Metal strip and method for manufacturing the same, magnetic core and coil component

By forming a concave and convex continuous stripe texture on the surface of the metal strip, the problems of toughness and magnetic permeability in the miniaturized magnetic core are solved, and high toughness and magnetic permeability are improved.

CN112368791BActive Publication Date: 2024-10-22MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980044223.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-06-29
Filing Date
2019-06-03
Publication Date
2024-10-22
Estimated Expiration
2039-06-03

AI Technical Summary

Technical Problem

In the process of miniaturizing the magnetic core, it is difficult to ensure the toughness and mechanical strength of the metal strip with the existing technology, and structural defects such as breakage and cracks are prone to occur. At the same time, it is difficult to increase the magnetic permeability.

Method used

By treating the surface of the metal strip with a concave and convex continuous stripe texture, and winding one side as the outside, the stress is reduced, the air layer is eliminated, and the adhesion is improved.

Benefits of technology

It achieves a metal strip with high toughness and mechanical strength under the condition of small core diameter, suppresses the occurrence of structural defects, and improves the magnetic permeability and magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112368791B_ABST
    Figure CN112368791B_ABST
Patent Text Reader

Abstract

The main component of the metal strip (100) is formed of a metal magnetic material, and the surface roughness of one main surface (1) is formed to be coarser than the surface roughness of the other main surface (2). The other main surface (2) is formed into a smooth surface with high surface smoothness, and the surface of one main surface (1) is treated to continuously form a striped texture (5) having a concave portion (3) and a convex portion (4). After the continuous strip is made by a single-roll liquid quenching method, a main surface of the continuous strip is subjected to surface treatment to form the striped texture (5). The metal strip (100) is wound into a ring to obtain a magnetic core or a coil component such as a common mode choke using the metal strip. Thus, a metal strip that can ensure sufficient toughness and has good mechanical strength, a method for manufacturing the metal strip, a magnetic core whose core diameter can be reduced using the metal strip, and a coil component such as a common mode choke using the metal strip are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a metal strip and a method for manufacturing the same, a magnetic core and a coil component, and more particularly to a metal strip suitable for a winding core such as a common mode choke coil and a method for manufacturing the same, a magnetic core such as a winding core, and a coil component such as a common mode choke coil using the same. Background Art

[0002] Metal magnetic materials are widely used in coil parts used in power transformers, high-frequency transformers, magnetic shields, etc.

[0003] Among these metal magnetic materials, amorphous alloys are particularly excellent in soft magnetic properties and have been actively researched and developed.

[0004] For example, Patent Document 1 proposes a wound core in which a thin strip of an amorphous magnetic alloy having a positive magnetostrictive characteristic is wound with its smoother surface being located inside.

[0005] In patent document 1, a molten amorphous magnetic alloy material is ejected onto a high-speed rotating roller serving as a solid refrigerant to produce a continuous thin strip, thereby obtaining a magnetic alloy thin strip in which the surface roughness of the free surface not in contact with the high-speed rotating roller is rougher than the surface roughness of the contact surface in contact with the high-speed rotating roller.

[0006] In the patent document 1, the contact surface with the high-speed rotating roller is formed as a smooth surface with high surface smoothness corresponding to the surface accuracy of the high-speed rotating roller, and on the other hand, the surface on the side opposite to the contact surface is a free surface that does not contact the high-speed rotating roller, so the surface smoothness is poorer than the contact surface side, and the surface roughness is formed coarsely. Therefore, by winding the magnetic alloy thin strip into a ring shape with the contact surface side with high surface smoothness as the inner side and the free surface side with poor surface smoothness as the outer side, a winding core (magnetic core) is formed, so that the compressive stress loaded on the inner side of the winding core becomes smaller than the case where the free surface side is wound as the inner side, and as a result, the magnetic anisotropy accompanying the compressive stress becomes smaller, which can reduce the iron loss.

[0007] Then, by winding a conducting wire around the annular wound core obtained as described above, a coil component such as a common mode choke coil can be obtained.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Laid-Open No. 56-153709 (claim 1, page (2), upper left column, line 11 to page (2), upper right column, line 2, page (2), lower right column, line 10 to page (2), lower right column, line 16, etc.) Summary of the invention

[0011] However, in recent years, there has been a demand for module components mounted on various electronic devices to be smaller and lighter, and accordingly, there has been a demand for coil components such as common mode choke coils built into the module components to be smaller in size.

[0012] On the other hand, in such coil components, the metal strip (magnetic alloy strip) is wound to make a magnetic core (wound iron core), and the toughness and mechanical strength of the metal strip are important. That is, when the metal strip is wound into a ring, the outer diameter is larger than the inner diameter. Since the metal strip is stretched on the outside, stress is applied to the metal strip. As a result, structural defects such as breakage and cracks of the metal strip are easily generated. Therefore, as mentioned above, the toughness and mechanical strength of the metal strip are important. In particular, in order to achieve miniaturization of the coil component, it is necessary to reduce the core diameter (inner diameter of the magnetic core), so it becomes increasingly important to ensure toughness and mechanical strength.

[0013] However, in Patent Document 1, since one main surface of the metal strip is made into a free surface that does not contact the high-speed rotating roller, the surface smoothness of the above-mentioned main surface is poor. Therefore, when the core diameter is formed into a small diameter (for example, less than 6 mm), sufficient toughness cannot be ensured, the mechanical strength is reduced, and the wound metal strip may have structural defects such as breakage and cracks.

[0014] In addition, in order to ensure good magnetic properties, it is preferred to obtain a large inductance in such a coil component, so it is desirable to increase the magnetic permeability of the magnetic core. In this case, the occupancy rate of the metal thin strips is increased by winding the metal thin strips in close contact with each other, thereby increasing the magnetic permeability.

