Flexible sensor and preparation method thereof
By designing a flexible sensor with a conductive flexible substrate and a dielectric layer dislocation structure, the problem of difficulty in detecting slip and tactile signals at the same time in the prior art is solved, and precise object perception during the soft grasping process of intelligent robots is realized.
Patent Information
- Application Number
- CN202011044691.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-09-28
AI Technical Summary
Existing flexible sensors are difficult to detect slip and tactile signals accurately at the same time, limiting their application in the field of intelligent robots, especially the problem of objects being damaged or shedding during soft grabbing.
A flexible sensor including a conductive first flexible substrate and a second flexible substrate are designed, both of which have a microstructure array and a dielectric layer on the surface, and a dielectric layer is provided in the gap between the microstructures, and a dislocation structure is formed by assembly to externally The pressure and shear force are feedback through the capacitance and resistance signals respectively.
It realizes simultaneous detection of sliding and tactile signals, and the structure is simple and accurate, improving the object perception ability of intelligent robots during soft grabbing.
Smart Images

Figure CN112254747B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of sensor technology, and in particular to a flexible sensor and a method for preparing the same. Background Art
[0002] Flexible sensors that can sense tactile signals and slip signals at the same time have great application prospects in the field of intelligent robots. At present, although intelligent robots can replace human hands to complete some simple object operations, it is difficult to achieve soft grasping of brittle objects. By installing the aforementioned flexible sensors on the surface of the manipulator to sense tactile and slip signals, the force between the manipulator and the object can be accurately controlled, which is expected to solve the problem of object damage or falling off during soft grasping. The key to soft grasping technology is that the manipulator can perceive information about the interaction with the external environment like a human hand. However, most of the current flexible sensors can only measure positive pressure, and there is a significant gap with human hands in terms of detection sensitivity, which limits its application in the field of intelligent robots. Summary of the invention
[0003] In response to the above technical problems, the present application provides a flexible sensor that can detect sliding signals and tactile signals at the same time, has a simple structure and is more accurate.
[0004] In order to solve the above technical problems, the present application provides a flexible sensor, including a first flexible substrate and a second flexible substrate, the first flexible substrate and the second flexible substrate are conductive, one side surface of the first flexible substrate has a first microstructure array, one side surface of the second flexible substrate has a second microstructure array, the microstructure gaps of the first microstructure array and the microstructure gaps of the second microstructure array are both provided with a dielectric layer, the first microstructure array and the second microstructure array are arranged opposite to each other and the microstructures are staggered with each other to form a structure in which the microstructures and the microstructure gaps match each other between the microstructure arrays.
[0005] Wherein, the first microstructure array and the second microstructure array include at least one of a pyramid microstructure array, a cone microstructure array, and a hemispherical microstructure array; and / or
[0006] Conductive material is dispersed in the first flexible substrate and the second flexible substrate, and the conductive material includes at least one of carbon nanotubes, graphene, carbon black, and silver nanowires.
[0007] Wherein, the first flexible substrate and the second flexible substrate are porous structures.
[0008] The microstructures in the first microstructure array and the microstructures in the second microstructure array are not in contact with each other, and the microstructures in the first microstructure array and the microstructures in the second microstructure array are respectively bonded to the dielectric layer in the microstructure gaps on the opposite side.
[0009] Wherein, the dielectric layer is prepared by using a dielectric material having a melting temperature lower than the melting temperature of the bases of the first flexible substrate and the second flexible substrate.
[0010] The present application also provides a method for preparing a flexible sensor, comprising:
[0011] a. providing a first flexible substrate and a second flexible substrate having conductivity, wherein one side surface of the first flexible substrate has a first microstructure array, one side surface of the second flexible substrate has a second microstructure array, and the microstructure gaps of the first microstructure array and the microstructure gaps of the second microstructure array are both provided with a dielectric layer;
[0012] b. Assembling the first flexible substrate and the second flexible substrate, the first microstructure array and the second microstructure array are facing each other and the microstructures are mutually offset to form a structure in which the microstructures and the microstructures are gap-matched between the microstructure arrays;
[0013] c. Get the flexible sensor.
[0014] Wherein, step a comprises:
[0015] preparing a mixture comprising a polymer prepolymer, a conductive material, a pore former and a curing agent;
[0016] The mixture is placed in a template having a microstructure array cavity on one side and cured into a shape;
[0017] The mold is demoulded and the pore-forming agent is removed to obtain a conductive flexible substrate having a microstructure array on one surface.
[0018] The above process is repeated or the conductive flexible substrate is cut to obtain the first flexible substrate and the second flexible substrate without a dielectric layer on the surface.
[0019] Wherein, the first microstructure array and the second microstructure array include at least one of a pyramid microstructure array, a cone microstructure array, and a hemispherical microstructure array; and / or
[0020] The conductive material includes at least one of carbon nanotubes, graphene, carbon black, and silver nanowires; and / or
[0021] The pore formers are particles that can be dissolved or removed by chemical reaction.
