An integrated light conversion glass diffuser plate and a method for preparing the same

By embedding quantum dot light conversion layer in the glass diffusion plate and using optical glue as the adhesive layer, the problems of poor weather resistance and high cost of traditional plastic diffusion plates are solved, and high color gamut, thin thickness and low cost optical conversion glass is achieved. Diffusion plate extends service life and improves the stability of quantum dots.

CN112363260BActive Publication Date: 2024-11-05CHANGZHOU ALMADEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011385857.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-01
Publication Date
2024-11-05
Estimated Expiration
2040-12-01

AI Technical Summary

Technical Problem

Traditional plastic diffusion plates have poor weather resistance, and conventional quantum dot diaphragms increase the thickness and processing cost of the diffusion plate, and have a lower color gamut.

Method used

The integrated light conversion glass diffusion plate is adopted, including a glass substrate, a diffusion layer, a quantum dot light conversion layer and an adhesive layer. The quantum dots are embedded inside the glass. Optical glue is used as an adhesive layer and medium to reduce the use of quantum film and improve the color gamut. and stability.

Benefits of technology

The photoconverted glass diffusion plate with higher color gamut, thinner thickness and lower processing cost is achieved, extending service life and improving the stability of quantum dots.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112363260B_ABST
    Figure CN112363260B_ABST
Patent Text Reader

Abstract

The present invention discloses an integrated light conversion glass diffusion plate and a preparation method thereof. It includes a glass substrate, a diffusion layer, a quantum dot light conversion layer, an adhesive layer and an optical film; the diffusion layer is arranged on the light emitting surface of the glass substrate, the quantum dot light conversion layer is attached to the diffusion layer, and the optical film is bonded to the quantum dot light conversion layer through the adhesive layer; the diffusion layer is formed by coating a light diffusion material on the glass substrate and curing; the light diffusion material includes the following components in weight percentage: 45-55% resin, 30-40% diffusion particles, 10-15% diluent and 1-5% silane coupling agent; the quantum dot light conversion layer is formed by dispersing quantum dots in silicone ink or UV glue and coating the diffusion layer and curing. The integrated light conversion glass diffusion plate of the present invention embeds quantum dots into the interior of the glass diffusion plate in an integrated manner, reduces the use of quantum films, reduces costs, and has a thinner product thickness. The integrated light conversion glass diffusion plate of the present invention has a high color gamut, and the embedded quantum dot light conversion layer increases the color gamut by 30%, and has a long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of diffuser plate preparation, and in particular to an integrated light conversion glass diffuser plate and a preparation method thereof. Background Art

[0002] Traditional diffusers usually use inorganic or organic light diffusers added to PMMA, PC, PS, PP and other base materials as scattering particles, so that the light will be refracted, reflected and scattered in two media with different refractive indices when passing through the scattering layer, thereby changing the light's path and achieving full scattering of the incident light to produce an optical diffusion effect. However, plastic materials such as PMMA, PC, PS, PP all have the common characteristics of swelling when absorbing moisture, bending when heated, and shrinking when cooled. Smaller diffusers do not change much, but large diffusers change significantly. When used alone, the material is relatively soft, and the support is not strong enough to easily cause the front and back to warp.

[0003] The light source of the diffuser is generally white light or blue light. The blue light needs to excite the red and green light conversion units and mix with the blue light to form white light. The diffuser with blue light as the light source has a higher color gamut than the diffuser with white light as the light source, but a light conversion unit needs to be introduced. The most commonly used light conversion units are quantum dots and phosphors. Quantum dots are a kind of nano-scale crystals composed of semiconductor materials. Compared with fluorescent particles, quantum dot nanomaterials have many advantages. For example, quantum dots can produce more intensive light in a narrow wavelength band and have high stability. They have excellent fluorescence emission properties in the visible light region, the excitation spectrum is continuously distributed, and the fluorescence peak position can be adjusted according to its physical size. Generally, the diffuser needs to be matched with a quantum dot membrane. The quantum dot membrane increases the thickness of the diffuser and increases the assembly process of the diffuser. Summary of the invention

[0004] The purpose of the present invention is to propose an integrated light-conversion glass diffuser plate in view of the poor weather resistance of plastic diffuser plates, the increase in the thickness of the diffuser plates and the increase in processing costs caused by conventional quantum dot membranes; the integrated light-conversion glass diffuser plate of the present invention has a higher color gamut, better color expression, thinner thickness and lower processing cost; another purpose of the present invention is to provide a simple method for preparing an integrated light-conversion glass diffuser plate.