[0015] However, when winding is performed with only the free surface that is not in contact with the high-speed rotating roller facing outward as in Patent Document 1, an air layer is formed between the wound metal strips, so the metal strips cannot be wound in close contact with each other, and the magnetic permeability cannot be fully improved, making it difficult to obtain the desired magnetic properties.

[0016] The present invention is made in view of such circumstances, and aims to provide a metal strip and a method for manufacturing the same that can ensure sufficient toughness and have good mechanical strength, a magnetic core that can reduce the core diameter using the metal strip, and coil components such as a common mode choke using the magnetic core.

[0017] When a magnetic core is formed by winding a metal strip with one principal surface as a free surface and the other principal surface as a smooth surface with high surface smoothness so that the one principal surface becomes the outer side as in Patent Document 1, good mechanical strength and toughness can be obtained when the core diameter is large. However, as described in the item [Problems to be Solved by the Invention], if the core diameter becomes a small diameter such as less than 6 mm, it is difficult to ensure sufficient mechanical strength and toughness, and the metal strip is prone to structural defects such as breakage and cracks.

[0018] Therefore, the inventors conducted in-depth research and obtained the following insights: by further performing surface treatment on the above-mentioned free surface to form a continuous stripe-like texture with projections and depressions, when the metal strip is wound into a ring, the convex parts of the stripe-like texture are extended in the circumferential direction, thereby reducing the stress loaded on the metal strip and achieving high toughness. As a result, even if the core diameter of the magnetic core is a small diameter of less than 6 mm, the stress loaded on the entire metal strip can be reduced, and the occurrence of structural defects such as breakage and cracks can be suppressed.

[0019] In addition, it is also known that when winding, the air sandwiched between the metal strips will be released to the outside because the concave parts of the above-mentioned striped texture will become escape channels, so the air layer generated between the metal strips can be removed, thereby improving the closeness of the wound metal strips to each other and the magnetic permeability, which can improve the magnetic properties.

[0020] The present invention is based on such insights, and the metal strip involved in the present invention is characterized in that it is a film-like metal strip whose main component is formed by a metal magnetic material and is formed in a manner that the surface roughness of one main surface is rougher than the surface roughness of the other main surface, the above-mentioned other main surface is formed as a smooth surface with high surface smoothness, and the above-mentioned one main surface is surface-treated to continuously form a striped texture with concave portions and convex portions.

[0021] It should be noted that the above-mentioned "metal magnetic material" also includes alloys.

[0022] In the metal strip of the present invention, it is preferable that the striped texture is formed in a direction perpendicular or substantially perpendicular to the longitudinal direction of the one main surface.

[0023] In addition, as described above, the metal strip of the present invention forms a continuous striped texture with concave and convex portions on one main surface and makes the other main surface a smooth surface with high surface smoothness, so that the toughness is enhanced and the mechanical strength is ensured. Regarding the surface properties of the metal strip, it is preferably numerically managed in a manner such that the three-dimensional surface property parameters such as the arithmetic mean height, maximum height, and aspect ratio of the three-dimensional surface roughness are within the following ranges.

[0024] That is, the metal strip of the present invention preferably has a surface roughness of the one main surface that is 5 times or more, preferably 10 times or more, the arithmetic mean height of the surface roughness of the other main surface converted into a three-dimensional surface texture parameter.

[0025] In addition, the maximum height of the surface roughness of the one main surface of the metal strip of the present invention, when converted into a three-dimensional surface texture parameter, is preferably at least twice as large as the maximum height of the surface roughness of the other main surface.

[0026] In addition, the surface roughness of the one main surface of the metal strip of the present invention is preferably 0.9 times or less when converted into an aspect ratio of a three-dimensional surface texture parameter.

[0027] Furthermore, in the metal strip of the present invention, the maximum width of the projections is preferably 5 to 60 μm.

[0028] Furthermore, in the metal strip of the present invention, the maximum length of the projections is preferably 10 to 600 μm.

[0029] Furthermore, the metal magnetic material of the metal strip of the present invention is preferably amorphous.

[0030] Furthermore, the metal magnetic material of the metal strip of the present invention preferably contains Fe as a main component.

[0031] In addition, the method for manufacturing a metal strip involved in the present invention is characterized in that it includes the following steps: a step of spraying a metal melt mainly composed of a metal magnetic material onto a rotating body to rapidly cool and solidify it so that one main surface is not in contact with the above-mentioned rotating body and the other main surface is in contact with the above-mentioned rotating body to produce a continuous thin strip; and a step of conveying the above-mentioned continuous thin strip in a specified direction while performing surface treatment on the above-mentioned one main surface to continuously form a striped texture with concave portions and convex portions on the above-mentioned one main surface so that the surface roughness of the above-mentioned one main surface is rougher than the surface roughness of the other main surface to produce a metal strip.

[0032] In the method for manufacturing a metal strip of the present invention, it is preferred that a surface treatment tool is intermittently loaded on one main surface of the continuous strip while heat treating the continuous strip, and the shape of the tip of the surface treatment tool is transferred to the one main surface.

[0033] Since the continuous thin strip is heat treated in this way, the internal strain formed by rapid cooling and solidification can be removed, and the front end shape of the above-mentioned surface treatment tool is transferred to a main surface that does not contact the rotating body when the continuous thin strip is produced, thereby making it easy to produce a metal strip with a striped texture with concave and convex portions formed on one main surface.

[0034] Furthermore, the magnetic core according to the present invention is a magnetic core obtained by winding any one of the metal thin strips described above into a ring shape, wherein the metal thin strip is wound with the one main surface as an outer side.

