Non-aqueous electrolyte secondary battery
By using a layered lithium transition metal composite oxide and a high-concentration amorphous tungsten concentrated layer in the positive electrode active substance of a nonaqueous electrolyte secondary battery, combined with the design of lithium tungsten compound particles, the positive electrode active substance in the prior art is solved. Inadequate output characteristics and durability achieves more efficient battery performance.
Patent Information
- Application Number
- CN202010680697.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-18
- Filing Date
- 2020-07-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-07-15
AI Technical Summary
The positive electrode active substance of the conventional non-aqueous electrolyte secondary battery has room for improvement in improving output characteristics and durability, especially the positive electrode active substance containing tungsten has limited effect in reducing the positive electrode resistance.
Using lithium transition metal composite oxide containing layered structure as the core, a high concentration of amorphous tungsten concentrated layer is formed on the surface, and lithium tungsten compound particles are attached. Through these structures, deterioration caused by oxygen detachment and electrolyte contact is suppressed, and Li ions are improved. diffusivity and resistance reduction.
It is possible to ensure durability and significantly improve output characteristics in a nonaqueous electrolyte secondary battery, and to enhance the overall performance of the battery by suppressing the deterioration of the positive electrode active material and reducing the positive electrode resistance.
Smart Images

Figure CN112242522B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a nonaqueous electrolyte secondary battery. Background Art
[0002] In recent years, nonaqueous electrolyte secondary batteries such as lithium ion secondary batteries have been suitably used as portable power sources such as personal computers and portable terminals, and vehicle driving power sources such as electric vehicles (EVs), hybrid vehicles (HVs), and plug-in hybrid vehicles (PHVs).
[0003] Generally, a positive electrode active material that can absorb and release ions that become charge carriers is used in the positive electrode of a non-aqueous electrolyte secondary battery. As an example of a positive electrode active material, a lithium transition metal composite oxide having a layered structure can be cited (for example, refer to Patent Documents 1 and 2). For example, Patent Document 1 uses a positive electrode active material in which a lithium tungsten compound (LW compound) is present in a layered lithium transition metal composite oxide. This can reduce the positive electrode resistance, improve output characteristics, etc. In addition, Patent Document 2 discloses a technology for forming a tungsten concentration layer on the surface of a metal composite hydroxide that is a precursor of a lithium transition metal composite oxide. Thus, a positive electrode active material (lithium transition metal composite oxide) having high output characteristics and high crystallinity can be generated.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2017-84628
[0007] Patent Document 2: Japanese Patent Application Publication No. 2019-19047 Summary of the invention
[0008] Problems to be solved by the invention
[0009] In recent years, the demand for improving the performance of non-aqueous electrolyte secondary batteries has been increasing, and it is necessary to develop positive electrode active materials that can exert performance that exceeds that of previous technologies. According to this requirement, the inventors conducted in-depth research and found that the positive electrode active materials containing tungsten (W) can exert an effect above a certain level in reducing the positive electrode resistance and thus improving the output characteristics, but there is still room for improvement.
[0010] The present invention has been made in response to the above-mentioned needs, and an object of the present invention is to ensure predetermined durability and to exhibit excellent output characteristics in a non-aqueous electrolyte secondary battery using a positive electrode active material containing tungsten.
[0011] Means for solving problems
[0012] The nonaqueous electrolyte secondary battery disclosed herein comprises a positive electrode, a negative electrode and a nonaqueous electrolyte. The positive electrode of the nonaqueous electrolyte secondary battery comprises a positive electrode active material layer containing a granular positive electrode active material. The positive electrode active material comprises: a core portion containing a layered lithium transition metal composite oxide, a W concentration layer formed on the surface of the core portion and confirmed to have a higher concentration of tungsten than the core portion in TEM-EDX analysis, and LW compound particles attached to at least a portion of the surface of the W concentration layer and containing lithium and tungsten. Moreover, in the nonaqueous electrolyte secondary battery disclosed herein, the W concentration layer has an amorphous structure.
[0013] According to the above configuration, it is possible to ensure predetermined durability and exhibit excellent output characteristics. The reason for achieving this effect is considered to be as follows.
[0014] First, since a W concentration layer is formed on the surface of the core, it is possible to suppress the degradation caused by the separation of oxygen from the core (lithium transition metal composite oxide with a layered structure). In addition, the LW compound attached to the surface of the W concentration layer can suppress the degradation caused by contact with the non-aqueous electrolyte. Therefore, in the non-aqueous electrolyte secondary battery disclosed herein, the degradation of the positive electrode active material is appropriately suppressed, so that the durability above a certain level can be ensured.
[0015] Secondly, in addition to the above-mentioned inhibition of core degradation, the W concentration layer also has the function of improving the solid diffusion at the surface of the active material, and can also contribute to the improvement of the diffusivity of Li ions in the positive electrode. In addition, the LW compound has the function of increasing the Li ion concentration at the surface of the positive electrode active material. Utilizing these functions, the output improvement effect caused by the reduction of positive electrode resistance is exerted.
[0016] In addition, in the battery disclosed herein, the W concentration layer is amorphized. As a result, the active sites on the surface of the active material increase, and the insertion and extraction of Li ions in the positive electrode are greatly improved. As a result, the positive electrode resistance is further reduced, and excellent output characteristics can be exerted.
[0017] In a preferred embodiment of the nonaqueous electrolyte secondary battery disclosed herein, the atomic concentration of tungsten in the W concentrated layer is 1 atomic % or more and 3.6 atomic % or less. This allows both durability and output characteristics to be achieved at a higher level.
[0018] In a preferred embodiment of the nonaqueous electrolyte secondary battery disclosed herein, the atomic concentration of tungsten in the core portion is 0.3 atomic % or less. This can further improve durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a cross-sectional view schematically showing the internal structure of a lithium ion secondary battery according to one embodiment of the present invention.