[0005] The present invention is achieved through the following technical solutions:

[0006] An integrated light conversion glass diffusion plate, characterized in that it includes a glass substrate, a diffusion layer, a quantum dot light conversion layer, an adhesive layer and an optical film; the diffusion layer is arranged on the light emitting surface of the glass substrate, the quantum dot light conversion layer is attached to the diffusion layer, and the optical film is bonded to the quantum dot light conversion layer through the adhesive layer; the diffusion layer is formed by coating a light diffusion material on the glass substrate and curing; the light diffusion material includes the following components in weight percentage: 45-55% resin, 30-40% diffusion particles, 10-15% diluent and 1-5% silane coupling agent; the quantum dot light conversion layer is formed by dispersing quantum dots in silicone ink or UV glue and coating the diffusion layer and curing. The present invention embeds quantum dots into the interior of the glass diffusion plate in an integrated manner, reduces the use of quantum films, reduces costs, and due to the reduction in the use of quantum films, the thickness of the integrated light conversion glass diffusion plate of the present invention is greatly reduced. In addition, the integrated light conversion glass diffuser plate of the present invention plays the role of bonding the optical film by setting the adhesive layer, and also plays the role of isolating moisture and oxygen, further improving the stability of the quantum dots and solving the problem that quantum dots are afraid of water and oxygen. The light diffusion material is attached to the light emitting surface of the glass substrate, and after curing, the adhesion between the light diffusion material and the glass substrate is increased. At the same time, the diffusion particles added to the light diffusion material can scatter the incident light, making the light emission more uniform. In addition, the adhesion between silicone ink or UV glue and the glass substrate is not enough, and the light diffusion material can be used as a medium to improve the adhesion with the glass substrate and increase the service life.

[0007] Furthermore, a scattering pattern for increasing the light scattering effect is provided on the light incident surface of the glass substrate. Preferably, the glass substrate may be a flat glass or a patterned glass. Preferably, a scattering pattern is provided on the light incident surface of the glass substrate to further improve the scattering effect of the incident light and make the light output more uniform. Specifically, the scattering pattern is provided on the side of the glass substrate away from the diffusion layer.

[0008] Furthermore, the thickness of the diffusion layer is 30-80 μm; the thickness of the quantum dot light conversion layer is 5-40 μm.

[0009] Furthermore, the material of the adhesive layer is optical glue. Preferably, the optical glue has high light transmittance and good bonding strength, and can be cured and formed at room temperature.

[0010] Furthermore, the resin is acrylic resin; the diffusion particles are titanium dioxide or silicon dioxide particles; the diluent is a mixture of divalent acid ester and isophorone; and the silane coupling agent is KH570.

[0011] Furthermore, the particle size of the titanium dioxide or silicon dioxide particles is 5-10 microns; the volume ratio of the divalent ester to the isophorone is (1-2): (1-2).

[0012] A method for preparing an integrated light conversion glass diffuser plate, characterized in that the method comprises the following steps:

[0013] S1, adding resin, diffusion particles and silane coupling agent into a diluent and stirring evenly to obtain a light diffusion material; coating the light diffusion material on the light emitting surface of the glass substrate and curing at 200-260° C. for 30-60 minutes to form the diffusion layer;

[0014] S2, dispersing the quantum dots in silica gel ink to obtain quantum dot light conversion glue A; or dispersing the quantum dots in UV glue to obtain quantum dot light conversion glue B;

[0015] S3, coating the quantum dot light conversion glue A on the diffusion layer, and curing at 80-120°C for 20-40 minutes to form the quantum dot light conversion layer; or coating the quantum dot light conversion glue B on the diffusion layer, and curing at 100-200W / cm 2 UV curing for 15-45 seconds under UV irradiation to form the quantum dot light conversion layer

[0016] S4, then coating the optical glue on the quantum dot light conversion layer to form the bonding layer;

[0017] S5. Finally, the optical film is attached to the adhesive layer to obtain an integrated light conversion glass diffuser plate. The present invention provides a simple method for preparing an integrated light conversion glass diffuser plate, which has a simple preparation process and low cost.

[0018] Furthermore, the light diffusion material in step S1 is coated on the light emitting surface of the glass substrate by screen printing.