[0022] Wherein, step a comprises:
[0023] Coating a dielectric layer on the surface of the first flexible substrate and the second flexible substrate having no dielectric layer on the surface thereof, respectively, on one side having the microstructure array;
[0024] The dielectric layer on each flexible substrate is patterned respectively, and the portion of the dielectric layer located in the microstructure gap is retained.
[0025] Wherein, the dielectric layer is prepared by using a dielectric material having a melting temperature lower than the melting temperature of the base of the first flexible substrate and the second flexible substrate, and step c comprises:
[0026] The assembled structure is heated to melt the dielectric layer and bond it to the microstructures in the gaps between the microstructures.
[0027] The present application also provides a flexible sensor, which is prepared using the flexible sensor preparation method as described above.
[0028] The flexible sensor of the present application includes a first flexible substrate and a second flexible substrate, the first flexible substrate and the second flexible substrate are conductive, one side surface of the first flexible substrate has a first microstructure array, one side surface of the second flexible substrate has a second microstructure array, the microstructure gaps of the first microstructure array and the microstructure gaps of the second microstructure array are both provided with a dielectric layer, the first microstructure array and the second microstructure array are arranged opposite to each other and the microstructures are mutually offset to form a structure in which the microstructures and the microstructure gaps cooperate between the microstructure arrays. When the microstructure is deformed due to external pressure, the capacitance signal at the dielectric layer changes to provide tactile feedback; when the external shear force changes the contact area between the microstructures of the two flexible substrates, the resistance signal changes to provide sliding feedback, so that the sliding tactile sensation can be detected at the same time, and the structure is simple and more accurate.
[0029] The method for preparing the flexible sensor of the present application first provides a first flexible substrate and a second flexible substrate with conductivity, one side surface of the first flexible substrate has a first microstructure array, one side surface of the second flexible substrate has a second microstructure array, a dielectric layer is formed in the microstructure gap of the first microstructure array and in the microstructure gap of the first microstructure array, and then the first flexible substrate and the second flexible substrate are assembled, the first microstructure array and the second microstructure array are facing each other and the microstructures are mutually staggered, so as to form a structure in which the microstructures and the microstructure gaps match each other between the microstructure arrays, and thus a flexible sensor is obtained. The preparation process is simple and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a schematic longitudinal cross-sectional view of a flexible sensor according to the first embodiment;
[0031] Figure 2is a bottom view of a first flexible substrate of a flexible sensor according to the first embodiment;
[0032] Figure 3 is a schematic flow chart of a method for preparing a flexible sensor according to the second embodiment. DETAILED DESCRIPTION
[0033] The following is an explanation of the implementation of the present application by means of specific embodiments. People familiar with the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification.
[0034] In the following description, reference is made to the accompanying drawings, which describe several embodiments of the present application. It should be understood that other embodiments may be used and that mechanical, structural, electrical, and operational changes may be made without departing from the spirit and scope of the present application. The following detailed description should not be considered limiting, and the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present application.
[0035] Although the terms first, second, etc. are used herein to describe various elements in some instances, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element.
[0036] Furthermore, as used in this article, the singular forms "one", "an" and "the" are intended to include plural forms as well, unless there is an indication to the contrary in the context. It should be further understood that the terms "comprise", "include" indicate the presence of the described features, steps, operations, elements, components, projects, kinds, and / or groups, but do not exclude the presence, occurrence or addition of one or more other features, steps, operations, elements, components, projects, kinds, and / or groups. The terms "or" and "and / or" used herein are interpreted as inclusive, or mean any one or any combination. Therefore, "A, B or C" or "A, B and / or C" means "any of the following: A; B; C; A and B; A and C; B and C; A, B and C". Exceptions to this definition will only occur when the combination of elements, functions, steps or operations is inherently mutually exclusive in some way.
[0037] First embodiment
[0038] Figure 1 FIG. 1 is a schematic longitudinal cross-sectional view of a flexible sensor according to the first embodiment. Figure 1As shown, the flexible sensor of this embodiment includes a first flexible substrate 11 and a second flexible substrate 12, the first flexible substrate 11 and the second flexible substrate 12 are conductive, a first microstructure array 112 is provided on one side surface of the first flexible substrate 11, a second microstructure array 122 is provided on one side surface of the second flexible substrate 12, a first dielectric layer 113 is provided in the microstructure gap of the first microstructure array 112, a second dielectric layer 123 is provided in the microstructure gap of the second microstructure array 122, the first microstructure array 112 and the second microstructure array 122 are arranged opposite to each other and the microstructures are staggered to form a structure in which the microstructures and the microstructure gaps match each other between the microstructure arrays.
