A gallium nitride wafer production process parameter design method
By designing the process parameters of the gallium nitride wafer, it is divided into three stages: filming, grinding and scribing, and the optimization conditions are determined, which solves the problems of high processing difficulty and low yield during the processing process of GaN materials, and improves the wafer Quality and efficiency.
Patent Information
- Application Number
- CN202011176972.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-10-28
AI Technical Summary
Gallium nitride (GaN) materials have problems such as difficult processing and low yield during wafer processing, which leads to easy breakage during semiconductor packaging grinding, and low efficiency and quality.
A gallium nitride wafer production process parameter design method is adopted. By designing the grinding film, grinding wheel and scribing parameters, it is divided into three stages: film patching, grinding and scribing, and the optimal process conditions are determined, including film patching speed , grinding speed, rotation speed, cutting volume and water flow parameters to ensure the accuracy and adaptability of the production process.
The yield rate of gallium nitride wafers is improved, the accuracy and suitability of production process parameters are ensured, and the processing efficiency and quality are improved.
Smart Images

Figure CN112287543B_ABST
Abstract
Description
[Technical field]
[0001] The invention belongs to the field of wafer processing, and in particular relates to a method for designing process parameters for gallium nitride wafer production. [Background technology]
[0002] Gallium nitride (GaN) is a new type of wafer material with the advantages of strong piezoelectricity (due to non-centrosymmetry) and ferroelectricity (spontaneous polarization along the hexagonal c-axis). Especially through the effect of heterojunction, its effective transport performance is not inferior to GaAs, and the effect of making microwave power devices (in terms of microwave output power density) is often far superior to all existing semiconductor materials.
[0003] Due to the special characteristics of the material, GaN material is difficult to process in the semiconductor packaging grinding and dicing process, is easy to break, and has a relatively low yield rate. [Summary of the invention]
[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a gallium nitride wafer production process parameter design method to solve the technical problems in the prior art that GaN materials are difficult to process, easy to break, and have low yield.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A gallium nitride wafer production process parameter design method comprises the following steps:
[0007] Step 1, determining the DOE matrix of the production process according to the existing production data, wherein the parameters of the DOE matrix include a grinding film, a grinding wheel, a grinding parameter, and a scribing parameter;
[0008] Step 2: According to the parameters of the DOE matrix, the GaN test piece is filmed, and then verified to determine the filming parameters;
[0009] Step 3, according to the parameters of the DOE matrix, the test piece of gallium nitride is ground and verified to determine the grinding parameters;
[0010] Step 4, according to the parameters of the DOE matrix, the test wafer of the gallium nitride is scribed and verified to determine the scribing parameters;
[0011] Step 5, producing gallium nitride wafers based on the above-mentioned film attaching parameters, grinding parameters and dicing parameters. When the yield rate reaches 100%, the above-mentioned film attaching parameters, grinding parameters and dicing parameters are determined as production process parameters.
[0012] A further improvement of the present invention is:
[0013] Preferably, in step 2, the film-sticking parameters include film-sticking speed, film-sticking pressure, film-sticking tension, workbench temperature and blade temperature.
[0014] Preferably, in step 2, the film-sticking speed is 5-20 mm / sec, the film-sticking pressure is 0.56 MPa, the main pressure of the film-sticking tension is 0.56 MPa, the workbench temperature is 20°C-60°C, and the blade temperature is 170°C.
[0015] Preferably, in step 3, the grinding parameters include coarse grinding speed, fine grinding speed, the rotation speed of the spindle during coarse grinding and fine grinding, the grinding amount and the grinding wheel model.
[0016] Preferably, in step 3, coarse grinding is divided into three stages, the speed of the first stage is 3-8um / s, the speed of the second stage is 2-6um / s, and the speed of the third stage is 1-4um / s; fine grinding is divided into two stages, the speed of the first stage is 0.2-0.8um / s, and the speed of the second stage is 0.1-0.6um / s.
[0017] Preferably, in step 3, the rotation speed of the spindle during coarse grinding is 500-5000 rpm, and the rotation speed of the spindle during fine grinding is 1000-5700 rpm.