[0019] Furthermore, the mass ratio of the quantum dots described in step S2 to the silicone ink or UV glue is (5-40): (60-95); the quantum dots include red light quantum dots and green light quantum dots, and the mass ratio of the red light quantum dots to the green light quantum dots is 1:1; the wavelength of the red light quantum dots is 620-630nm, and the wavelength of the green light quantum dots is 520-530nm.

[0020] Beneficial effects of the present invention:

[0021] (1) The integrated light-conversion glass diffuser plate of the present invention embeds quantum dots into the interior of the glass diffuser plate, reduces the use of quantum films, reduces costs, and greatly reduces the thickness of the product due to the reduction in the use of quantum films. The present invention uses optical glue to not only bond the optical film to the quantum dot light conversion layer, but also isolate moisture and oxygen, further improving the stability of the quantum dots and solving the problem that quantum dots are afraid of water and oxygen. The light diffusion material in the present invention is attached to the light-emitting surface of the glass substrate, and after curing, the adhesion between the light diffusion material and the glass substrate is increased, and the addition of diffusion particles to the light diffusion material can further scatter the incident light, making the light output more uniform. In addition, the adhesion between silicone ink or UV glue and the glass substrate is insufficient, and the light diffusion material can be used as a medium to improve the adhesion between the light diffusion material and the glass substrate, thereby increasing the service life.

[0022] (2) The integrated light-conversion glass diffuser plate of the present invention has a higher color gamut (embedded quantum dot light-conversion layer can increase the color gamut by 30%), better color expression, thinner thickness, low processing cost, and long service life; the preparation method of the integrated light-conversion glass diffuser plate of the present invention has a simple preparation process and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 It is a schematic structural diagram of the integrated light conversion glass diffuser plate of the present invention.

[0025] In the figure: 1 glass substrate, 2 diffusion layer, 3 quantum dot light conversion layer, 4 adhesive layer, 5 optical film, 6 scattering pattern, 21 diffusion particles, 31 quantum dots. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] An integrated light conversion glass diffusion plate comprises a glass substrate 1, a diffusion layer 2, a quantum dot light conversion layer 3, an adhesive layer 4 and an optical film 5; the diffusion layer 2 is arranged on the light emitting surface of the glass substrate 1, the quantum dot light conversion layer 3 is attached to the diffusion layer 2, and the optical film 5 is bonded to the quantum dot light conversion layer 3 through the adhesive layer 4 (the material of the adhesive layer 4 is optical glue); the diffusion layer 2 is formed by coating a light diffusion material on the glass substrate 1 and curing it; the light diffusion material comprises the following components in weight percentage: 50% resin, 35% diffusion particles, 5% silane coupling agent and 10% diluent; the quantum dot light conversion layer 3 is formed by dispersing quantum dots 31 in UV glue and coating it on the diffusion layer 2 and curing it.

[0029] Preferably, a scattering pattern 6 is provided on the light incident surface of the glass substrate 1, and the scattering pattern 6 is used to increase the scattering effect of the incident light. Preferably, the thickness of the diffusion layer 2 is set to 60 μm, and the thickness of the quantum dot light conversion layer 3 is set to 20 μm.

[0030] The method for preparing the above-mentioned integrated light conversion glass diffuser plate comprises the following steps:

[0031] S1. Add the resin, the diffusion particles 21 and the silane coupling agent into the diluent and stir evenly to obtain a light diffusion material; then apply the light diffusion material on the light emitting surface of the glass substrate 1 by screen printing, and cure it at 200° C. for 30 minutes to form the diffusion layer 2 (the thickness of the diffusion layer 2 is set to 60 μm); wherein: the resin is acrylic resin; the diffusion particles 21 are titanium dioxide particles, and the particle size of the titanium dioxide particles is 8 μm; the silane coupling agent is KH570; and the diluent is a mixture of divalent acid ester and isophorone in a volume ratio of 1:1;

[0032] S2, mixing the quantum dots 31 with UV glue to obtain quantum dot light conversion glue B; wherein: the quantum dots 31 include red light quantum dots and green light quantum dots, and the mass ratio of the red light quantum dots to the green light quantum dots is 1:1; the wavelength of the red light quantum dots is 625nm, and the wavelength of the green light quantum dots is 520nm; the mass ratio of the red light quantum dots, the green light quantum dots and the UV glue is 20:20:60;

[0033] S3, coating the quantum dot light conversion glue B on the diffusion layer 2, and 2 UV curing for 20 seconds under UV irradiation to form the quantum dot light conversion layer 3 (the thickness of the quantum dot light conversion layer 3 is set to 20 μm);

[0034] S4, then coating the optical glue on the quantum dot light conversion layer 3 to form an adhesive layer 4;

[0035] S5. Finally, the optical film 5 is attached to the adhesive layer 4 to obtain an integrated light conversion glass diffuser plate.