[0020] Figure 2 This is a schematic diagram showing the structure of a wound electrode body of a lithium ion secondary battery according to one embodiment of the present invention.
[0021] Figure 3 This is a cross-sectional view schematically showing an example of a positive electrode active material used in a lithium ion secondary battery according to an embodiment of the present invention.
[0022] Description of Reference Numerals
[0023] 10. Positive electrode active material
[0024] 12 Nuclear
[0025] 14 W Concentrated layer
[0026] 16 LW compound particles
[0027] 20 Wound electrode body
[0028] 30 Battery housing
[0029] 36 Safety valve
[0030] 42 Positive terminal
[0031] 42a Positive electrode collector plate
[0032] 44 Negative terminal
[0033] 44a Negative collector plate
[0034] 50 positive electrode sheet (positive electrode)
[0035] 52 positive electrode collector
[0036] 52a Positive electrode active material layer not formed portion
[0037] 54 Positive electrode active material layer
[0038] 60 negative electrode sheet (negative electrode)
[0039] 62 negative electrode collector
[0040] 62a Negative electrode active material layer not formed part
[0041] 64 Negative electrode active material layer
[0042] 70 separator
[0043] 100 Lithium-ion secondary battery DETAILED DESCRIPTION
[0044] As an embodiment of the non-aqueous electrolyte secondary battery of the present invention, the lithium ion secondary battery is described with reference to the accompanying drawings. It should be noted that matters other than those specifically mentioned in this specification and necessary for the implementation of the present invention (such as the general structure and manufacturing process of the non-aqueous electrolyte secondary battery that does not characterize the present invention) can be grasped as design matters for those skilled in the art based on the prior art in this field. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in this field. In addition, in the following drawings, the same figure marks are marked on the components and parts that play the same role for explanation. In addition, the dimensional relationships (length, width, thickness, etc.) in each figure do not reflect the actual dimensional relationships.
[0045] In addition, the "secondary battery" in this specification refers to a general power storage device that can be repeatedly charged and discharged, and is a term that includes power storage elements such as so-called storage batteries and electric double layer capacitors.
[0046] 1. Lithium-ion secondary battery
[0047] Hereinafter, a flat rectangular lithium ion secondary battery having a flat wound electrode body and a flat battery case will be described as one embodiment of the present invention, but the present invention is not intended to be limited to the contents described in this embodiment.
[0048] (1) Overall structure
[0049] Figure 1 It is a cross-sectional view schematically showing the internal structure of the lithium ion secondary battery 100 according to the present embodiment. Figure 1 The lithium-ion secondary battery 100 shown in the figure is constructed by accommodating a flat-shaped wound electrode body 20 and a non-aqueous electrolyte (not shown) in a flat square battery case (i.e., an outer packaging container) 30. As the material of the battery case 30, a metal material such as aluminum, which is lightweight and has good thermal conductivity, is used. In addition, in the battery case 30, a positive terminal 42 and a negative terminal 44 are provided as external connection terminals. The positive terminal 42 is electrically connected to the positive electrode collector plate 42a. The negative terminal 44 is electrically connected to the negative electrode collector plate 44a. Furthermore, in the battery case 30, a safety valve 36 for suppressing deformation of the shell when the internal pressure rises and an injection port (omitted from the figure) for injecting the non-aqueous electrolyte are also provided.
[0050] Figure 2 Schematic diagram showing the structure of the wound electrode body 20 of the lithium ion secondary battery 100 according to the present embodiment. Figure 1 and Figure 2As shown in , the wound electrode body 20 is formed by winding a stacked body formed by overlapping a long positive electrode sheet 50 and a negative electrode sheet 60 via two long separators 70. The positive electrode sheet 50 includes a long foil-shaped positive electrode collector 52 (for example, aluminum foil) and a positive electrode active material layer 54 provided on the surface (for example, both sides) of the positive electrode collector 52. The negative electrode sheet 60 includes a long foil-shaped negative electrode collector 62 (for example, copper foil) and a negative electrode active material layer 64 provided on the surface (for example, both sides) of the negative electrode collector 62.
[0051] In addition, a portion (positive electrode active material layer non-formed portion 52a) is formed at one side edge portion in the width direction of the positive electrode sheet 50, where the positive electrode active material layer 54 is not provided and the positive electrode current collector 52 is exposed. On the other hand, a portion (negative electrode active material layer non-formed portion 62a) is formed at the other side edge portion in the width direction of the negative electrode sheet 60, where the negative electrode active material layer 64 is not provided and the negative electrode current collector 62 is exposed. Moreover, in the present embodiment, after the positive electrode sheet 50 and the negative electrode sheet 60 are stacked in such a manner that the positive electrode active material layer non-formed portion 52a extends from one side edge portion and the negative electrode active material layer non-formed portion 62a extends from the other side edge portion, the stacked body is wound. Furthermore, as Figure 1 As shown in FIG. 1 , the positive electrode current collector plate 42 a is joined to the portion 52 a without the positive electrode active material layer formed after winding, and the negative electrode current collector plate 44 a is joined to the portion 62 a without the negative electrode active material layer formed after winding.
