pigment particles before and after the intermittent stirring treatment are shown in Table 12 below.
[0404] [Table 12]
[0405]
[0406] The average primary particle size of the cyan organic pigment particles after step c (cleaning) and step 2 (action) was calculated by TEM observation, and the crystallinity was measured and compared by XRD measurement (Table 12). The meanings of symbols, abbreviations, etc. are the same as those in the case of using a microreactor.
[0407] According to the above experimental results, similarly to Example C in which the above microreactor was used, even in the case of the batch method, in the case where the solvent (simply described as solvent in Table 12) having a partial solubility for the cyan organic pigment particles did not contain a surfactant and a dispersant in step 2, particle growth and necking occurred. As an example, a TEM observation photograph of the copper-titanyl-cobalt phthalocyanine particles obtained in Experiment No. 4-4 is shown in FIG. Fig.36 On the other hand, when the production method of the present invention is applied to Example C, it can be seen that the obtained cyan organic pigment fine particles can suppress necking and growth due to the effect of the particle property control solution.
[0408] As described above, Example A, Example B, and Example C show that the present invention is effective for all organic particles.
[0409] Explanation of symbols
[0410] 1. First treatment surface
[0411] 2 Second treatment surface
[0412] 10 First processing part
[0413] 11. Bracket 1
[0414] 20 Second processing unit
[0415] 21 No. 2 Bracket
[0416] d1 First induction section
[0417] d2 2nd introduction section
[0418] d10 opening
[0419] d20 opening
Claims
1. A method for producing organic microparticles, characterized in that: include: Step 1 of preparing organic fine particles, at least a portion of which includes amorphous organic matter, as a treatment object; and Step 2 of preparing a particle property control solution in which a surfactant is added to a solvent having a partial solubility for the organic particles, and allowing the particle property control solution to act on the organic particles, The solubility of the organic particles in the solvent having a partial solubility is 1 μg / g or more and 1000 μg / g or less, The step 2 acts to improve the crystallinity of the organic particles or to cause the organic particles to undergo a crystal transformation. When the particle size of the organic particles after the particle property control solution acts on the organic particles is taken as (A) and the particle size of the organic particles before the particle property control solution acts on the organic particles is taken as (B), the particle size change rate of the organic particles, i.e., (A) / (B), is 1 to 4, The organic particles are particles of indomethacin, curcumin or pirenoxine, The solvent is pentane, hexane, heptane, octane, nonane, decane, undecane, cyclohexane or water, The surfactant is one or two selected from polyvinyl pyrrolidone, polyvinyl alcohol, hydroxypropyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, methyl cellulose, Span80, Lutrol F127, Tween80, polyoxyethylene solidified castor oil, and benzalkonium chloride.
2. A method for producing organic microparticles, characterized in that: include: Step 1 of preparing organic fine particles, at least a portion of which includes amorphous organic matter, as a treatment object; and Step 2 of preparing a particle property control solution in which a surfactant is added to a solvent having a partial solubility for the organic particles, and allowing the particle property control solution to act on the organic particles, The solubility of the organic particles in the solvent having a partial solubility is 1 μg / g or more and 1000 μg / g or less, The step 2 acts to improve the crystallinity of the organic particles or to cause the organic particles to undergo a crystal transformation. When the particle size of the organic particles after the particle property control solution acts on the organic particles is taken as (A) and the particle size of the organic particles before the particle property control solution acts on the organic particles is taken as (B), the particle size change rate of the organic particles, i.e., (A) / (B), is 1 to 4, The organic particles are polypropylene particles, The solvent is methanol, isopropanol, isopropanol aqueous solution, toluene or xylene, The surfactant is Tween80.
3. A method for producing organic microparticles, characterized in that: include: Step 1 of preparing organic fine particles, at least a portion of which includes amorphous organic matter, as a treatment object; and Step 2 of preparing a particle property control solution in which a surfactant is added to a solvent having a partial solubility for the organic particles, and allowing the particle property control solution to act on the organic particles, The solubility of the organic particles in the solvent having a partial solubility is 1 μg / g or more and 1000 μg / g or less, The step 2 acts to improve the crystallinity of the organic particles and / or to cause the organic particles to undergo a crystal transformation. When the particle size of the organic particles after the particle property control solution acts on the organic particles is taken as (A) and the particle size of the organic particles before the particle property control solution acts on the organic particles is taken as (B), the particle size change rate of the organic particles, i.e., (A) / (B), is 1 to 4, The organic particles are particles of organic pigments, The surfactant is selected from acrylic acid polymers, high molecular block copolymers, carboxylates containing hydroxyl groups, sodium dialkyl sulfosuccinates, and sodium dodecylbenzene sulfonate. The combination of the organic pigment particles and the solvent is at least one selected from the following first to third combinations, The first combination: the organic pigment particles are CI Pigment Red 254 particles, and the solvent is a combination of propylene glycol monomethyl ether acetate, methanol or toluene; The second combination: the organic pigment particles are CI Pigment Red 122 particles, and the solvent is isopropyl alcohol; The third combination: the organic pigment particles are copper-titanium-cobalt phthalocyanine particles, and the solvent is styrene, tetrahydrofuran or isopropyl alcohol.