[0018] Preferably, in step 4, the dicing parameters include feed speed, spindle speed, blade penetration and water flow rate.
[0019] Preferably, in step 4, the feed speed is 7-60 mm / s; the spindle speed of the first cutter is 20000-55000 rpm, and the spindle speed of the second cutter is 20000-55000 rpm.
[0020] Preferably, in step 4, the cutting thickness of the first cutter is 1 / 3-2 / 3 of the thickness of the wafer, and after the second cutter cuts through the wafer, it cuts into the film 15-40 um.
[0021] Preferably, in step 4, the water flow rate is 0.6±0.3MΩ.cm 2 .
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention discloses a gallium nitride wafer production process parameter design method. The method performs DOE design on all parameters used in producing wafers using GaN materials, divides the design into three stages: film pasting, grinding and dicing, and determines the optimal process conditions for the three stages, so that the designed parameters are accurate and suitable for production conditions, thereby improving the yield rate.
Brief Description of the Drawings
[0024] Figure 1is a flow chart of the present invention; [Specific implementation method]
[0025] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0026] See also Figure 1 The present invention discloses a method for designing process parameters for gallium nitride wafer production, the method comprising the following steps:
[0027] Step 1: Obtain GaN test pieces and determine the DOE test plan to determine the grinding film, grinding wheel, grinding parameters, dicing parameters and process control when producing GaN wafers.
[0028] The function of the grinding disc film is to be a front protective film. Choose a front film with a thick adhesive layer, strong support and good wrapping properties.
[0029] Coarse grinding wheel: the particle size can be selected from Disco 320#; fine grinding wheel: the particle size can be selected from Disco 2000#, 6000#, 8000#.
[0030] Step 2, according to the DOE matrix, use the Nitto film laminating machine to verify the film laminating of the GaN test piece, and obtain the film laminating process parameter conditions suitable for this GaN piece, wherein the process parameters include a film laminating speed of 5 to 20 mm / sec, preferably 10 mm / sec, a main pressure of 0.560 MPa, preferably 80%, preferably pressure A (0 position, 40%), pressure B (45 mm position, 50%), pressure C (90 mm position, 60%), pressure D (135 mm position, 50%), pressure E (180 mm position, 40%), preferably 80%, a workbench temperature of 20°C-60°C, preferably 40°C, a blade temperature of 170°C, and a lower knife angle of inward, outward and free angle, preferably a free angle.
[0031] Step 3, according to the DOE matrix, a DISCO grinder is used to perform grinding verification on a GaN test piece, and grinding process conditions suitable for the GaN piece are obtained. The grinding process is divided into coarse grinding and fine grinding. The process parameters include grinding speed. The coarse grinding is divided into three stages, the speed of the first stage is 3-8um / s, the speed of the second stage is 2-6um / s, and the speed of the third stage is 1-4um / s. The fine grinding is divided into two stages, the speed of the first stage is 0.2-0.8um / s, and the speed of the second stage is 0.1-0.6um / s. The preferred coarse grinding three The speeds of the stages are 5um / s, 3um / s and 1um / s respectively, the rotation speeds of the two stages of fine grinding are 0.4um / s and 0.3um / s respectively, the rotation speed of the spindle during coarse grinding is 4500-5000rpm, preferably 4800rpm, the rotation speed of the spindle during fine grinding is 1000-5700rpm, preferably 3500rpm, the grinding amount is 20μm-40μm, preferably 35um, the particle size of the grinding wheel model of the coarse grinding wheel is 320#; the particle size of the grinding wheel model of the fine grinding wheel is 6000#.