[0052] The positive electrode active material layer 54 in this embodiment contains Figure 3 The positive electrode active material 10 shown in . The positive electrode active material 10 will be described in detail later. Furthermore, although there is no particular limitation, the content of the positive electrode active material in the positive electrode active material layer 54 (ie, relative to the total mass of the positive electrode active material layer 54) is preferably 70% by mass or more, and more preferably 80% by mass or more. In addition, the positive electrode active material layer 54 may further include components other than the positive electrode active material 10, such as trilithium phosphate, a conductive material, a binder, and the like. As a conductive material, for example, carbon black such as acetylene black (AB) and other carbon materials (such as graphite, etc.) can be preferably used. As a binder, for example, polyvinylidene fluoride (PVDF) and the like can be used. Without intending to limit the present invention, in the case of adding trilithium phosphate to the positive electrode active material layer 54, the content of the trilithium phosphate is preferably 1% by mass or more and 15% by mass or less, and more preferably 2% by mass or more and 12% by mass or less. In addition, in the case of adding a conductive material, the content of the conductive material is preferably 1% by mass or more and 15% by mass or less, and more preferably 3% by mass or more and 13% by mass or less. When a binder is added, the content of the binder is preferably 1% by mass or more and 15% by mass or less, and more preferably 1.5% by mass or more and 10% by mass or less.
[0053] On the other hand, the negative electrode active material layer 64 contains a granular negative electrode active material. As the negative electrode active material, for example, carbon materials such as graphite, hard carbon, and soft carbon can be used. Graphite can be natural graphite, artificial graphite, or amorphous carbon-coated graphite in the form of graphite coated with an amorphous carbon material. Although there is no particular limitation, the content of the negative electrode active material in the negative electrode active material layer is preferably 90% by mass or more, more preferably 95% by mass or more and 99% by mass or less. In addition, the negative electrode active material layer 64 may contain components other than the negative electrode active material, such as a binder and a thickener. As a binder, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), etc. can be used. As a thickener, for example, carboxymethyl cellulose (CMC) can be used. Without intending to limit the present invention, when a binder is added to the negative electrode active material layer 64, the content of the binder is preferably 0.1% by mass or more and 8% by mass or less, more preferably 0.5% by mass or more and 3% by mass or less. Moreover, when a thickener is added, the content of the thickener is preferably 0.3 mass % or more and 3 mass % or less, and more preferably 0.5 mass % or more and 2 mass % or less.
[0054] For the separator 70, an insulating sheet having fine pores through which charge carriers (e.g., lithium ions) can be used. For the separator 70, for example, a porous sheet (membrane) made of a resin such as polyethylene (PE), polypropylene (PP), polyester, cellulose, polyamide, etc. can be used. In addition, the separator 70 can be a single-layer structure, or a multilayer structure in which two or more layers are stacked. As an example of the separator 70 of a multilayer structure, a separator of a three-layer structure in which PP layers are stacked on both sides of a PE layer can be cited. In addition, a heat-resistant layer (HRL) can be provided on the surface of the separator 70.
[0055] The nonaqueous electrolyte typically contains a nonaqueous solvent and a supporting salt.
[0056] As non-aqueous solvent, organic solvents such as various carbonates, ethers, esters, nitrile, sulfones, lactones used in the electrolyte of general lithium ion secondary battery can be used without particular limitation. As specific example, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), trifluorodimethyl carbonate (TFDMC) etc. can be illustrated. Such non-aqueous solvent can be used alone as one, or two or more kinds can be suitably used in combination.
[0057] As the supporting salt, for example, lithium salts such as LiPF6, LiBF4, and lithium bis(fluorosulfonyl)imide (LiFSI) (preferably LiPF6) can be preferably used. The concentration of the supporting salt is preferably 0.7 mol / L or more and 1.3 mol / L or less.
[0058] Furthermore, as long as the effect of the present invention is not significantly impaired, the non-aqueous electrolyte may contain components other than the above components. As components (additives) that can be added to the non-aqueous electrolyte, for example, gas generating agents such as biphenyl (BP) and cyclohexylbenzene (CHB) and thickeners can be listed.
[0059] (2) Positive electrode active material
[0060] Next, the positive electrode active material used in this embodiment will be described. Figure 3 1 is a cross-sectional view schematically showing an example of a positive electrode active material 10 used in a lithium ion secondary battery 100 according to the present embodiment. Figure 3 As shown in FIG. 1 , the positive electrode active material 10 includes a core portion 12, a tungsten concentrated layer (W concentrated layer) 14, and lithium tungsten compound particles (LW compound particles) 16. Each of these will be described below.
[0061] (a) Nuclear Department
[0062] The core 12 is a particle containing a layered structure of a lithium transition metal composite oxide. The lithium transition metal composite oxide is a metal oxide containing at least lithium (Li) and a transition metal element constituting a layered structure. Examples of the lithium transition metal composite oxide include lithium nickel composite oxides, lithium manganese composite oxides, lithium cobalt composite oxides, lithium nickel cobalt aluminum composite oxides, lithium iron nickel manganese composite oxides, and lithium nickel cobalt manganese composite oxides. Among these, lithium nickel cobalt manganese composite oxides can exert particularly excellent output characteristics, so they are preferred. It should be noted that the so-called "lithium nickel cobalt manganese composite oxide" in this specification is not limited to metal oxides with only Li, Ni, Co, Mn, and O as constituent elements, but also includes oxides containing additive elements other than Li, Ni, Co, Mn, and O. At this time, as additive elements, for example, metal elements such as W, Mg, Ca, Al, Ti, V, Cr, Si, Y, Zr, Nb, Mo, Hf, Ta, Na, Fe, Zn, and Sn can be listed. In addition, the additive elements may also include semi-metallic elements such as B, C, Si, and P, and non-metallic elements such as S, F, Cl, Br, and I. Furthermore, the content of the additive element relative to lithium in the core portion 12 is preferably 0.1 mol or less. This is not limited to lithium nickel cobalt manganese composite oxides, and the same is true when other lithium transition metal composite oxides (lithium nickel composite oxides, lithium cobalt composite oxides, lithium manganese composite oxides, lithium nickel cobalt aluminum composite oxides, lithium iron nickel manganese composite oxides, etc.) are used as the core portion 12.