[0035] In addition, the core diameter of the magnetic core of the present invention is preferably 6 mm or less.

[0036] Therefore, even if the core diameter is as small as 6 mm or less, the metal strip will not have structural defects such as breakage and cracks, and a magnetic core with excellent mechanical strength and toughness can be obtained.

[0037] In addition, in the present invention, "core diameter" refers to the inner diameter of the magnetic core.

[0038] Furthermore, a coil component according to the present invention includes the above-mentioned magnetic core and a coil conductor.

[0039] Furthermore, the coil component of the present invention is preferably a common mode choke coil.

[0040] It should be noted that in the present invention, the thin strip before the stripe-like texture is formed is simply referred to as a thin strip or a continuous thin strip, and the thin strip having the stripe-like texture formed thereon by surface treatment is referred to as a metal thin strip.

[0041] According to the metal strip of the present invention, since the main component is formed by a metal magnetic material, and the surface roughness of one main surface is rougher than that of the other main surface, the other main surface is formed as a smooth surface with high surface smoothness, and the surface of the one main surface is treated in a manner of continuously forming a stripe-like texture with concave and convex parts, even if the metal strip is wound into a ring, the convex part will extend in the circumferential direction, so the stress loaded on the metal strip can be reduced, and the toughness can be high. That is, even if the core diameter (hollow core) is small, the stress loaded on the metal strip can be reduced, so the toughness is enhanced, the occurrence of structural defects such as breakage and cracks can be suppressed, and a metal strip with good mechanical strength can be obtained. In addition, when winding, the air sandwiched between the metal strips will be released to the outside because the concave part of the stripe-like texture will become an escape channel, so the air layer generated between the metal strips can be removed, thereby improving the closeness of the wound metal strips and improving the magnetic permeability. Therefore, even if the core diameter is small, a large inductance can be obtained, and the magnetic characteristics can be improved.

[0042] In addition, the method for manufacturing a metal strip according to the present invention includes the following steps: a step of spraying a metal melt mainly composed of a metal magnetic material onto a rotating body to rapidly cool and solidify it so that one main surface is not in contact with the rotating body and the other main surface is in contact with the rotating body to produce a continuous thin strip, and a step of surface-treating the one main surface while conveying the continuous thin strip in a prescribed direction to continuously form a striped texture having concave portions and convex portions on the one main surface so that the surface roughness of the one main surface is rougher than that of the other main surface to produce the metal strip; therefore, only the one main surface that is not in contact with the rotating body is surface-treated when producing the continuous thin strip, thereby making it easy to produce a metal strip having a striped texture having concave portions and convex portions formed on one main surface.

[0043] According to the magnetic core of the present invention, since the metal thin strip described in any one of the above items is wound into a ring shape, and the metal thin strip is wound so that the one main surface becomes the outer side, the convex portion extends in the lateral direction when the metal thin strip is wound, and the toughness is strengthened, and the stress loaded on the metal thin strip can be effectively reduced. That is, even if the hollow core is small, the toughness of the metal thin strip can be strengthened, so that the mechanical strength can be improved, and the magnetic core that can suppress the occurrence of structural defects such as breakage and cracks can be obtained.

[0044] Furthermore, according to the coil component of the present invention, since it includes the magnetic core and the coil conductor, it is possible to obtain a small coil component such as a common mode choke coil that has good toughness and can ensure mechanical strength, thereby contributing to the miniaturization and weight reduction of module components. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a plan view schematically showing a main part of one embodiment of the metal strip according to the present invention.

[0046] Figure 2 It is a cross-sectional view of the main parts of the above-mentioned metal strip.

[0047] Figure 3 This is a diagram (1 / 2) for explaining one embodiment of the method for producing a metal strip according to the present invention.

[0048] Figure 4 This is a diagram (2 / 2) for explaining one embodiment of the method for producing a metal strip according to the present invention.

[0049] Figure 5 This is a perspective view schematically showing one embodiment of a magnetic core according to the present invention.

[0050] Figure 6 It is a cross-sectional view of the main parts of the above-mentioned magnetic core.

[0051] Figure 7 It is a manufacturing process diagram showing one embodiment of the manufacturing method of the magnetic core according to the present invention.

[0052] Figure 8 It is a front view of a common mode choke coil which is a coil component according to the present invention. DETAILED DESCRIPTION

[0053] Next, embodiments of the present invention will be described in detail.

[0054] Figure 1 is a top view schematically showing an embodiment of the metal strip involved in the present invention, Figure 2 yes Figure 1 Cross-sectional view along the direction of arrow A-A.

[0055] The main component of the metal strip 100 is formed of a metal magnetic material, and is formed in such a manner that the surface roughness of one main surface 1 is rougher than the surface roughness of the other main surface 2. Specifically, the other main surface 2 is formed as a smooth surface with high surface smoothness, and the surface of one main surface 1 is treated in such a manner that a stripe-like texture 5 having concave portions 3 and convex portions 4 is continuously formed.

[0056] By forming the metal strip 100 as described above and winding it into a ring shape with one main surface 1 located outside, the convex portion 4 is elongated in the circumferential direction and the toughness is enhanced. This can reduce the stress applied to the metal strip 100 and suppress the occurrence of structural defects such as breakage and cracks even when the core diameter is small.

[0057] That is, if a thin strip having smooth surfaces with high surface smoothness on both main surfaces is wound into a ring shape, the outer diameter is larger than the inner diameter, the outer side is elongated compared with the inner side, and stress is applied to the thin strip. Thus, the stress may cause structural defects such as breakage and cracks to occur in the thin strip.