[0036] The color gamut (sRGB) and service life of the integrated light conversion glass diffuser plate prepared in Example 1 were tested using a blue light source, as shown in Table 1.

[0037] Example 2

[0038] An integrated light conversion glass diffusion plate comprises a glass substrate 1, a diffusion layer 2, a quantum dot light conversion layer 3, an adhesive layer 4 and an optical film 5; the diffusion layer 2 is arranged on the light emitting surface of the glass substrate 1, the quantum dot light conversion layer 3 is attached to the diffusion layer 2, and the optical film 5 is bonded to the quantum dot light conversion layer 3 through the adhesive layer 4 (the material of the adhesive layer 4 is optical glue); the diffusion layer 2 is formed by coating a light diffusion material on the glass substrate 1 and curing it; the light diffusion material comprises the following components in weight percentage: 45% resin, 40% diffusion particles, 12% diluent and 3% silane coupling agent; the quantum dot light conversion layer 3 is formed by dispersing quantum dots 31 in silicone ink and coating it on the diffusion layer 2 and curing it.

[0039] Preferably, a scattering pattern 6 is provided on the light incident surface of the glass substrate 1, and the scattering pattern 6 is used to increase the scattering effect of the incident light. Preferably, the thickness of the diffusion layer 2 is set to 30 μm, and the thickness of the quantum dot light conversion layer 3 is set to 5 μm.

[0040] The method for preparing the above-mentioned integrated light conversion glass diffuser plate comprises the following steps:

[0041] S1. Add the resin, silane coupling agent and diffusion particles 21 into the diluent and stir evenly to obtain a light diffusion material; then apply the light diffusion material on the light emitting surface of the glass substrate 1 by screen printing, and cure at 260° C. for 40 minutes to form the diffusion layer 2 (the thickness of the diffusion layer 2 is set to 30 μm); wherein: the resin is acrylic resin; the diffusion particles 21 are silica particles, and the particle size of the silica particles is 5 μm; the silane coupling agent is KH570; and the diluent is a mixture of divalent acid ester and isophorone in a volume ratio of 1:2;

[0042] S2, mixing the quantum dots 31 with the silicone ink to obtain quantum dot light conversion glue A; wherein: the quantum dots 31 include red light quantum dots and green light quantum dots, and the mass ratio of the red light quantum dots to the green light quantum dots is 1:1; the wavelength of the red light quantum dots is 620nm, and the wavelength of the green light quantum dots is 530nm; the mass ratio of the red light quantum dots, the green light quantum dots and the UV glue is 10:10:80;

[0043] S3, coating the quantum dot light conversion glue A on the diffusion layer 2, and curing it at 80° C. for 40 minutes to form the quantum dot light conversion layer 3 (the thickness of the quantum dot light conversion layer 3 is set to 5 μm);

[0044] S4, then coating the optical glue on the quantum dot light conversion layer 3 to form an adhesive layer 4;

[0045] S5. Finally, the optical film 5 is attached to the adhesive layer 4 to obtain an integrated light conversion glass diffuser plate.

[0046] The color gamut (sRGB) and service life of the integrated light conversion glass diffuser plate prepared in Example 2 were tested using a blue light source, as shown in Table 1.

[0047] Example 3

[0048] An integrated light conversion glass diffusion plate comprises a glass substrate 1, a diffusion layer 2, a quantum dot light conversion layer 3, an adhesive layer 4 and an optical film 5; the diffusion layer 2 is arranged on the light emitting surface of the glass substrate 1, the quantum dot light conversion layer 3 is attached to the diffusion layer 2, and the optical film 5 is bonded to the quantum dot light conversion layer 3 through the adhesive layer 4 (the material of the adhesive layer 4 is optical glue); the diffusion layer 2 is formed by coating a light diffusion material on the glass substrate 1 and curing it; the light diffusion material comprises the following components in weight percentage: 54% resin, 30% diffusion particles, 1% silane coupling agent and 15% diluent; the quantum dot light conversion layer 3 is formed by dispersing quantum dots 31 in silicone ink and coating it on the diffusion layer 2 and curing it.