[0063] In addition, from the viewpoint of improving output characteristics and durability, tungsten (W) is particularly preferred as an additive element in the core portion 12. On the other hand, when the W content in the core portion 12 increases excessively, it becomes a cause of increased dissolution of the constituent elements in a high temperature environment, and durability may be reduced instead. Considering this point, the upper limit of the atomic concentration (B) of tungsten in the core portion 12 is preferably 0.4 atomic % or less, more preferably 0.3 atomic % or less, and particularly preferably 0.2 atomic % or less. On the other hand, the presence or absence of W in the core portion 12 does not limit the present invention. That is, the atomic concentration (B) of tungsten in the core portion 12 can be 0 atomic %. However, considering the output characteristics and durability, the atomic concentration (B) of tungsten in the core portion 12 is preferably 0.01 atomic % or more, more preferably 0.05 atomic % or more, and particularly preferably 0.1 atomic % or more.
[0064] It should be noted that the "atomic concentration of tungsten in the core (B)" in this specification is measured based on the following steps. First, a plurality of (e.g., 20) arbitrary positive electrode active materials 10 are photographed using TEM-EDX, and a region with a radius of 3 nm centered on a position 100 nm inward in the radial direction from the surface of the W concentration layer 14 described later is set as the measurement region ( Figure 3 M B ). Next, a plurality of (for example, five) measurement regions M are set in each of the positive electrode active materials 10 to be measured. B , measure each measurement area M B The "atomic number of tungsten (W)" and the "atomic number of transition metal elements (such as Ni, Co, Mn, W, etc.)" are calculated. Then, the ratio of the total number of W atoms when the total number of transition metal atoms measured in each measurement area is set to 100 atomic % is calculated, so that the "atomic concentration of tungsten in the core (B)" can be measured.
[0065] In addition, although there is no particular limitation, the average particle size (median diameter: D50) of the core portion 12 is preferably, for example, 20 μm or less, more preferably 15 μm or less, and further preferably 10 μm or less. In this way, the specific surface area of the core portion 12 can be ensured, and the positive electrode resistance can be further reduced. On the other hand, from the viewpoint of suppressing the formation of coarse secondary particles caused by the aggregation of the core portions 12, the lower limit of the average particle size of the core portion 12 is preferably 0.1 μm or more, more preferably 0.5 μm or more, and further preferably 3 μm or more. It should be noted that the "average particle size" in this specification can be obtained, for example, by obtaining a cross-sectional TEM image of the positive electrode active material layer 54, arbitrarily selecting more than 20 positive electrode active materials 10 in the cross-sectional TEM image, and calculating the average value of the particle size of the measurement object (such as the core portion) confirmed by the selected positive electrode active material 10. It should be noted that in the cross-sectional TEM image, the core portion 12 is observed as a particle in which a layered crystal structure is confirmed.
[0066] Furthermore, the core 12 can be prepared by any known method used in the preparation of particles of lithium transition metal composite oxides without particular limitation. For example, a precursor of lithium transition metal composite oxide (e.g., metal hydroxide) is generated by a crystallization method, and lithium is introduced into the precursor, thereby forming the core 12 of lithium transition metal composite oxide containing a layered structure.
[0067] (b) W concentration layer
[0068] like Figure 3 As shown in , the positive electrode active material 10 in this embodiment has a W concentration layer 14 formed on the surface of the core part 12, in which the tungsten concentration is higher than that of the core part 12. Typically, the W concentration layer 14 is composed of a metal oxide containing lithium (Li), tungsten (W) and other elements. The "other elements" in the W concentration layer 14 may be the same elements as the constituent elements of the core part 12 described above. That is, in addition to Li and W, the W concentration layer 14 may contain Ni, Co, Mn, Mg, Ca, Al, Ti, V, Cr, Si, Y, Zr, Nb, Mo, Hf, Ta, Na, Fe, Zn, Sn, B, C, Si, P, S, F, Cl, etc. In addition, the constituent elements of the W concentration layer 14 do not have to be the same as the constituent elements of the core part 12, and can be appropriately changed. For example, when the core portion 12 is formed of a lithium nickel cobalt manganese composite oxide containing W, the W concentrated layer 14 may be formed of a lithium nickel cobalt manganese composite oxide containing W, or may be formed of a lithium nickel composite oxide containing W, a lithium manganese composite oxide containing W, a lithium cobalt composite oxide containing W, a lithium nickel cobalt aluminum composite oxide containing W, or a lithium iron nickel manganese composite oxide containing W. However, considering the ease of formation on the surface of the core portion 12, it is preferred that the constituent elements of the W concentrated layer 14 are the same as those of the core portion 12.
[0069] Moreover, a higher concentration of W is confirmed in the W concentrated layer 14 than in the core 12. In other words, in the positive electrode active material 10 in the present embodiment, the atomic concentration (A) of W in the W concentrated layer 14 is higher than the atomic concentration (B) of W in the core 12 described above (A>B). By forming the W concentrated layer 14 on the surface of the core 12 in this way, the deterioration of the positive electrode active material 10 caused by the separation of oxygen from the core 12 can be prevented, and the durability of the battery can be improved. In addition, the W concentrated layer 14 can improve the solid diffusion at the surface of the positive electrode active material 10 and improve the diffusivity of Li ions, so it can also contribute to reducing the positive electrode resistance.
[0070] It should be noted that the "atomic concentration of W in the W concentrated layer (A)" in this specification can be measured by the same procedure as the "atomic concentration of W in the core (B)" described above. That is, a plurality of (e.g., 20) positive electrode active materials 10 are photographed using TEM-EDX, and a plurality of measurement regions M are set near the surface of each positive electrode active material 10. A , measure the multiple measurement areas M A The atomic concentration of W in the W concentrated layer (atom %) is then averaged. A This is a region with a radius of 3 nm centered at a position 5 nm inward in the radial direction from the surface of the W concentration layer 14 .