4. The method for producing organic microparticles according to any one of claims 1 to 3, characterized in that: The step 1 is a step of mixing a raw material solution of organic particles with a precipitation solvent L for precipitating at least one type of organic particles from the raw material solution of organic particles to precipitate organic particles (P1) containing amorphous organic particles in at least a part thereof; and Step 2 is a step of allowing the particle property control solution to act on the organic fine particles (P1).
5. The method for producing organic microparticles according to claim 4, characterized in that: The method comprises a step c of washing and / or replacing the solvent of the organic fine particles (P1) obtained in the step 1, wherein the particle property control solution is allowed to act on the organic fine particles (P2) obtained in the step c.
6. The method for producing organic microparticles according to any one of claims 1 to 3, characterized in that: When the particle property control solution is allowed to act on the organic fine particles, a stirring process is performed, and the properties of the organic fine particles are controlled by the stirring energy.
7. The method for producing organic microparticles according to claim 4, characterized in that: When the particle property control solution is allowed to act on the organic fine particles, a stirring process is performed, and the properties of the organic fine particles (P1) are controlled by the stirring energy.
8. The method for producing organic microparticles according to claim 5, characterized in that: When the particle property control solution is allowed to act on the organic fine particles, a stirring process is performed, and the properties of the organic fine particles (P2) are controlled by the stirring energy.
9. The method for producing organic microparticles according to claim 4, characterized in that: The process 1 is as follows: Introducing at least two kinds of processed fluids including a raw material solution of organic particles and a precipitation solvent L into between a first processing surface and a second processing surface which are disposed opposite to each other in a manner that allows access and separation, and at least one of which is relatively rotatable relative to the other; By applying an introduction pressure between the first processing surface and the second processing surface, a separation force acting in a direction to separate the first processing surface from the second processing surface is generated; The separation force is used to maintain a small gap between the first processing surface and the second processing surface, and the at least two processed fluids are combined between the first processing surface and the second processing surface maintained at the small gap; Passing between the first processing surface and the second processing surface, thereby forming a thin film fluid; The process is carried out in a microreactor in which the treated fluids react with each other in the thin film fluid.
10. The method for producing organic microparticles according to claim 5, characterized in that: The process 1 is as follows: Introducing at least two kinds of processed fluids including a raw material solution of organic particles and a precipitation solvent L into between a first processing surface and a second processing surface which are disposed opposite to each other in a manner that allows access and separation, and at least one of which is relatively rotatable relative to the other; By applying an introduction pressure between the first processing surface and the second processing surface, a separation force acting in a direction to separate the first processing surface from the second processing surface is generated; The separation force is used to maintain a small gap between the first processing surface and the second processing surface, and the at least two processed fluids are combined between the first processing surface and the second processing surface maintained at the small gap; Passing between the first processing surface and the second processing surface, thereby forming a thin film fluid; The process is carried out in a microreactor in which the treated fluids react with each other in the thin film fluid.
11. The method for producing organic microparticles according to claim 6, characterized in that: The stirring is performed using a stirrer equipped with a rotating stirring blade.
12. The method for producing organic microparticles according to claim 7, characterized in that: The stirring is performed using a stirrer equipped with a rotating stirring blade.
13. The method for producing organic microparticles according to claim 8, characterized in that: The stirring is performed using a stirrer equipped with a rotating stirring blade.
14. The method for producing organic microparticles according to any one of claims 1 to 3, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
15. The method for producing organic microparticles according to claim 4, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
16. The method for producing organic microparticles according to claim 5, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
17. The method for producing organic microparticles according to claim 6, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
18. The method for producing organic microparticles according to claim 7, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
19. The method for producing organic microparticles according to claim 8, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
20. The method for producing organic microparticles according to claim 9, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
21. The method for producing organic microparticles according to claim 10, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
22. The method for producing organic microparticles according to claim 11, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
23. The method for producing organic microparticles according to claim 12, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
24. The method for producing organic microparticles according to claim 13, characterized in that: The particle diameter of the organic fine particles before and after the particle shape control solution is allowed to act on the organic fine particles is 100 nm or less.