[0049] Preferably, a scattering pattern 6 is provided on the light incident surface of the glass substrate 1, and the scattering pattern 6 is used to increase the scattering effect of the incident light. Preferably, the thickness of the diffusion layer 2 is set to 80 μm, and the thickness of the quantum dot light conversion layer 3 is set to 40 μm.

[0050] The method for preparing the above-mentioned integrated light conversion glass diffuser plate comprises the following steps:

[0051] S1. Add the resin, the silane coupling agent and the diffusion particles 21 into the diluent and stir evenly to obtain a light diffusion material; then apply the light diffusion material on the light emitting surface of the glass substrate 1 by screen printing, and cure at 230° C. for 60 minutes to form a diffusion layer 2 (the thickness of the diffusion layer 2 is set to 80 μm); wherein: the resin is acrylic resin; the diffusion particles 21 are titanium dioxide particles, and the particle size of the titanium dioxide particles is 10 μm; the silane coupling agent is KH570; and the diluent is a mixture of divalent acid ester and isophorone in a volume ratio of 2:1;

[0052] S2, the quantum dots 31 and the silicone ink are mixed to obtain quantum dot light conversion glue A; wherein: the quantum dots 31 include red light quantum dots and green light quantum dots, and the mass ratio of the red light quantum dots to the green light quantum dots is 1:1; the wavelength of the red light quantum dots is 630nm, and the wavelength of the green light quantum dots is 525nm; the mass ratio of the red light quantum dots, the green light quantum dots and the UV glue is 2.5:2.5:95;

[0053] S3, coating the quantum dot light conversion glue A on the diffusion layer 2, and curing it at 100° C. for 20 minutes to form the quantum dot light conversion layer 3 (the thickness of the quantum dot light conversion layer 3 is set to 40 μm);

[0054] S4, then coating the optical glue on the quantum dot light conversion layer 3 to form an adhesive layer 4;

[0055] S5. Finally, the optical film 5 is attached to the adhesive layer 4 to obtain an integrated light conversion glass diffuser plate.

[0056] The color gamut (sRGB) and service life of the integrated light conversion glass diffuser plate prepared in Example 3 were tested using a blue light source, as shown in Table 1.

[0057] Comparative Example 1

[0058] An integrated light conversion glass diffusion plate comprises a glass substrate 1, a quantum dot light conversion layer 3, an adhesive layer 4 and an optical film 5; the quantum dot light conversion layer 3 is directly arranged on the light emitting surface of the glass substrate 1, and the optical film 5 is bonded to the quantum dot light conversion layer 3 through the adhesive layer 4 (the material of the adhesive layer 4 is optical glue); the quantum dot light conversion layer 3 is formed by dispersing quantum dots 31 in UV glue and coating the diffusion layer 2 and curing. Preferably, a scattering pattern 6 is arranged on the light incident surface of the glass substrate 1, and the scattering pattern 6 is used to increase the scattering effect of the incident light; the thickness of the quantum dot light conversion layer 3 is set to 20μm.

[0059] The difference between Comparative Example 1 and Example 1 is that the diffusion layer 2 is not provided in Comparative Example 1, and the quantum dot light conversion layer 3 is directly provided on the light emitting surface of the glass substrate 1 in Comparative Example 1, and the rest is the same as Example 1.

[0060] The color gamut and service life of the diffuser plate produced by the blue light source test are shown in Table 2.

[0061] Comparative Example 2

[0062] An integrated light conversion glass diffusion plate comprises a glass substrate 1, a diffusion layer 2 and an optical film 5; the diffusion layer 2 is arranged on the light emitting surface of the glass substrate 1, and the optical film 5 is directly attached to the diffusion layer 2; the diffusion layer 2 is formed by coating a light diffusion material on the glass substrate 1 and curing it; and the light diffusion material comprises the following components in weight percentage: 50% of resin, 35% of diffusion particles, 5% of silane coupling agent and 10% of diluent.

[0063] The difference between Comparative Example 2 and Example 1 is that the quantum dot light conversion layer 3 and the adhesive layer 4 are not provided in Comparative Example 2. In Comparative Example 2, the optical film 5 is directly attached to the diffusion layer 2. The rest is the same as Example 1.

[0064] The color gamut and service life of the diffuser plate obtained by testing with a white light source are shown in Table 2.