[0058] In this case, when the core diameter is large (for example, more than 10 mm), as in Patent Document 1, one main surface of the thin strip is made a free surface with a rough surface roughness, and the other main surface is made a smooth surface with a high surface smoothness, and the magnetic core is formed by winding with one main surface 1 located on the outside, thereby ensuring good toughness and mechanical strength.

[0059] However, if the core diameter is as small as 6 mm or less, for example, simply winding the thin strip into a ring shape with the free surface facing outward will easily cause stress load caused by elongation of the outer side of the wound thin strip, resulting in structural defects such as breakage and cracks.

[0060] Therefore, in the present invention, the free surface is further subjected to surface treatment in a manner of forming a continuous concavo-convex stripe-shaped texture 5, and a metal strip 100 is produced. When the metal strip 100 is wound into a ring shape in a manner of positioning the stripe-shaped texture 5 on the outside, the convex portion 4 extends in the circumferential direction. That is, when the metal strip 100 is wound into a ring shape, the toughness can be enhanced by stretching the convex portion 4 in the circumferential direction. Even when the core diameter of the magnetic core is small, the stress loaded on the metal strip 100 can be reduced, thereby suppressing the occurrence of structural defects such as breakage and cracks, and obtaining a metal strip 100 with high toughness and good mechanical strength.

[0061] Furthermore, the air sandwiched between the metal strips 100 and the metal strips 100 during winding can be released to the outside because the concave portion 3 of the stripe-shaped texture 5 becomes an escape channel, so the air layer generated between the metal strips 100 can be removed, thereby improving the closeness of the wound metal strips 100 and improving the magnetic permeability. Therefore, even if the core diameter is small, a large inductance can be obtained, and the magnetic properties can be improved.

[0062] The maximum length L and the maximum width W of the convex portion 4 forming the stripe-like texture 5 are not particularly limited as long as they can ensure that the elongation of structural defects such as breakage and cracks can be suppressed when the metal thin strip 100 is wound. The maximum width W is preferably 5 to 60 μm, and more preferably 10 to 50 μm. In addition, the maximum length L is preferably 10 to 600 μm, and more preferably 30 to 600 μm. Therefore, it is preferred to use a surface treatment tool described later to perform surface treatment in such a manner as to achieve such a maximum width W and maximum length L.

[0063] In addition, the formation direction of the stripe-shaped texture 5 is not particularly limited and can be parallel to the long side direction, but is usually as follows: Figure 1 As shown, the long side direction of the metal strip 100 is preferably a vertical direction or a substantially vertical direction.

[0064] There is no particular limitation on the metal magnetic material that forms the main component of the metal strip 100 as long as it is a metal magnetic material, and Fe-based materials with Fe as the main component, such as Fe-Si-B-Cu-Nb, Fe-Si-B-P-Cu, Fe-P-B-C-Si-Ge-Al, Fe-Ni-P-B-C-Si-Ge-Al, Fe-Ni-Co-P-B-C-Si-Ge-Al, Fe-Si, Fe-Si-Cr, and Fe-Si-Al, can be used.

[0065] The thickness of the metal strip 100 is not particularly limited either, but is generally 15 to 80 μm, preferably 20 to 30 μm.

[0066] The metal magnetic material may be crystalline, but is more preferably amorphous due to its excellent soft magnetic properties.

[0067] The outer dimensions of the metal strip 100 are appropriately determined according to the required texture, and are formed to have a total length of about 1500 mm and a total width of about 50 mm, for example.

[0068] However, the present metal strip 100 forms a continuous striped texture 5 having concave portions 3 and convex portions 4 on one main surface 1, and makes the other main surface 2 a smooth surface with high surface smoothness, thereby enhancing toughness and ensuring mechanical strength. However, in order to obtain the desired mechanical strength and toughness, it is preferred to numerically manage three-dimensional surface property parameters such as the arithmetic mean height Sa of the three-dimensional surface roughness, the maximum height Sz, and the aspect ratio (hereinafter referred to as "aspect ratio") Str of the surface property.

[0069] In the past, this type of surface roughness was generally numerically managed as two-dimensional linear roughness, but in recent years, two-dimensional parameters have been expanded to numerically manage surface roughness as three-dimensional parameters, and the details are specified in ISO25178 of the International Organization for Standardization (ISO). The three-dimensional surface property parameters can evaluate the surface property three-dimensionally, so the deviation of the measurement results caused by the dependence on the measurement position and scanning direction like the two-dimensional surface property parameters can be eliminated. In addition, the surface anisotropy that cannot be numerically expressed in the two-dimensional surface property parameters can be numerically managed.

[0070] In addition to the above-mentioned arithmetic mean height Sa, maximum height Sz, and aspect ratio Str, the three-dimensional surface property parameters also include the arithmetic mean curvature of the peak apex (hereinafter referred to as "arithmetic mean curvature") Spc, the developed area ratio of the interface (hereinafter referred to as "developed area ratio") Sdr, etc., and the preferred ranges of each are described in detail.

[0071] (1) Arithmetic mean height Sa

[0072] The arithmetic mean height Sa is the arithmetic mean of the absolute value of the height from the reference surface in the measurement target area. Therefore, when the arithmetic mean height Sa is large, it means that the surface smoothness is low and the surface roughness is rough, and when the arithmetic mean height Sa is small, it means that the surface smoothness is high. In addition, in order to form the desired striped texture 5, the surface roughness of one main surface 1 is preferably converted into an arithmetic mean height Sa of 0.2 μm or more, more preferably 0.3 μm or more, and the ratio of the arithmetic mean height Sa converted to the surface roughness of the other main surface 2 is preferably 5 times or more, more preferably 10 times or more.