[0071] In addition, from the viewpoint of more appropriately exerting the resistance reduction effect, the atomic concentration (A) of W in the W concentration layer 14 is preferably 0.5 atomic % or more, and more preferably 0.8 atomic % or more. In particular, when the atomic concentration (A) of W in the W concentration layer 14 is 1 atomic % or more, it is confirmed that the positive electrode resistance is greatly reduced. On the other hand, from the viewpoint of suppressing the reduction in durability caused by the dissolution of the constituent elements, the upper limit of the atomic concentration (A) of W in the W concentration layer 14 is preferably 3.6 atomic % or less, more preferably 3.3 atomic % or less, and particularly preferably 2.6 atomic % or less.
[0072] In addition, in the present embodiment, in order to further reduce the positive electrode resistance, the W concentration layer 14 is made amorphous. It has been confirmed through experiments that by forming a W concentration layer 14 having such an amorphous structure on the surface of the positive electrode active material 10, excellent output characteristics can be exerted. Without intending to limit the present invention, it is speculated that such an effect is exerted through the following effects. The surface of a general positive electrode active material is composed of a lithium transition metal composite oxide with a layered structure. In such a lithium transition metal composite oxide with a layered structure, the insertion and separation of Li ions occur between the layers of the crystal structure, so the direction and location of the insertion and separation of Li ions at the surface of the particle are limited. In the present embodiment, since the W concentration layer 14 with an amorphous structure that does not have an ordered crystal structure is formed on the surface of the particle, the active points at the surface of the particle increase, and the insertion and separation of Li ions become smooth. As a result, the positive electrode resistance is greatly reduced, so that excellent output characteristics can be exerted.
[0073] It should be noted that the so-called "amorphous structure" in this specification refers to a structure in a state in which a clear crystal structure cannot be confirmed in crystal analysis using electron diffraction. For example, when observing the electron diffraction image of the positive electrode active material, when a halo image indicating amorphization is observed in the W concentrated layer 14, it can be said that the W concentrated layer 14 has an amorphous structure.
[0074] In addition, there is no particular limitation on the thickness of the W concentrated layer 14, which may be 100 nm or less. Furthermore, if the durability reduction caused by the increase in the W concentration in the entire positive electrode active material 10 is taken into consideration, the thickness of the W concentrated layer 14 is preferably 80 nm or less, more preferably 70 nm or less, further preferably 60 nm or less, and particularly preferably 50 nm or less. On the other hand, from the perspective of appropriately exerting the durability improvement effect and resistance reduction effect produced by the W concentrated layer 14, the lower limit of the thickness of the W concentrated layer 14 is preferably 10 nm or more, more preferably 20 nm or more, further preferably 30 nm or more, and particularly preferably 40 nm or more. Furthermore, the thickness of the W concentrated layer 14 can be obtained, for example, by obtaining a cross-sectional TEM image of the positive electrode active material layer 54, arbitrarily selecting more than 20 positive electrode active materials 10 in the cross-sectional TEM image, and calculating the average value of the thickness of the W concentrated layer 14 of the selected positive electrode active material 10.
[0075] In addition, without limiting the present invention, the W concentration layer 14 having an amorphous structure can be formed, for example, by physical impact using a sputtering method. Specifically, the precursor of the core portion 12 is dispersed in a solution having a higher W composition ratio (e.g., W / (W+Ni+Co+Mn)) than the solution used to generate the core portion 12, and a crystallization method is performed in this state, thereby generating precursor particles of the precursor of the W concentration layer 14 formed on the surface of the precursor of the core portion 12. Then, by sintering the precursor particles together with a lithium compound, lithium is introduced, thereby forming a W concentration layer having a layered structure on the surface of the core portion. Then, by using a sputtering method, tungsten oxide (WO3) is collided with the W concentration layer having a layered structure, and the crystal structure of the W concentration layer is destroyed, thereby obtaining core-shell particles having an amorphous W concentration layer 14 formed on the surface of the core portion 12 having a layered structure.
[0076] (c) LW compound particles
[0077] Next, in the positive electrode active material 10 in the present embodiment, LW compound particles 16 are attached to at least a portion of the surface of the W concentration layer 14. Thus, the degradation of the core portion 12 caused by contact with the non-aqueous electrolyte can be suppressed, and thus it can contribute to the improvement of durability. In addition, the LW compound particles 16 also have the function of increasing the Li ion concentration at the surface of the positive electrode active material 10. In addition, it also has the function of increasing the Li ion conductivity at the surface of the positive electrode active material 10. Thus, it can also contribute to the improvement of the output characteristics caused by the reduction of the positive electrode resistance.
[0078] The LW compound particles 16 are particles containing Li and W. Typically, the LW compound particles 16 are formed by introducing Li into precursor particles containing tungsten oxide (WO3) as a main component, and contain lithium tungstate as a main component. In addition, there is no particular restriction on the atomic ratio of Li and W constituting lithium tungstate. For example, lithium tungstate may have Li2WO4, Li4WO5, Li6WO6, Li2W4O 13 , Li2W2O7, Li6W2O9, Li2W2O7, Li2W5O 16 ,Li9W 19 O 55 、Li3W 10 O 30 , Li 18 W5W 15 Of these, preferably one having Li p WO qThe composition represented by (0.3≦p≦6.0, 3.0≦q≦6.0) is particularly preferably a composition represented by Li2WO4. Furthermore, lithium tungstate can be hydrated. In addition, a precursor substance (WO3) in a state where Li is not introduced may exist in the LW compound particles 16. Furthermore, the atomic concentration of W in the LW compound particles 16 is higher than that in the core 12 and the W concentrated layer 14 described above. For example, when measured using TEM-EDX, W with an atomic concentration of 90 atomic % or more is confirmed in the LW compound particles 16.