[0039] When the above-mentioned flexible sensor is subjected to external pressure, the local microstructure on the first flexible substrate 11 and / or the second flexible substrate 12 is deformed, which can cause the capacitance signal at the dielectric layer at the corresponding position to change, so that tactile feedback can be performed; when subjected to external shear force, the local microstructure on the first flexible substrate 11 and the microstructure at the corresponding position on the second flexible substrate 12 are offset, resulting in a change in the contact area between the microstructures of the two flexible substrates, which can cause a change in the resistance signal for sliding feedback. In this way, the flexible sensor of this embodiment can detect sliding signals and tactile signals at the same time, that is, it can sense positive pressure and shear force at the same time, and the structure is simple. Moreover, the sliding signals and tactile signals are generated based on the deformation of the microstructure, and the detection is more accurate and real-time.
[0040] The first microstructure array 112 can be at least one of a pyramid microstructure array, a cone microstructure array, and a hemispherical microstructure array. The side length or diameter range of the microstructure is 1 to 1000 μm, the height range is 1 to 1000 μm, the distance between the tops of adjacent microstructures is less than or equal to 2000 μm, and adjacent microstructures refer to microstructures that are adjacent in the horizontal or vertical direction of the substrate plane. Figure 2Taking the first microstructure array 112 as a pyramid microstructure array as an example, the pyramid-shaped microstructures 1121 are arranged horizontally and vertically on the substrate plane, and two adjacent rows of microstructures 1121 are staggered with each other, and there are gaps (i.e., microstructure gaps) between the four microstructures 1121 to form an array. When the gap width between the microstructures 1121 is equal to the side length of the microstructure 1121, the corners of the microstructures 1121 are in contact, and a first dielectric layer 113 is provided in each microstructure gap. The second microstructure array 122 may be at least one of a pyramid microstructure array, a cone microstructure array, and a hemispherical microstructure array. The structure of the second flexible substrate 12 is the same as that of the first flexible substrate 11, except that the microstructure on the second flexible substrate 12 is horizontally or vertically offset by a microstructure size relative to the microstructure on the first flexible substrate 11. Thus, after the first flexible substrate 11 and the second flexible substrate 12 are assembled, the microstructures of the upper and lower microstructure arrays are displaced from each other to form a structure in which microstructures and microstructure gaps cooperate. Each microstructure is located in the microstructure gap on the opposite flexible substrate, and forms a tactile sensing structure with the dielectric layer in the microstructure gap, and forms a slip sensing structure with adjacent microstructures.
[0041] The substrates of the first flexible substrate 11 and the second flexible substrate 12 can be prepared by selecting materials with good biocompatibility, such as polydimethylsiloxane (PDMS), polyurethane elastomer (TPU), polytrimethylene carbonate (PTMC), etc. PDMS is preferred because it has the best biocompatibility and thermal stability. Conductive materials are dispersed in the first flexible substrate 11 and the second flexible substrate 12 to have conductivity, and the conductive materials include at least one of carbon nanotubes, graphene, carbon black, and silver nanowires.
[0042] In order to further improve the sensitivity of detection, the first flexible substrate 11 and the second flexible substrate 12 can be made into a porous structure. The porous structure can make the deformation of the microstructure more sensitive, improve the sensitivity of tactile sensing, and at the same time, the porous structure can increase the roughness of the microstructure surface, make the contact between the microstructures more sensitive, and improve the sensitivity of slip sensing. The porous structure can be obtained by using a pore-forming agent to form pores. The pore-forming agent is a particle that can be dissolved or removed by chemical reaction. Among them, the pore-forming agent can be a polymer microsphere, such as polystyrene (PS), polymethyl methacrylate (PMMA), etc., which can be dissolved and removed; the pore-forming agent can also be an inorganic salt particle, such as NaCl, NaCO3, etc., which can be dissolved and removed; the pore-forming agent can also be a metal particle, such as Ag, Cu, etc., which can be removed by chemical reaction.
[0043] The microstructures in the first microstructure array 112 and the microstructures in the second microstructure array 122 do not contact each other when not under stress, and the distance between the microstructures of the two flexible substrates can be adjusted by designing the height, side length or diameter of the microstructures. It can be understood that the sliding signal is obtained through the change of the resistance signal, so the microstructures in the first microstructure array 112 and the microstructures in the second microstructure array 122 can also partially contact each other when not under stress, and it is only necessary to have a space for displacement when under stress to generate a change in the resistance signal.