[0073] (2) Maximum height Sz

[0074] The maximum height Sz is the sum of the maximum peak height Sp and the maximum valley depth Sv in the measurement target area (=Sp+Sv). The maximum height Sz indicates low surface smoothness and rough surface roughness, and the small maximum height Sz indicates high surface smoothness. In addition, in order to form the desired striped texture 5, the surface roughness of one main surface 1 is preferably 2 μm or more, more preferably 2.5 μm or more, and the ratio of the maximum height Sz relative to the surface roughness of the other main surface 2 is preferably 2 times or more, more preferably 5 times or more.

[0075] (3) Aspect ratio Str

[0076] The aspect ratio Str is defined as the ratio of the horizontal distance at which the autocorrelation function, which is an evaluation index of periodicity, decays to a specific value the slowest to the horizontal distance at which the above autocorrelation function decays to a specific value the fastest, and a value of 0≤Str<1 is adopted. The aspect ratio Str is a standard for representing the uniformity of surface properties. The closer the aspect ratio is to 1, the better the uniformity of the isotropic surface becomes. As it approaches 0, the non-uniformity increases and the surface becomes an anisotropic surface. Moreover, in the present embodiment, since the striped texture 5 is formed on the first main surface 1, a non-uniform anisotropic surface is preferred. From this point of view, the surface roughness of one main surface 1 converted into an aspect ratio Str is preferably less than 0.33, more preferably less than 0.30, and the ratio of the aspect ratio Str converted to the surface roughness of the other main surface 2 is preferably less than 0.9 times, more preferably less than 0.85 times.

[0077] (4) Arithmetic mean curvature Spc

[0078] The arithmetic mean curvature Spc is the average of the main curvatures of the peak apex of the surface. When the arithmetic mean curvature Spc is small, it means that the convex portion 4 is rounded, and on the other hand, when the arithmetic mean curvature Spc is large, it means that the convex portion 4 is sharp. Moreover, since the arithmetic mean curvature Spc of one main surface 1 preferably has a sharp convex portion 4, the surface roughness of one main surface 1 converted into the arithmetic mean curvature Spc is preferably 400 (1 / mm) or more, more preferably 600 (1 / mm) or more, and the ratio of the arithmetic mean curvature Spc converted to the surface roughness of the other main surface 2 is preferably 2 times or more, more preferably 3 times or more.

[0079] (5) Development area ratio Sdr

[0080] The developed area ratio Sdr indicates how much the developed area (surface area) of the measurement target area increases relative to the area of ​​the measurement target area. In a completely flat surface, the developed area ratio Sdr is 0. If the surface is inclined, the developed area ratio Sdr becomes larger. The surface roughness of the first main surface 1 on which the stripe-shaped texture 5 is to be formed is preferably 0.010 or more, more preferably 0.015, and the ratio of the developed area ratio Sdr relative to the surface roughness of the second main surface 2 is preferably 20 times or more, more preferably 30 times or more.

[0081] In the present embodiment, it is preferred that the surface roughness be numerically managed so as to satisfy at least one of the numerical ranges described in (1) to (5), particularly at least one of the numerical ranges described in (1) to (3).

[0082] Thus, since the main component of the metal strip 100 is formed of a metal magnetic material, and the surface roughness of one main surface 1 is formed in a manner that is rougher than the surface roughness of the other main surface 2, the other main surface 2 is formed as a smooth surface with high surface smoothness, and the surface of one main surface 1 is treated in a manner that a stripe-shaped texture 5 having a concave portion 3 and a convex portion 4 is continuously formed, even if the metal strip 100 is wound into a ring shape, the convex portion 4 will extend in the circumferential direction, so that the stress loaded on the metal strip 100 can be reduced, and the toughness can be high. That is, even if the core diameter is small, the stress loaded on the metal strip 100 can be reduced, so the toughness is enhanced, the occurrence of structural defects such as breakage and cracks can be suppressed, and a metal strip with good mechanical strength can be obtained. Furthermore, the air sandwiched between the metal strips 100 and the metal strips 100 during winding can be released to the outside because the concave portion 3 of the stripe-shaped texture 5 becomes an escape channel, so the air layer generated between the metal strips 100 can be removed, thereby improving the closeness of the wound metal strips 100 and improving the magnetic permeability. Therefore, even if the core diameter is small, a large inductance can be obtained, and the magnetic properties can be improved.

[0083] Next, the method for producing the above-mentioned metal strip will be described in detail.

[0084] The method for manufacturing a metal thin strip includes a continuous thin strip manufacturing step of continuously manufacturing a thin strip from a metal melt and a striped texture imparting step of surface treating one main surface of the continuous thin strip to impart a striped texture, wherein the continuous thin strip manufacturing step and the striped texture imparting step are continuously implemented.

[0085] Figure 3 FIG. 1 is a diagram schematically showing one embodiment of a continuous ribbon production process. In this embodiment, a continuous ribbon is produced by a single-roll liquid quenching method.

[0086] That is, the continuous thin strip production process comprises: a crucible 7 formed of alumina or the like for accommodating a metal melt 6, an induction heating coil 8 arranged on the outer periphery of the crucible 7, a roller (rotating body) 9 formed of Cu or the like that rotates at a high speed in the direction of arrow A, and a first winding section 11 that rotates in the direction of arrow B and winds up the continuous thin strip 10.

[0087] Then, the continuous thin strip 10 can be manufactured as follows.

[0088] First, prepare the raw materials such as Fe, Si, B, P, etc., the monomers of the elements that form the Fe-based metal magnetic material or the compounds containing these elements, weigh the specified amounts and blend them, heat them to above the melting point using a high-frequency induction heating furnace, etc., and then cool them to obtain a mother alloy.