[0079] In addition, the LW compound particles 16 may contain elements other than Li and W. For example, depending on the manufacturing conditions and the use conditions, elements from other components (core part 12, W concentration layer 14, non-aqueous electrolyte, etc.) may be contained in the LW compound particles 16. In this case, as the elements that may be contained in the LW compound particles 16, for example, Ni, Co, Mn, Mg, Ca, Al, Ti, V, Cr, Si, Y, Zr, Nb, Mo, Hf, Ta, Na, Fe, Zn, Sn, B, C, Si, P, S, F, Cl, etc. can be listed.
[0080] In addition, the LW compound particles 16 may be attached to at least a portion of the surface of the W concentration layer 14, and the form of the LW compound particles 16 is not particularly limited. Figure 3 As shown in , the primary particles are attached to the surface of the W concentration layer 14 in a dispersed state, or the primary particles may be aggregated to form secondary particles attached at specific positions. In addition, the LW compound particles may further aggregate to form a thin film to cover a portion of the surface of the W concentration layer. In addition, from the viewpoint of more appropriately exerting the durability improvement effect and resistance reduction effect of the LW compound particles 16, the coverage rate of the LW compound particles 16 is preferably 5% or more, more preferably 10% or more, further preferably 15% or more, and particularly preferably 20% or more. On the other hand, from the viewpoint of appropriately exerting the resistance reduction effect of the W concentration layer 14 of the amorphous structure, it is preferred that the coverage rate of the LW compound particles 16 is 50% or less (more preferably 45% or less, further preferably 40% or less, and particularly preferably 35% or less) to ensure the contact area between the W concentration layer 14 and the non-aqueous electrolyte. In addition, in the reflected electron image of the surface SEM, the portion where the LW compound particles 16 are attached has a higher W concentration than the portion where they are not attached, and thus becomes a bright image. Therefore, by performing image processing on the reflected electron image and obtaining the area ratio of the bright portion (area of bright portion / (area of bright portion+area of dark portion)), the "coverage rate by the LW compound particles" can be calculated.
[0081] In addition, although there are no particular restrictions, the average particle size (D50) of the LW compound particles 16 is, for example, preferably 1 nm or more, more preferably 5 nm or more, and further preferably 10 nm or more. This allows the resistance reduction effect of the LW compound particles 16 to be appropriately exerted. On the other hand, the upper limit of the average particle size of the LW compound particles 16 is preferably 500 nm or less, more preferably 300 nm or less, further preferably 200 nm or less, and particularly preferably 100 nm or less. At this time, it can also contribute to the improvement of the resistance reduction effect. It should be noted that the average particle size of the LW compound particles 16 can be measured in the same manner as the average particle size of the core 12 described above.
[0082] Furthermore, without limiting the present invention, the LW compound particles 16 can be generated according to the known methods disclosed in Japanese Patent Application Publication No. 2017-84628. For example, core-shell particles having an amorphous W concentration layer 14 formed on the surface of the layered core 12 are prepared, and the core-shell particles are mixed with tungsten compound particles (e.g., WO3 particles) that do not contain Li in a predetermined solvent (water, alcohol, etc.), and then the solvent is dried by heating at about 150°C. Thus, Li from the core-shell particles is supplied to the tungsten compound particles to form LW compound particles 16, which are attached to the surface of the W concentration layer 14.
[0083] (d) Overall composition of positive electrode active material
[0084] As described above, the positive electrode active material 10 in this embodiment includes: a core portion 12 containing a layered lithium transition metal composite oxide; a W concentration layer 14 having an amorphous structure and a higher W concentration than the core portion 12; and LW compound particles 16 containing Li and W. Such a positive electrode active material 10 can appropriately suppress various degradations and can also exert an appropriate resistance reduction effect. Therefore, the lithium ion secondary battery 100 using the positive electrode active material 10 can ensure the prescribed durability and exert excellent output characteristics.
[0085] The lithium ion secondary battery according to one embodiment of the present invention has been described above, but the above description is for illustrative purposes only, and various configurations may be appropriately changed according to the application and purpose as long as the effects of the present invention are not significantly impaired.
[0086] For example, in the above-mentioned embodiment, the positive electrode active material 10 is used in which the W concentration layer 14 is formed on the surface of the primary particle of the core portion 12 and the LW compound particles 16 are attached to the W concentration layer 14 (see Figure 3). However, the form of the positive electrode active material used in the non-aqueous electrolyte secondary battery disclosed herein is not limited to the above-mentioned embodiments. For example, a W concentration layer can be formed on the surface of the secondary particles formed by the aggregation of the primary particles of the core (i.e., the area in contact with the electrolyte), and the LW compound particles are attached to the W concentration layer. Even in this way, the positive electrode active material that forms the W concentration layer and the LW compound particles with the secondary particles of the core as the core can appropriately suppress various degradations and exert a suitable resistance reduction effect.
[0087] In addition, if Figure 1 As shown in , the above-mentioned embodiment is based on a square lithium-ion secondary battery 100 having a flat wound electrode body 20. However, the non-aqueous electrolyte secondary battery disclosed herein is not limited to the lithium-ion secondary battery 100. For example, the technology disclosed herein can also be applied to a lithium-ion secondary battery having a stacked electrode body, a cylindrical lithium-ion secondary battery, a laminated lithium-ion secondary battery, etc. Furthermore, the technology disclosed herein can also be applied to non-aqueous electrolyte secondary batteries other than lithium-ion secondary batteries.