[0065] Table 1 Performance parameters of the integrated light conversion glass diffuser plate prepared in Examples 1-3 of the present invention

[0066]

[0067]

[0068] Table 2 Performance parameters of the diffuser plate obtained in Comparative Example 1-2

[0069] Comparative Example Color gamut sRGB Service life / h Comparative Example 1 >130% Failure Comparative Example 2 100% qualified

[0070] It can be seen from the above-mentioned comparative example 1 and the test data that the adhesion of the quantum dot light conversion layer 3 directly coated on the surface of the glass substrate 1 is poor, which greatly affects the service life of the diffuser plate, and its service life is unqualified; it can be seen from the above-mentioned comparative example 2 and the test data of Tables 1 and 2 that embedding the quantum dot light conversion layer 3 can increase the color gamut of the diffuser plate by 30%.

[0071] The above are preferred embodiments of the present invention and are only used to explain the present invention, not to limit the present invention. Any obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. An integrated light conversion glass diffuser plate, characterized in that: The invention comprises a glass substrate (1), a diffusion layer (2), a quantum dot light conversion layer (3), an adhesive layer (4) and an optical film (5); the diffusion layer (2) is arranged on the light emitting surface of the glass substrate (1), the quantum dot light conversion layer (3) is attached to the diffusion layer (2), and the optical film (5) is bonded to the quantum dot light conversion layer (3) through the adhesive layer (4); the diffusion layer (2) is formed by coating a light diffusion material on the glass substrate (1) and curing the light diffusion material; the light diffusion material comprises the following components in weight percentage: 45-55% of resin, 30-40% of diffusion particles, 10-15% of diluent and 1-5% of silane coupling agent; the quantum dot light conversion layer (3) is formed by dispersing quantum dots in silicone ink or UV glue and coating the diffusion layer (2) and curing the resulting material.

2. The integrated light conversion glass diffuser plate according to claim 1, characterized in that: A scattering pattern (6) for increasing the light scattering effect is arranged on the light incident surface of the glass substrate (1).

3. The integrated light conversion glass diffuser plate according to claim 1, characterized in that: The thickness of the diffusion layer (2) is 30-80 μm; the thickness of the quantum dot light conversion layer (3) is 5-40 μm.

4. The integrated light conversion glass diffuser plate according to claim 1, characterized in that: The material of the adhesive layer (4) is optical glue.

5. The integrated light conversion glass diffuser plate according to claim 1, characterized in that: The resin is acrylic resin; the diffusion particles are titanium dioxide or silicon dioxide particles; the diluent is a mixture of divalent acid ester and isophorone; and the silane coupling agent is KH570.

6. The integrated light conversion glass diffuser plate according to claim 5, characterized in that: The particle size of the titanium dioxide or silicon dioxide particles is 5-10 microns; the volume ratio of the divalent ester to the isophorone is (1-2): (1-2).

7. A method for preparing an integrated light conversion glass diffuser plate according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: S1, adding resin, diffusion particles and silane coupling agent into a diluent and stirring evenly to obtain a light diffusion material; coating the light diffusion material on the light emitting surface of the glass substrate (1), and curing at 200-260° C. for 30-60 minutes to form the diffusion layer (2); S2, dispersing the quantum dots in silica gel ink to obtain quantum dot light conversion glue A; or dispersing the quantum dots in UV glue to obtain quantum dot light conversion glue B; S3, coating the quantum dot light conversion glue A on the diffusion layer (2), and curing it at 80-120° C. for 20-40 minutes to form the quantum dot light conversion layer (3); or coating the quantum dot light conversion glue B on the diffusion layer (2), and curing it at 100-200 W / cm 2 UV curing under UV irradiation for 15-45 seconds to form the quantum dot light conversion layer (3); S4, then coating optical glue on the quantum dot light conversion layer (3) to form the bonding layer (4); S5. Finally, the optical film (5) is attached to the adhesive layer (4).

8. The method for preparing an integrated light conversion glass diffuser plate according to claim 7, characterized in that: The light diffusion material in step S1 is coated on the light emitting surface of the glass substrate (1) by screen printing.

9. The method for preparing an integrated light conversion glass diffuser plate according to claim 7, characterized in that: The mass ratio of the quantum dots to the silicone ink or UV glue in step S2 is (5-40): (60-95); the quantum dots include red light quantum dots and green light quantum dots, and the mass ratio of the red light quantum dots to the green light quantum dots is 1:1; the wavelength of the red light quantum dots is 620-630nm, and the wavelength of the green light quantum dots is 520-530nm.