[0089] Next, the mother alloy is pulverized and placed in a crucible 7. Then, a high-frequency power source is applied to the induction heating coil 8 to heat the crucible 7 to melt the mother alloy, thereby producing a molten metal 6.

[0090] Next, the molten metal 6 is ejected from the nozzle 7a of the crucible 7 and falls onto the roller 9 rotating at a high speed in the direction of arrow A. The molten metal 6 is thus rapidly solidified by the roller 9 to form an amorphous continuous thin strip 10, which is then wound by the first winding unit 11 rotating in the direction of arrow B.

[0091] In the continuous thin strip 10 formed in this way, the other main surface 13 in contact with the roller 9 is limited by the surface accuracy of the roller 9 and becomes a smooth surface with high surface smoothness, and one main surface 12 becomes a free surface that does not contact the roller 9, and has a lower surface smoothness than the other main surface 13, and is formed in a manner having an appropriate surface roughness.

[0092] Figure 4 This is a diagram schematically showing one embodiment of the stripe-shaped texture imparting step.

[0093] That is, the striped texture imparting process includes: a heating furnace 14 for heat treating the continuous thin strip 10 wound by the first winding section 11, a surface treatment tool 15 installed at the front end portion of the heating furnace 14, a second winding section 16 for winding the metal thin strip 100 surface-treated by the surface treatment tool 15, a first guide roller 17 for guiding the continuous thin strip 10 to the heating furnace 14, and a second guide roller 18 for guiding the metal thin strip 100 transported from the heating furnace 14 to the second winding section 16.

[0094] The surface treatment tool 15 reciprocates in a vertical direction relative to the continuous thin strip 10 conveyed in the direction of arrow C, and is intermittently loaded on the first main surface 12 to perform surface treatment, and a striped texture 5 having concave portions 3 and convex portions 4 is continuously formed on the first main surface 1 after surface treatment. That is, the front end of the surface treatment tool 15 is configured in such a way that the striped texture 5 is formed on the first main surface 1 of the metal thin strip 100 after surface treatment by shape transfer.

[0095] That is, in the above-mentioned stripe-like texture imparting step, the continuous thin strip 10 wound by the first winding part 11 is guided to the heating furnace 14 via the first guide roller 17, and is conveyed in the direction of the arrow C. The continuous thin strip 10 is subjected to heat treatment in the heating furnace 14 to remove the thermal strain of the continuous thin strip 10, and the continuous thin strip 10 is crystallized as needed, and the continuous thin strip 10 is subjected to surface treatment via the surface treatment tool 15. Specifically, the surface treatment tool 15 is reciprocated in a direction perpendicular to the conveying direction of the continuous thin strip 10, so that the shape of the tip of the surface treatment tool 15 is transferred to the first main surface 12 of the continuous thin strip 10, thereby obtaining the metal thin strip 100 having the stripe-like texture 5 formed on the first main surface 1 after the surface treatment, and the above-mentioned metal thin strip 100 is wound on the second winding part 16 via the second guide roller 18.

[0096] Thus, according to the manufacturing method of the present metal thin strip, the following steps are included: a step of spraying a metal melt 6 mainly composed of a metal magnetic material onto a roller 9 rotating in the direction of arrow A to rapidly cool and solidify it, so that one main surface 12 is not in contact with the roller 9 and the other main surface 13 is in contact with the roller 9 to produce a continuous thin strip 10; a step of performing surface treatment on one main surface 12 while conveying the continuous thin strip 10 in the direction of arrow C, and continuously forming a striped texture 5 having concave portions 3 and convex portions 4 on one main surface 1 in a manner that the surface roughness of the one main surface 1 after the surface treatment is rougher than the surface roughness of the other main surface 2, thereby producing a metal thin strip; therefore, only the one main surface 12 that is not in contact with the roller 9 during the production of the continuous thin strip is surface treated, thereby forming a striped texture 5 having concave portions 3 and convex portions 4 on the one main surface 1 after the surface treatment, and the desired metal thin strip 100 can be easily produced.

[0097] Furthermore, since the continuous ribbon 10 is subjected to heat treatment, internal strain formed by rapid cooling and solidification can be effectively removed.

[0098] Figure 5 This is a perspective view schematically showing one embodiment of a magnetic core obtained by using the above-mentioned metal thin strip.

[0099] This magnetic core is as Figure 5 As shown, the metal strip 100 is wound into a ring shape with the first main surface 1 located on the outside and the other main surface 2 located on the inside. The first main surface 1 is formed with a striped texture 5 in a roughened surface, and the other main surface 2 is a smooth surface with high surface smoothness.

[0100] Figure 6 It is a cross-sectional view schematically showing an example of the outer peripheral surface of the magnetic core.

[0101] Figure 6In the figure, the metal strip 100 has a striped texture 5 having a concave portion 3 and a convex portion 4 before winding as shown by the dotted line, and the convex portion 4' is extended in the circumferential direction by winding, and as a result, the stress loaded on the metal strip 100 can be suppressed. That is, by continuously forming the striped texture 5 having the concave portion 3 and the convex portion 4, the stress loaded on the metal strip 100 can be reduced, so even if the metal strip 100 is wound into a ring shape to form a magnetic core with a small core diameter, a magnetic core with high toughness and good mechanical strength can be obtained, and structural defects such as cracks in the metal strip 100 can be suppressed.

[0102] In addition, when winding, the air sandwiched between the metal strips 100 and the metal strips 100 is released to the outside because the concave portion 3 of the above-mentioned striped texture 5 serves as an escape channel, so the air layer generated between the metal strips can be removed, thereby improving the closeness between the metal strips and the magnetic permeability. As a result, a large inductance can be obtained and the magnetic properties can be improved.