[0044] The first dielectric layer 113 and the second dielectric layer 123 can be formed in the microstructure gap of the corresponding flexible substrate by patterning after surface coating. Patterning can be achieved by laser etching technology. Since ultrafast laser has obvious nonlinear absorption effect, the heat effect generated by etching is small and the quality is good, so ultrafast laser etching coating is preferred. In addition, as the laser wavelength increases, the photothermal effect becomes more obvious. In order to reduce the thermal effect, the laser wavelength is preferably 355nm. The laser single pulse energy range is 20 to 300μJ. When the single pulse energy is less than 20μJ, the etching time is long and the efficiency is low; when the single pulse energy is greater than 300μJ, the thermal effect increases, affecting the etching quality. At the same time, the laser scanning speed range is 100 to 3000mm / s. When the scanning speed is less than 100mm / s, the accumulated heat effect will also affect the etching quality; when the scanning speed is greater than 3000mm / s, the laser spot overlap rate is low, and the coating at the microstructure cannot be completely removed.
[0045] The thickness of the first dielectric layer 113 and the second dielectric layer 123 is less than the height of the microstructure, for example, the thickness of the first dielectric layer 113 and the second dielectric layer 123 is 1 to 300 μm, preferably 10 to 200 μm. In this embodiment, the first dielectric layer 113 and the second dielectric layer 123 are prepared by using a dielectric material having a melting temperature lower than the melting temperature of the base of the first flexible substrate 11 and the second flexible substrate 12, preferably a dielectric material having a melting temperature of 50 to 200°C, for example, polycaprolactone (PCL) is used, and the melting temperature is 50 to 70°C, so that the assembled first flexible substrate 11 and the second flexible substrate 12 can be placed in an environment of 50 to 70°C, so that the first dielectric layer 113 and the second dielectric layer 123 are bonded to the microstructure on the opposite side after melting, and the first flexible substrate 11 and the second flexible substrate 12 are fixed together. It can be understood that the first dielectric layer 113 and the second dielectric layer 123 can also be prepared by other dielectric materials such as PDMS. In this case, the first flexible substrate 11 and the second flexible substrate 12 can be fixed together by encapsulating them at the edges of the first flexible substrate 11 and the second flexible substrate 12.
[0046] After the first flexible substrate 11 and the second flexible substrate 12 are fixed together, two thin wires are cut and connected to the first flexible substrate 11 and the second flexible substrate 12 respectively, and then a layer of conductive silver glue is coated to fix the wires, so that a flexible sensor can be obtained.
[0047] The flexible sensor of this embodiment includes a first flexible substrate and a second flexible substrate, the first flexible substrate and the second flexible substrate are conductive, a first microstructure array is provided on one side surface of the first flexible substrate, a second microstructure array is provided on one side surface of the second flexible substrate, a dielectric layer is provided in the microstructure gaps of the first microstructure array and the microstructure gaps of the second microstructure array, the first microstructure array and the second microstructure array are arranged opposite to each other and the microstructures are mutually offset to form a structure in which the microstructures and the microstructure gaps cooperate between the microstructure arrays. When the microstructure is deformed by external pressure, the capacitance signal at the dielectric layer changes to provide tactile feedback; when the contact area between the microstructures of the two flexible substrates changes due to external shear force, the resistance signal changes to provide sliding feedback, so that the sliding tactile sense can be detected at the same time, and the structure is simple and more accurate.
[0048] Second embodiment
[0049] Figure 3 FIG. 1 is a flow chart of a method for preparing a flexible sensor according to the second embodiment. Figure 3 As shown, the method for preparing the flexible sensor of this embodiment includes:
[0050] Step 210, providing a first flexible substrate and a second flexible substrate with conductivity, wherein one side surface of the first flexible substrate has a first microstructure array, and one side surface of the second flexible substrate has a second microstructure array, and microstructure gaps of the first microstructure array and microstructure gaps of the second microstructure array are both provided with a dielectric layer.
[0051] First, prepare a mixture containing a polymer prepolymer, a conductive material, a pore former and a curing agent, wherein the particle size of the pore former is 1 to 500 μm, and the mass accounts for more than 60% of the total mass, which can avoid that some of the pore-forming particles are coated after curing and difficult to completely remove, and the mass of the conductive material accounts for more than 1% of the total mass and less than 30% of the total mass, so as to achieve the conductive function. Specifically, the polymer prepolymer, the conductive material, the pore former, etc. can be placed in a solvent such as n-hexane and dichloromethane, and the ratio of the total mass of the polymer prepolymer, the conductive material and the pore former to the mass of the solvent is 1:5 to 1:20. After vacuum stirring, add the curing agent, and the ratio of the mass of the curing agent to the mass of the polymer prepolymer is 0.9 to 1.1:10. Then, stir again to remove bubbles, and then heat to remove the solvent to obtain a mixture containing a polymer prepolymer, a conductive material, a pore former and a curing agent. Among them, the polymer material prepolymer can be polydimethylsiloxane (PDMS), polyurethane elastomer (TPU), polytrimethylene carbonate (PTMC), etc., the conductive material includes at least one of carbon nanotubes, graphene, carbon black, and silver nanowires, and the pore-forming agent is soluble and removable inorganic salt particles.