[0032] Step 4: According to the DOE matrix, the DISCO dicing machine is used to verify the dicing process for the GaN test wafer, and the dicing process conditions suitable for this material are obtained. The dicing process includes two dicing tools, namely the first cutter and the second cutter. Each cutter is connected to a spindle. The first cutter is used to cut the wafer to 1 / 2-2 / 3 of its thickness, and the second cutter is used to cut through the wafer and then cut into the film. During the cutting process, the feed speed of the two dicing tools is 7-60mm / s, preferably 25mm / s, the spindle speed of the first cutter is 20000-55000rpm, preferably 42000rpm, the spindle speed of the second cutter is 20000-55000rpm, preferably 35000rpm, the thickness of the product cut by the first cutter is 1 / 3-2 / 3 of the product thickness, preferably 240um, the second cutter, after cutting through the wafer, cuts into the film with a thickness of 15-40um, preferably 55um), the water flow rate of pure water is 0.6±0.3MΩ.cm 2 , preferably 0.5MΩ.cm 2 .
[0033] Step 5: Use the best process parameters of steps 2, 3 and 4 to conduct a small batch trial production of the formal wafers, follow up the stability, and plan to follow up the processing of 50 wafers. The yield rate reaches 100%, which can meet the formal mass production.
[0034] Step 6: Collect data and control points of small-batch trial production, assign process parameters to dedicated WI, update them in the reduction process control standards, update process problems in the OCAP file, and improve the PFMEA file of this type of wafer material.
[0035] Table 1 The following table is the PFMEA form
[0036] Station Verification Project standard Sampling volume Film Film appearance No film filaments, bubbles and wrinkles 100% Thinning Grinding current value 5-15A 5pcs / piece Thinning thickness Grinding thickness ±10um 25pcs / group Thinning TTV ≤5um 25pcs / group Thinning Roughness Ra≤45nm 5pcs / group Slicing Blade life Product thickness + cut into blue film + allowance 100% Slicing Collapse Do not damage the outermost safety line 25pcs / group Slicing Back Collapse Back collapse height < 1 / 2 chip thickness 25pcs / group Slicing Side collapse Side collapse height <1 / 2 chip thickness 25pcs / group
[0037] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A gallium nitride wafer production process parameter design method, characterized in that: The following steps are involved: Step 1, determining the DOE matrix of the production process according to the existing production data, wherein the parameters of the DOE matrix include a grinding film, a grinding wheel, a grinding parameter, and a scribing parameter; Step 2: According to the parameters of the DOE matrix, the GaN test piece is filmed, and then verified to determine the filming parameters; The film-sticking parameters include film-sticking speed, film-sticking pressure, film-sticking tension, workbench temperature and blade temperature; In step 2, the film sticking speed is 5-20 mm / sec, the film sticking pressure is 0.56 MPa, the main pressure of the film sticking tension is 0.56 MPa, the workbench temperature is 20° C.-60° C., and the blade temperature is 170° C.; Step 3, according to the parameters of the DOE matrix, the test piece of gallium nitride is ground and verified to determine the grinding parameters; Grinding parameters include coarse grinding speed, fine grinding speed, spindle speed during coarse and fine grinding, grinding fine grinding amount and grinding wheel model; The coarse grinding is divided into three stages. The speed of the first stage is 3-8um / s, the speed of the second stage is 2-6um / s, and the speed of the third stage is 1-4um / s. Fine grinding is divided into two stages, the speed of the first stage is 0.2-0.8um / s, and the speed of the second stage is 0.1-0.6um / s; The spindle speed is 500-5000rpm during coarse grinding, and the spindle speed is 1000-5700rpm during fine grinding; Step 4, according to the parameters of the DOE matrix, the test wafer of the gallium nitride is scribed and verified to determine the scribing parameters; Slicing parameters include feed speed, spindle speed, blade penetration and water flow rate; The feed speed is 7-60mm / s; the spindle speed of the first cutter is 20000-55000rpm, and the spindle speed of the second cutter is 20000-55000rpm; The first cutter cuts into 1 / 3-2 / 3 of the wafer thickness. The second cutter cuts through the wafer and into the film 15-40um. Water flow rate is 0.6±0.3MΩ.cm 2 ; Step 5, producing gallium nitride wafers based on the above-mentioned film attaching parameters, grinding parameters and dicing parameters. When the yield rate reaches 100%, the above-mentioned film attaching parameters, grinding parameters and dicing parameters are determined as production process parameters.