[0103] Figure 7 is a diagram schematically showing an embodiment of a method for manufacturing a magnetic core. In this embodiment, as Figure 3 and Figure 4 The process after the metal strip manufacturing process shown in is carried out.

[0104] That is, in the present manufacturing method, first, a core rod 21 having a small diameter portion 20 with a diameter of 6 mm or less and a large diameter portion 19 larger than the small diameter portion 20 is prepared. Then, while the core rod 21 is rotated in the direction of arrow E, the metal strip 100 wound on the second winding portion 15 is guided to the outer peripheral surface of the core rod 21, and the metal strip 100 is wound multiple times in a manner that is closely attached to the outer peripheral surface of the core rod 21, and the metal strip 100 is wound around the small diameter portion 20 of the core rod 21. And then, the core rod 21 is separated from the metal strip 100, thereby making it possible to manufacture a magnetic core.

[0105] Figure 8 This is a front view showing an embodiment of a coil component using the above-mentioned magnetic core, and this coil component is a common mode choke coil.

[0106] That is, the common mode choke coil is configured such that the first and second coil conductors 23a and 23b are wound around the annular core 22 in opposite directions to each other, and a common mode current flows through the first coil conductor 23a and a normal mode current flows through the second coil conductor 23b.

[0107] In the common mode choke coil configured in this way, the noise component is transmitted in the common mode and the signal component is transmitted in the normal mode. Therefore, the difference between these transmission modes can be utilized to separate the signal and the noise, thereby performing noise removal.

[0108] Moreover, the magnetic core 22 of the common mode choke is formed by the above-mentioned metal strip 100 of the present invention, so even when the core diameter is a small diameter of less than 6 mm, the occurrence of structural defects such as cracks can be suppressed, and a small common mode choke with high toughness and good mechanical strength can be obtained, which helps to miniaturize and lighten the module components.

[0109] For example, in the above embodiment, a common mode choke coil is exemplified as a coil component, but the present invention is applicable to various coil components using a metal magnetic material that require a small core diameter.

[0110] Next, embodiments of the present invention will be described in detail.

[0111] Example 1

[0112] 〔Sample Preparation〕

[0113] Fe, Si, B, and Fe3P are prepared as raw materials, blended in a manner to achieve a specified composition, heated to a temperature above the melting point in a high-frequency induction heating furnace to melt, and then the melt is flowed into a copper casting mold and cooled to produce a master alloy.

[0114] Next, the mother alloy is crushed to a size of about 5 mm, and is placed in a crucible of a single-roll liquid quenching device, where high-frequency induction heating is performed to melt the mother alloy to obtain a molten metal.

[0115] Next, the molten metal is ejected from a nozzle at the front end of the crucible and poured onto a roller rotating at a high speed to be rapidly condensed and solidified, thereby manufacturing a continuous ribbon in which the ribbon is continuously formed.

[0116] Next, the continuous thin strip is passed through a heating furnace adjusted to 400°C and equipped with a surface treatment tool near the outlet, and the continuous thin strip is heat treated to remove thermal strain, and the surface treatment tool is moved back and forth in a vertical direction relative to the first main surface of the continuous thin strip, so that the surface treatment tool is intermittently loaded on the continuous thin strip. Thus, the front end shape of the surface treatment tool is transferred to the above-mentioned first main surface, and a sample (metal thin strip) with a striped texture having concave and convex parts is continuously formed. The outer dimensions of the sample are 100m in length, 50mm in width, and 25μm in thickness.

[0117] [Evaluation of samples]

[0118] The first and second main surfaces of the prepared sample were subjected to three-dimensional image analysis using a laser microscope (Keyence, shape analysis laser microscope VK-X series), and various surface roughnesses (arithmetic mean roughness Sa, maximum height Sz, aspect ratio Str, arithmetic mean curvature Spc, and development area ratio Sdr) were calculated based on ISO25178. It should be noted that the target area for image analysis is 280 μm in length and 200 μm in width.

[0119] Table 1 shows the measurement results of the surface roughness of each of the first main surface and the second main surface, and the ratio of the first main surface to the second main surface.

[0120]

[0121] (1) Arithmetic mean height Sa

[0122] The arithmetic mean height Sa of the second main surface without surface treatment is as low as 0.024 μm, and the surface smoothness is high. In contrast, the arithmetic mean height Sa of the first main surface after surface treatment is 0.31 μm because of the formation of stripe-like texture. That is, when the arithmetic mean height Sa of the three-dimensional surface property parameter is used for evaluation, the surface roughness of one main surface is 12.9 times the average roughness of the other main surface, which is more than 10 times. It can be seen that the desired concave-convex stripe-like texture is continuously formed on the first main surface.

[0123] (2) Maximum height Sz

[0124] The maximum height Sz of the second main surface that has not been surface treated is 0.46μm, and the height difference is small. In contrast, the maximum height Sz of the first main surface that has been surface treated is 2.5μm, and the height difference is large. The ratio is 5.4 times, which is more than 5 times. Even when the maximum height Sz is used to evaluate the surface roughness, the first main surface is much rougher than the second main surface. It can be seen that the desired concave and convex striped texture is continuously formed on the first main surface.

[0125] (3) Aspect ratio Str

[0126] The aspect ratio Str of the second main surface that has not been surface treated is 0.35, while the aspect ratio Str of the first main surface that has been surface treated is 0.31, which is 0.9 times. That is, since the aspect ratio Str of the first main surface is smaller than that of the second main surface, the surface anisotropy is stronger than that of the second main surface, and the surface is uneven, and it can be seen that the desired concavo-convex stripe texture is continuously formed on the first main surface.