[0052] Next, the mixture is loaded into a template having a microstructure array cavity on one side for solidification and molding. The microstructure array includes at least one of a pyramid microstructure array, a cone microstructure array, and a hemispherical microstructure array. The side length or diameter range of the microstructure is 1 to 1000 μm, and the height range is 1 to 1000 μm.
[0053] Then, after molding, the mold is removed and the pore-forming agent is removed to obtain a conductive flexible substrate with a microstructure array on one side of the surface. Taking the pore-forming particles as NaCl particles as an example, the formed flexible substrate is placed in clean water for ultrasonic cleaning for 8 hours to remove the NaCl particles.
[0054] Repeat the above process to prepare another conductive flexible substrate or cut the conductive flexible substrate prepared above to obtain a first flexible substrate and a second flexible substrate (ie, a base) having no dielectric layer on the surface.
[0055] The dielectric layer is preferably made of a dielectric material having a melting temperature lower than the melting temperature of the base of the first flexible substrate and the second flexible substrate, preferably a dielectric material having a melting temperature of 50 to 200° C., such as polycaprolactone (PCL) having a melting temperature of 50 to 70° C. In actual implementation, the dielectric layer can also be made of other dielectric materials such as PDMS.
[0056] When making the dielectric layer, the dielectric layer is coated on the surface of the first flexible substrate and the second flexible substrate with a microstructure array on the surface without the dielectric layer. Specifically, a certain amount of polycaprolactone (PCL) is weighed and placed in a beaker, and after adding dichloromethane and stirring the PCL to completely dissolve, the PCL is spin-coated on the surface of the flexible substrate with the microstructure array, and the spin coating thickness is 1 to 300 μm. After that, the dielectric layer on each flexible substrate is patterned, and the portion of the dielectric layer located in the microstructure gap is retained, so that the first flexible substrate and the second flexible substrate can be obtained. The first flexible substrate has a first microstructure array on one side surface, and the second flexible substrate has a second microstructure array on one side surface. The microstructure gap of the first microstructure array and the microstructure gap of the second microstructure array are both provided with a dielectric layer. The thickness of the first flexible substrate and the second flexible substrate is 10 to 1000 μm.
[0057] Step 220 , assembling the first flexible substrate and the second flexible substrate, with the first microstructure array and the second microstructure array facing each other and the microstructures being offset from each other to form a structure with gaps between the microstructure arrays.
[0058] The microstructure on the second flexible substrate is horizontally or vertically offset from the microstructure on the first flexible substrate by a microstructure size. During assembly, the microstructure of the first flexible substrate and the microstructure of the second flexible substrate do not contact each other. Preferably, the top of the microstructure of the first flexible substrate is aligned with the center of the area between the tops of the microstructures of the second flexible substrate (the center of the microstructure gap), so that the microstructures of the upper and lower microstructure arrays are misaligned with each other to form a structure in which the microstructures and the microstructure gaps cooperate. Each microstructure is located in the microstructure gap on the opposite flexible substrate, and forms a tactile sensing structure with the dielectric layer in the microstructure gap, and forms a slip sensing structure with adjacent microstructures.
[0059] Step 230: obtaining a flexible sensor.
[0060] Wherein, when the dielectric layer is prepared by a dielectric material having a melting temperature lower than the melting temperature of the base of the first flexible substrate and the second flexible substrate, the assembled structure can be heated, for example, placed in an environment of 50 to 200°C, so that the dielectric layer is melted and adheres to the microstructure in the gap of the microstructure, thereby fixing the first flexible substrate and the second flexible substrate together. When the dielectric layer is prepared by other dielectric materials such as PDMS, the first flexible substrate and the second flexible substrate can be fixed together by encapsulating them at the edges of the first flexible substrate and the second flexible substrate. Afterwards, two thin wires are cut and connected to the first flexible substrate and the second flexible substrate respectively, and then a layer of conductive silver glue is applied to fix the wires, thereby obtaining a flexible sensor.
[0061] Next, several specific preparation processes are listed based on the above preparation process.