25. The method for producing organic microparticles according to claim 4, characterized in that: The particle size of the organic particles (P1) is less than 30 nm.
26. The method for producing organic microparticles according to claim 5, characterized in that: The particle size of the organic particles (P1) is less than 30 nm.
27. The method for producing organic microparticles according to claim 3, characterized in that: The particle shape controlling solution does not contain any pigment derivative.
28. A method for modifying organic particles, characterized in that: include: Step 1 of preparing organic fine particles at least part of which contain amorphous substances as a treatment object; and Step 2 of allowing a particle property control solution prepared by adding a surfactant to a solvent having a partial solubility for the organic particles to act on the organic particles, The solubility of the organic particles in the solvent having a partial solubility is 1 μg / g or more and 1000 μg / g or less, When the particle size of the organic particles after the particle property control solution acts on the organic particles is taken as (A) and the particle size of the organic particles before the particle property control solution acts on the organic particles is taken as (B), the particle size change rate of the organic particles, i.e., (A) / (B), is 1 to 4, The crystallinity of the organic particles is increased by step 2, thereby modifying the organic particles into organic particles having a crystallinity that matches the target setting conditions, or the crystal form of the organic particles is changed by step 2, thereby modifying the organic particles into organic particles having a crystal form that matches the target setting conditions, The organic particles are particles of indomethacin, curcumin or pirenoxine, The solvent is pentane, hexane, heptane, octane, nonane, decane, undecane, cyclohexane or water, The surfactant is one or two selected from polyvinyl pyrrolidone, polyvinyl alcohol, hydroxypropyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, methyl cellulose, Span80, Lutrol F127, Tween80, polyoxyethylene solidified castor oil, and benzalkonium chloride.
29. A method for modifying organic particles, characterized in that: include: Step 1 of preparing organic fine particles at least part of which contain amorphous substances as a treatment object; and Step 2 of allowing a particle property control solution prepared by adding a surfactant to a solvent having a partial solubility for the organic particles to act on the organic particles, The solubility of the organic particles in the solvent having a partial solubility is 1 μg / g or more and 1000 μg / g or less, When the particle size of the organic particles after the particle property control solution acts on the organic particles is taken as (A) and the particle size of the organic particles before the particle property control solution acts on the organic particles is taken as (B), the particle size change rate of the organic particles, i.e., (A) / (B), is 1 to 4, The crystallinity of the organic particles is increased by step 2, thereby modifying the organic particles into organic particles having a crystallinity that matches the target setting conditions, or the crystal form of the organic particles is changed by step 2, thereby modifying the organic particles into organic particles having a crystal form that matches the target setting conditions, The organic particles are polypropylene particles, The solvent is methanol, isopropanol, isopropanol aqueous solution, toluene or xylene, The surfactant is Tween80.
30. A method for modifying organic particles, characterized in that: include: Step 1 of preparing organic fine particles at least part of which contain amorphous substances as a treatment object; and Step 2 of allowing a particle property control solution prepared by adding a surfactant to a solvent having a partial solubility for the organic particles to act on the organic particles, The solubility of the organic particles in the solvent having a partial solubility is 1 μg / g or more and 1000 μg / g or less, When the particle size of the organic particles after the particle property control solution acts on the organic particles is taken as (A) and the particle size of the organic particles before the particle property control solution acts on the organic particles is taken as (B), the particle size change rate of the organic particles, i.e., (A) / (B), is 1 to 4, The crystallinity of the organic particles is improved by step 2, thereby modifying the organic particles into organic particles having a crystallinity that matches the target setting conditions, and / or the crystal form of the organic particles is changed by step 2, thereby modifying the organic particles into organic particles having a crystal form that matches the target setting conditions, The organic particles are particles of organic pigments, The surfactant is selected from acrylic acid polymers, high molecular block copolymers, carboxylates containing hydroxyl groups, sodium dialkyl sulfosuccinates, and sodium dodecylbenzene sulfonate. The combination of the organic pigment particles and the solvent is at least one selected from the following first to third combinations, The first combination: the organic pigment particles are CI Pigment Red 254 particles, and the solvent is a combination of propylene glycol monomethyl ether acetate, methanol or toluene; The second combination: the organic pigment particles are CI Pigment Red 122 particles, and the solvent is isopropyl alcohol; The third combination: the organic pigment particles are copper-titanium-cobalt phthalocyanine particles, and the solvent is styrene, tetrahydrofuran or isopropyl alcohol.