[0127] (4) Arithmetic mean curvature Spc

[0128] The second main surface without surface treatment is 236 (1 / mm), while the first main surface with surface treatment is 765 (1 / mm), which is 3.2 times. That is, it can be seen that the surface shape of the first main surface is much sharper than that of the second main surface.

[0129] (5) Development area ratio Sdr

[0130] The second main surface without surface treatment is 0.0008, which is close to a completely smooth surface, while the first main surface with surface treatment is 0.02, which is 25 times. In other words, it can be seen that the surface of the first main surface is much rougher than that of the second main surface.

[0131] Example 2

[0132] Using the metal thin strip of Example 1, 10 magnetic cores were produced in such a manner that the core diameters became 4 mm, 6 mm, and 12 mm, and these cores were used as samples of the present invention.

[0133] In addition, using the continuous thin strip that was not subjected to surface treatment in Example 1, 10 magnetic cores each were produced so that the core diameters would be 4 mm, 6 mm, and 12 mm, as comparative example samples.

[0134] Then, each of the samples of the present invention and the comparative example samples was observed visually and with an optical microscope to analyze whether structural defects such as breakage and cracks occurred.

[0135] Table 2 shows the defective generation rates of the samples of the present invention and the samples of the comparative examples.

[0136] [Table 2]

[0137]

[0138] As can be seen from Table 2, when the core diameter was 12 mm, no defective products such as structural defects such as breakage and cracks occurred in either the present invention or the comparative example.

[0139] However, it is found that when the core diameter is changed to 6 mm, no defective products are generated in the samples of the present invention, whereas 5 defective products are generated among 10 samples of the comparative example, resulting in a decrease in the product yield.

[0140] Furthermore, when the core diameter was changed to 4 mm, no structural defects were observed in the samples of the present invention, whereas structural defects occurred in all 10 samples of the comparative example.

[0141] In summary, it can be seen that the sample of the present invention is different from the sample of the comparative example. Even if the core diameter is small, a magnetic core with good mechanical strength including toughness can be obtained.

[0142] Industrial Applicability

[0143] A metal thin strip having excellent mechanical strength and toughness and a method for producing the same can be achieved, in which structural defects such as cracks can be suppressed even when the core diameter is as small as 6 mm or less.

[0144] Explanation of symbols

[0145] 1. One main surface

[0146] 2 The other side

[0147] 3 concavity

[0148] 4 convex part

[0149] 5 Striped Texture

[0150] 6 Molten Metal

[0151] 9 Roller (rotating body)

[0152] 10 Continuous thin strip

[0153] 12 A main surface

[0154] 13 Another main face

[0155] 15 Surface treatment tools

[0156] 22 Magnetic core

[0157] 23a, 23b Coil conductor

[0158] 100 Metal Strip

Claims

1. A metal strip, characterized in that: The main component is a metal magnetic material, and the surface roughness of one main surface is rougher than that of the other main surface. The other main surface is formed as a smooth surface with high surface smoothness, Furthermore, the one main surface is subjected to surface treatment so that a striped texture having concave portions and convex portions is continuously formed, The surface roughness of the one main surface is 5 times or more the arithmetic mean height of the surface roughness of the other main surface converted into a three-dimensional surface texture parameter.

2. The metal strip according to claim 1, characterized in that: The striped texture is formed in a perpendicular direction or a substantially perpendicular direction to the long side direction of the one main surface.

3. The metal strip according to claim 1, characterized in that: The surface roughness of the one main surface is 10 times or more the surface roughness of the other main surface in terms of the arithmetic mean height.

4. The metal strip according to claim 1 or 2, characterized in that: The maximum height of the surface roughness of the one main surface converted into a three-dimensional surface texture parameter is at least twice the surface roughness of the other main surface.

5. The metal strip according to claim 1 or 2, characterized in that: The aspect ratio of the surface roughness of the one main surface converted into a three-dimensional surface texture parameter is 0.9 times or less relative to the surface roughness of the other main surface.

6. The metal strip according to claim 1 or 2, characterized in that: The maximum width of the convex portion is 5 to 60 μm.

7. The metal strip according to claim 1 or 2, characterized in that: The maximum length of the protrusion is 10 to 600 μm.

8. The metal strip according to claim 1 or 2, characterized in that: The metal magnetic material is amorphous.

9. The metal strip according to claim 1 or 2, characterized in that: The metal magnetic material contains Fe as a main component.

10. A method for manufacturing a metal thin strip, characterized in that: The process includes the following steps: The process of producing a continuous thin strip by ejecting a metal melt mainly composed of a metal magnetic material onto a rotating body and rapidly solidifying the metal melt so that one main surface is not in contact with the rotating body and the other main surface is in contact with the rotating body, and A step of performing surface treatment on the one main surface while conveying the continuous thin strip in a predetermined direction, continuously forming a stripe-like texture having concave portions and convex portions on the one main surface so that the surface roughness of the one main surface is rougher than that of the other main surface, thereby manufacturing the metal thin strip; The surface treatment is performed by intermittently placing a surface treatment tool on one main surface of the continuous thin strip while the continuous thin strip is subjected to heat treatment, and the shape of the tip of the surface treatment tool is transferred to the one main surface.

11. A magnetic core, characterized in that: A magnetic core obtained by winding the metal thin strip according to any one of claims 1 to 9 into a ring shape, The metal strip is wound with a main surface having a striped texture as the outer side.

12. The magnetic core according to claim 11, characterized in that The core diameter is less than 6 mm.

13. A coil component, characterized in that: A magnetic core according to claim 11 or 12 and a coil conductor.

14. The coil component according to claim 13, characterized in that It is a common mode choke.