[0062] Preparation process 1:
[0063] (1) PDMS prepolymer, carbon nanotubes (CNT) and NaCl particles are weighed in proportion, wherein the particle size of the NaCl particles is 1 to 500 μm, the mass of the NaCl particles accounts for more than 60% of the total mass, when the mass fraction of the NaCl particles is less than 60%, some of the NaCl particles are completely coated by PDMS in the subsequent steps and are difficult to completely remove, the mass of the CNT accounts for more than 2% of the total mass and less than 30% of the total mass, and the conductive function is achieved. PDMS prepolymer, carbon nanotubes (CNT) and NaCl particles are added to a dichloromethane solvent, and the ratio of the total mass of the PDMS prepolymer, carbon nanotubes (CNT) and NaCl particles to the mass of the solvent is 1:5 to 1:20. After vacuum stirring, a curing agent is added, and the ratio of the mass of the curing agent to the mass of the PDMS prepolymer is 0.9 to 1.1:10. Then, after stirring again, bubbles are removed, and the resulting mixture is heated to 30 to 50° C. to remove the solvent. Then, the mixture is poured into a silicon template with a pyramid microstructure array for curing (the side length of the pyramid microstructure is 50 μm, the height is 30 μm, and the gap width between the microstructures is 50 μm). After curing, the mixture is demolded and placed in clean water for 8 hours to remove NaCl particles, forming a porous PDMS / CNT conductive composite material with a pyramid microstructure array on one side surface, and obtaining a base of the first flexible substrate and the second flexible substrate with a thickness of 10 to 1000 μm;
[0064] (2) PCL was dissolved in dichloromethane with a mass ratio of PCL to dichloromethane of 1:5 to 1:20, and spin-coated on the surface of the substrate with the pyramid microstructure array to a thickness of 10 μm. The PCL on the microstructure surface was then removed by laser etching to expose the conductive layer while retaining the portion located in the gap between the microstructures. The laser wavelength was 355 nm, the single pulse energy was 50 μJ, and the laser scanning speed was 1000 mm / s.
[0065] (3) Align the top of the pyramid microstructure of the first flexible substrate to the center of the area between the tops of the pyramid microstructure of the second flexible substrate, so that the top of the microstructure contacts the dielectric layer, and then place it in a 60°C environment for 2 minutes, so that the melted PCL is bonded to the top of the microstructure on the opposite flexible substrate. After that, cut two thin wires and connect them to the upper and lower flexible substrates respectively, and then apply a layer of conductive silver glue to fix the wires to obtain a flexible sensor.
[0066] Preparation process 2:
[0067] (1) TPU prepolymer, silver nanowires (AgNW) and NaCl particles are weighed in proportion, wherein the particle size of the NaCl particles is 1 to 500 μm, and the mass of the NaCl particles accounts for more than 60% of the total mass. When the mass fraction of the NaCl particles is less than 60%, some NaCl particles are completely coated by TPU in the subsequent steps and are difficult to be completely removed. The mass of the AgNW accounts for more than 1% of the total mass and less than 30% of the total mass, thereby achieving the conductive function. The TPU prepolymer, silver nanowires (AgNW) and NaCl particles are added to a dichloromethane solvent, and the ratio of the total mass of the TPU prepolymer, silver nanowires (AgNW) and NaCl particles to the mass of the solvent is 1:5 to 1:20. After vacuum stirring, a curing agent is added, and the ratio of the mass of the curing agent to the mass of the TPU prepolymer is 0.9 to 1.1:10. Then, after stirring again, bubbles are removed, and the resulting mixture is heated to 30 to 50° C. to remove the solvent. Then, the mixture was poured into a silicon template with a pyramid microstructure array for curing (the side length of the pyramid microstructure was 50 μm, the height was 30 μm, and the gap width between the microstructures was 50 μm). After curing, the mixture was demoulded and placed in clean water for 8 hours to remove the NaCl particles, forming a porous TPU / AgNW conductive composite material with a pyramid microstructure array on one side surface, and the substrate of the first flexible substrate and the second flexible substrate was obtained, with a thickness of 10 to 1000 μm;
[0068] (2) PCL was dissolved in dichloromethane with a mass ratio of PCL to dichloromethane of 1:5 to 1:20, and spin-coated on the surface of the substrate with the pyramid microstructure array to a thickness of 10 μm. The PCL on the microstructure surface was then removed by laser etching to expose the conductive layer while retaining the portion located in the gap between the microstructures. The laser wavelength was 355 nm, the single pulse energy was 50 μJ, and the laser scanning speed was 1000 mm / s.
[0069] (3) Align the top of the pyramid microstructure of the first flexible substrate to the center of the area between the tops of the pyramid microstructure of the second flexible substrate, so that the top of the microstructure contacts the dielectric layer, and then place it in a 60°C environment for 2 minutes, so that the melted PCL is bonded to the top of the microstructure on the opposite flexible substrate. After that, cut two thin wires and connect them to the upper and lower flexible substrates respectively, and then apply a layer of conductive silver glue to fix the wires to obtain a flexible sensor.