[0088] [Test example]
[0089] Hereinafter, test examples according to the present invention will be described, but the present invention is not intended to be limited to the contents shown in these test examples.
[0090] A. First Test
[0091] In this test, eight types of lithium ion secondary batteries were constructed using a positive electrode active material having a W concentration layer with an amorphous structure and a positive electrode active material not having a W concentration layer with an amorphous structure, and the performance of each battery was evaluated.
[0092] 1. Sample preparation
[0093] (1) Sample 1
[0094] First, a first raw material aqueous solution containing nickel (Ni), cobalt (Co), manganese (Mn) and tungsten (W) in a molar ratio of 1:1:1:0.0015 is prepared. On the other hand, a reaction solution whose pH is adjusted using sulfuric acid and ammonia water is prepared and injected into a reaction container. Then, while controlling the pH using a pH adjusting solution composed of a mixture of an aqueous sodium carbonate solution and an aqueous ammonium carbonate solution, the reaction solution is stirred and the first raw material aqueous solution is dripped into the reaction solution at a prescribed speed, thereby causing the particles of the transition metal composite hydroxide that serves as a precursor of the core to crystallize and precipitate (crystallization).
[0095] Next, a raw material aqueous solution (second raw material aqueous solution) having a higher tungsten concentration than the first raw material aqueous solution is dripped into the reaction solution in which the precursor of the core portion is crystallized, thereby generating precursor particles of the precursor having a W concentration layer formed on the surface of the precursor of the core portion. It should be noted that the second raw material aqueous solution used here is an aqueous solution containing Ni, Co, Mn and W in a molar ratio of 1:1:1:0.02.
[0096] Next, the generated precursor particles were washed with water, filtered and dried to obtain dry powder. Then, the dry powder of the precursor particles was mixed with lithium carbonate and calcined (calcination temperature: 800°C, calcination time: 6 hours). Thus, Li was introduced into the respective precursors of the core part and the W concentration layer, and core-shell particles (parent material) were obtained in which a W concentration layer with a higher W concentration than the core part was formed on the surface of the core part composed of a layered lithium nickel cobalt manganese composite oxide.
[0097] Next, a drum sputtering device (Ballersputter device) manufactured by Fluya Metal Co., Ltd. was used to collide tungsten oxide (WO3) with the surface of the core-shell particles, and the W concentration layer was amorphized by physical collision. Next, the amorphized core-shell particles and WO3 were added to a solvent (water) at a ratio of 100:10 and mixed, and the mixture was dried (temperature: 150°C, time: 12 hours) to introduce a portion of Li in the core and W concentration layer into WO3. Thus, a positive electrode active material was generated in which an amorphous W concentration layer was formed on the surface of the layered core and the LW compound was attached to the surface of the W concentration layer.
[0098] Then, a positive electrode active material layer was prepared by mixing the positive electrode active material obtained in the above process, a conductive material (acetylene black) and a binder (PVDF) in a ratio of 98:1:1, and the positive electrode active material layer was applied to the surface of the positive electrode collector (aluminum foil) to obtain a positive electrode sheet. On the other hand, a negative electrode active material layer was prepared by mixing the negative electrode active material (natural graphite), a thickener (CMC) and a binder (SBR) in a ratio of 98:1:1, and the negative electrode active material layer was formed on the surface of the negative electrode collector (copper foil) to obtain a negative electrode sheet. Next, the positive electrode sheet and the negative electrode sheet were stacked via a separator (a three-layer sheet of PP-PE-PP) with a thickness of 24 μm, and the obtained stack was wound to obtain a wound electrode body. Then, the wound electrode body was housed in a square outer casing made of aluminum alloy, and the outer casing was sealed after injecting a non-aqueous electrolyte, thereby constructing a lithium ion secondary battery (sample 1) for evaluation test. Furthermore, as the non-aqueous electrolyte, a product in which 1 M of a supporting salt (LiPF6) was dissolved in a mixed solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:4:3 was used.
[0099] It should be noted that in this experiment, before making the positive electrode sheet, the positive electrode active material was analyzed using TEM-EDX, and the atomic concentration of W in the W concentrated layer (A) and the atomic concentration of W in the core (B) were measured according to the above steps. The measurement results are shown in Table 1.
[0100] (2) Sample 2
[0101] In Sample 2, only the core (lithium nickel cobalt manganese composite oxide with a layered structure) was used as the positive electrode active material. That is, a lithium ion secondary battery for testing was prepared under the same conditions as Sample 1, except that the W concentration layer and LW compound particles were not formed and lithium nickel cobalt manganese composite oxide without W was used as the positive electrode active material.
[0102] (3) Sample 3
[0103] No W-concentrated layer was formed in Sample 3. Specifically, a test battery was prepared under the same conditions as Sample 1 except that LW compound particles were directly attached to the surface of a W-free lithium nickel cobalt manganese composite oxide (core) as the positive electrode active material.
[0104] (4) Sample 4
[0105] In Sample 4, the W concentration layer was not amorphized and the LW compound particles were not attached. Specifically, a test battery was prepared under the same conditions as Sample 1 except that core-shell particles having a layered W concentration layer formed on the surface of the core were used as the positive electrode active material.
[0106] (5) Sample 5
[0107] In Sample 5, the W concentration layer was not amorphized. That is, a test battery was produced under the same conditions as Sample 1 except that a W concentration layer having a layered structure was formed on the surface of the core and LW compound particles were attached to the surface of the W concentration layer as the positive electrode active material.
[0108] (6) Samples 6 to 8
[0109] In addition, in this test, a positive electrode active material was prepared in which a surface layer with a tungsten concentration lower than that of the core part or a surface layer with a tungsten concentration equal to that of the core part was formed on the surface of the core part, and LW compound particles were attached to the surface layer. The evaluation batteries constructed using these positive electrode active materials were designated as samples 6 to 8. It should be noted that the conditions other than the positive electrode active material were the same as those of sample 1.