[0070] Preparation process 3:
[0071] (1) PDMS prepolymer, carbon nanotubes (CNT) and PS microspheres are weighed in proportion, wherein the particle size of the PS microspheres is 1 to 500 μm, the mass of the NaCl particles accounts for more than 60% of the total mass, when the mass fraction of the PS microspheres is less than 60%, some of the PS microspheres are completely coated by PDMS in the subsequent steps and are difficult to completely remove, the mass of the CNT accounts for more than 2% of the total mass and less than 30% of the total mass, and the conductive function is achieved. PDMS prepolymer, carbon nanotubes (CNT) and PS microspheres are added to n-hexane solvent, and the ratio of the total mass of the PDMS prepolymer, carbon nanotubes (CNT) and PS microspheres to the mass of the solvent is 1:5 to 1:20. After vacuum stirring, a curing agent is added, and the ratio of the mass of the curing agent to the mass of the PDMS prepolymer is 0.9 to 1.1:10. Then, after stirring again, bubbles are removed, and the resulting mixture is heated to 50 to 80° C. to remove the solvent. Then, the mixture was poured into a silicon template with a pyramid microstructure array for curing (the side length of the pyramid microstructure was 50 μm, the height was 30 μm, and the gap width between the microstructures was 50 μm). After curing, the mixture was demolded and placed in acetone for 8 hours to remove the PS microspheres to form a porous PDMS / CNT conductive composite material with a pyramid microstructure array on one side, and the substrate of the first flexible substrate and the second flexible substrate was obtained, with a thickness of 10 to 1000 μm.
[0072] (2) PCL was dissolved in dichloromethane with a mass ratio of PCL to dichloromethane of 1:5 to 1:20, and spin-coated on the surface of the substrate with the pyramid microstructure array to a thickness of 10 μm. The PCL on the microstructure surface was then removed by laser etching to expose the conductive layer while retaining the portion located in the gap between the microstructures. The laser wavelength was 355 nm, the single pulse energy was 50 μJ, and the laser scanning speed was 1000 mm / s.
[0073] (3) Align the top of the pyramid microstructure of the first flexible substrate to the center of the area between the tops of the pyramid microstructure of the second flexible substrate, so that the top of the microstructure contacts the dielectric layer, and then place it in a 60°C environment for 2 minutes, so that the melted PCL is bonded to the top of the microstructure on the opposite flexible substrate. After that, cut two thin wires and connect them to the upper and lower flexible substrates respectively, and then apply a layer of conductive silver glue to fix the wires to obtain a flexible sensor.
[0074] Preparation process 4:
[0075] (1) Weigh TPU prepolymer, carbon nanotubes (CNT) and NaCl particles in proportion, wherein the particle size of NaCl particles is 1 to 500 μm, the mass of NaCl particles accounts for more than 60% of the total mass, when the mass fraction of NaCl particles is less than 60%, some NaCl particles are completely coated by TPU in the subsequent steps and are difficult to completely remove, the mass of CNT accounts for more than 2% of the total mass and less than 30% of the total mass, and the conductive function is achieved. Add TPU prepolymer, carbon nanotubes (CNT) and NaCl particles to dichloromethane solvent, the total mass of TPU prepolymer, carbon nanotubes (CNT) and NaCl particles to the mass of solvent is 1:5 to 1:20. After vacuum stirring, add curing agent, the mass ratio of curing agent to TPU prepolymer mass is 0.9 to 1.1:10. Then, after stirring again, remove bubbles, and heat the obtained mixture to 30 to 50°C to remove the solvent. Then, the mixture was poured into a silicon template with a cone microstructure array for curing (the cone microstructure had a diameter of 100 μm, a height of 50 μm, and a gap width of 100 μm between the microstructures). After curing, the mixture was demoulded and placed in clean water for 8 hours to remove NaCl particles, forming a porous TPU / CNT conductive composite material with a cone microstructure array on one surface, and obtaining the base of the first flexible substrate and the second flexible substrate, with a thickness of 10 to 1000 μm;
[0076] (2) PCL was dissolved in dichloromethane with a mass ratio of PCL to dichloromethane of 1:5 to 1:20, and spin-coated on the surface of the substrate with the pyramid microstructure array to a thickness of 10 μm. The PCL on the microstructure surface was then removed by laser etching to expose the conductive layer while retaining the portion located in the gap between the microstructures. The laser wavelength was 355 nm, the single pulse energy was 50 μJ, and the laser scanning speed was 1000 mm / s.
[0077] (3) Align the top of the cone microstructure of the first flexible substrate to the center of the area between the tops of the cone microstructure of the second flexible substrate, so that the top of the microstructure contacts the dielectric layer, and then place it in a 60°C environment for 2 minutes, so that the melted PCL is bonded to the top of the microstructure on the opposite flexible substrate. After that, cut two thin wires and connect them to the upper and lower flexible substrates respectively, and then apply a layer of conductive silver glue to fix the wires to obtain a flexible sensor.
[0078] The present application also provides a flexible sensor, which is prepared by the method for preparing the flexible sensor described in the second embodiment above.