[0110] 2. Evaluation test
[0111] Here, the battery resistance of the test battery of each sample was measured to evaluate the output characteristics, and the capacity retention rate after the endurance treatment was measured to evaluate the durability.
[0112] (1) Output characteristics evaluation
[0113] First, the activation treatment (initial charge) of the evaluation battery of each sample was performed in an environment of 25°C. The activation treatment was set to a constant current-constant voltage method. After constant current charging to 4.2V with a current value of 1 / 3C, constant voltage charging was performed until the current value became 1 / 50C, thus reaching a fully charged state. Then, constant current discharge was performed with a current value of 1 / 3C until the voltage reached 3.0V.
[0114] Next, the evaluation battery after activation treatment was adjusted to an open circuit voltage of 3.70V and maintained at a temperature environment of -28°C. Then, it was discharged for 8 seconds with a current value of 20C, and the voltage drop ΔV at this time was calculated. The voltage drop ΔV was divided by the discharge current value (20C) to calculate the battery resistance. As the battery resistance decreases, it can be evaluated as having high output characteristics. The calculation results are shown in Table 1. In addition, Table 1 records the relative evaluation when the battery resistance of Sample 2 is set to 100.
[0115] (2) Durability evaluation
[0116] Here, a high-temperature durability test at 60°C was performed on the evaluation battery after the above-mentioned activation treatment. While maintaining the temperature (60°C) of the durability test, CC charging at a rate of 2C was performed until the voltage rose to 4.2V, and then CC discharge was performed at a rate of 2C until the voltage dropped to 3.0V, and such a charge and discharge cycle was repeated for 500 cycles. Then, the CC discharge capacity of the 1st cycle and the 500th cycle was measured, and the ratio of the CC discharge capacity of the 500th cycle to the CC discharge capacity of the 1st cycle was calculated as the capacity retention rate (%). As the capacity retention rate increases, it can be evaluated as high durability. The calculation results are shown in Table 1.
[0117]
Table 1
[0118] Table 1
[0119]
[0120] As shown in Table 1, in samples 1, 3 to 5, 7, and 8, except for sample 2 in which LW compound particles were not attached and sample 6 in which a surface layer with a low W concentration was formed, high durability (capacity retention rate) of about 67% to 69% was confirmed. On the other hand, when the output characteristics (battery resistance) were compared, it was confirmed that sample 1 exhibited the most excellent output characteristics. It can be seen from this that when a W concentrated layer is formed on the surface of the core, LW compound particles are attached to the W concentrated layer, and the W concentrated layer is amorphized, a secondary battery that ensures the specified durability and exhibits excellent output characteristics can be constructed.
[0121] B. Second Test
[0122] In this test, conditions for achieving higher levels of durability and output characteristics when a positive electrode active material having an amorphous W concentration layer formed on the surface of the core portion and LW compound particles attached to the W concentration layer was used as in Sample 1 were examined.
[0123] 1. Sample preparation
[0124] Seven kinds of positive electrode active materials prepared under the same conditions as sample 1 except that the atomic concentration of W in the W concentrated layer (A) and the atomic concentration of W in the core (B) were different were prepared, and evaluation batteries (samples 9 to 15) using each positive electrode active material were prepared. The atomic concentration of W in the W concentrated layer (A) and the atomic concentration of W in the core (B) of each sample are shown in Table 2.
[0125] 2. Evaluation test
[0126] The battery resistance and capacity retention rate were measured under the same conditions as in the first test, and the output characteristics and durability were evaluated. The results are shown in Table 2. Table 2 also lists the battery resistance and capacity retention rate of Sample 1 measured in the first test.
[0127]
Table 2
[0128] Table 2
[0129]
[0130] As shown in Table 2, when the atomic concentration (A) of W in the W concentrated layer increases, a tendency of a decrease in battery resistance (improvement in output characteristics) is found. On the other hand, when the atomic concentration (A) of W in the W concentrated layer increases excessively, a tendency of a decrease in capacity retention rate (durability) is found. In addition, when the atomic concentration (B) of W in the core increases, a tendency of a decrease in durability is also found. Considering these tendencies, it can be seen that if the atomic concentration (A) of W in the W concentrated layer is made to be greater than 1 atomic % and less than 3.6 atomic %, and the atomic concentration (B) of W in the core is made to be less than 0.3 atomic %, a particularly high level of durability and output characteristics can be achieved.
[0131] Although the specific examples of the present invention have been described in detail above, these are merely examples and do not limit the claims. The technology described in the claims includes various modifications and changes made to the specific examples described above.
Claims
1. A non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte, wherein: The positive electrode comprises a positive electrode active material layer containing a particulate positive electrode active material. The positive electrode active material comprises: a core portion including a layered lithium transition metal composite oxide, a W concentrated layer formed on the surface of the core portion and having a higher atomic concentration of tungsten than that of the core portion as confirmed by TEM-EDX analysis, and LW compound particles containing lithium and tungsten attached to at least a portion of the surface of the W concentrated layer, The W concentrated layer has an amorphous structure, and a thickness of the W concentrated layer is greater than or equal to 40 nm and less than or equal to 100 nm. The atomic concentration A of tungsten in the W concentrated layer is greater than or equal to 1 atomic % and less than or equal to 3.6 atomic %, The atomic concentration B of tungsten in the core portion is 0.3 atomic % or less, The atomic concentration of tungsten in the LW compound particles is higher than the atomic concentration of tungsten in the W concentrated layer. When measured using TEM-EDX, the LW compound particles have an atomic concentration of W of 90 atomic % or more.