[0079] The method for preparing the flexible sensor of the present application first provides a first flexible substrate and a second flexible substrate with conductivity, wherein one side surface of the first flexible substrate has a first microstructure array, and one side surface of the second flexible substrate has a second microstructure array, and then a dielectric layer is formed in the microstructure gap of the first microstructure array and in the microstructure gap of the first microstructure array, respectively, and then the first flexible substrate and the second flexible substrate are assembled, wherein the first microstructure array and the second microstructure array face each other and the microstructures are mutually staggered, so as to form a structure in which the microstructures and the microstructure gaps match each other between the microstructure arrays, and thus a flexible sensor is obtained. The preparation process is simple and the cost is low.
[0080] The above embodiments are merely illustrative of the principles and effects of the present application and are not intended to limit the present application. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present application. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present application shall still be covered by the claims of the present application.
Claims
1. A flexible sensor for an intelligent robot, characterized in that: The invention can detect sliding signals and tactile signals at the same time, and comprises a first flexible substrate and a second flexible substrate, wherein the first flexible substrate and the second flexible substrate are conductive, a first microstructure array is provided on one side surface of the first flexible substrate, a second microstructure array is provided on one side surface of the second flexible substrate, a dielectric layer is provided on the microstructure gaps of the first microstructure array and the microstructure gaps of the second microstructure array, the first microstructure array and the second microstructure array are arranged facing each other and the microstructures are staggered with each other to form a structure in which the microstructures and the microstructure gaps match each other between the microstructure arrays.
2. The flexible sensor according to claim 1, characterized in that: The first microstructure array and the second microstructure array include at least one of a pyramid microstructure array, a cone microstructure array, and a hemispherical microstructure array; and / or Conductive material is dispersed in the first flexible substrate and the second flexible substrate, and the conductive material includes at least one of carbon nanotubes, graphene, carbon black, and silver nanowires.
3. The flexible sensor according to claim 1 or 2, characterized in that: The first flexible substrate and the second flexible substrate are porous structures.
4. The flexible sensor according to claim 1, characterized in that: The microstructures in the first microstructure array and the microstructures in the second microstructure array are not in contact with each other, and the microstructures in the first microstructure array and the microstructures in the second microstructure array are respectively bonded to the dielectric layer in the microstructure gaps on the opposite side.
5. The flexible sensor according to claim 4, characterized in that: The dielectric layer is made of a dielectric material having a melting temperature lower than the melting temperatures of the bases of the first flexible substrate and the second flexible substrate.
6. A method for preparing a flexible sensor for an intelligent robot, characterized in that: The flexible sensor can detect sliding signals and tactile signals simultaneously, and the preparation method comprises: a. providing a first flexible substrate and a second flexible substrate having conductivity, wherein one side surface of the first flexible substrate has a first microstructure array, one side surface of the second flexible substrate has a second microstructure array, and the microstructure gaps of the first microstructure array and the microstructure gaps of the second microstructure array are both provided with a dielectric layer; b. Assembling the first flexible substrate and the second flexible substrate, the first microstructure array and the second microstructure array are facing each other and the microstructures are mutually offset to form a structure in which the microstructures and the microstructures have gaps between the microstructure arrays; c. Get the flexible sensor.
7. The method for preparing a flexible sensor according to claim 6, characterized in that: Step a includes: preparing a mixture comprising a polymer prepolymer, a conductive material, a pore former and a curing agent; The mixture is placed in a template having a microstructure array cavity on one side and cured into a shape; Demolding and removing the pore-forming agent to obtain a conductive flexible substrate having a microstructure array on one surface; The above process is repeated or the conductive flexible substrate is cut to obtain the first flexible substrate and the second flexible substrate without a dielectric layer on the surface.
8. The method for preparing a flexible sensor according to claim 7, characterized in that: The first microstructure array and the second microstructure array include at least one of a pyramid microstructure array, a cone microstructure array, and a hemispherical microstructure array; and / or The conductive material includes at least one of carbon nanotubes, graphene, carbon black, and silver nanowires; and / or The pore formers are particles that can be dissolved or removed by chemical reaction.
9. The method for preparing a flexible sensor according to claim 7, characterized in that: Step a includes: Coating a dielectric layer on the surface of the first flexible substrate and the second flexible substrate having no dielectric layer on the surface thereof, respectively, on one side having the microstructure array; The dielectric layer on each flexible substrate is patterned respectively, and the portion of the dielectric layer located in the microstructure gap is retained.
10. The method for preparing a flexible sensor according to claim 6, characterized in that: The dielectric layer is prepared by using a dielectric material having a melting temperature lower than the melting temperature of the base of the first flexible substrate and the second flexible substrate, and step c comprises: The assembled structure is heated to melt the dielectric layer and bond it to the microstructures in the gaps between the microstructures.
11. A flexible sensor for an intelligent robot, characterized in that: The flexible sensor can detect sliding signals and tactile signals simultaneously, and is prepared by the method for preparing a flexible sensor for an intelligent robot as described in any one of claims 6 to 10.