Semiconductor device and method for forming the same

By forming discretely arranged fins on the semiconductor device substrate and performing ion implantation, the problem of β ratio adjustment in static random access memory is solved, and the writing redundancy and overall performance are improved.

CN112447729BActive Publication Date: 2024-10-29SEMICON MFG INT (SHANGHAI) CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201910832713.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-09-04
Publication Date
2024-10-29
Estimated Expiration
2039-09-04

AI Technical Summary

Technical Problem

Existing technology makes it difficult to adjust the beta ratio in static random access memory (SRAM), resulting in poor write redundancy and limiting the performance of semiconductor devices.

Method used

Discretely arranged fins are formed on the substrate of the semiconductor device, and specific fin surfaces are exposed through a mask layer, and N-type or P-type ion implantation is performed to adjust the threshold voltage and thereby adjust the β ratio.

Benefits of technology

The formation process of the mask layer is simplified, the β ratio is flexibly adjusted, the writing redundancy of the static random access memory is improved, and the overall performance of the semiconductor device is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112447729B_ABST
    Figure CN112447729B_ABST
Patent Text Reader

Abstract

The present invention provides a semiconductor device and a method for forming the same, the method comprising: providing a substrate, the substrate comprising a pull-up transistor region, a pull-down transistor region and a transmission transistor region; forming a plurality of discretely arranged fins on the substrate, the fins comprising a first fin located at both the transmission transistor region and the pull-down transistor region, a second fin located at the pull-down transistor region and a third fin located at the pull-up transistor region; forming a mask layer on the substrate, the mask layer simultaneously exposing the surface of the second fin and the surface of the third fin, or the mask layer exposing the surface of the first fin; adjusting the threshold voltage of the surface exposed by the fin by ion implantation. The formation method of the present invention makes it easy to adjust the β ratio, improves the write redundancy of the static random access memory, and thus improves the overall performance of the formed semiconductor device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a semiconductor device and a method for forming the same. Background Art

[0002] In the current semiconductor industry, integrated circuit products can be primarily categorized into three main types: logic, memory, and analog circuits. Memory accounts for a significant portion of integrated circuit products. With the advancement of semiconductor technology, the wider application of memory requires integrating memory with other components on a single chip to create embedded semiconductor memory devices. For example, memory can be embedded within a central processing unit (CPU) for compatibility while maintaining the original memory specifications and corresponding electrical performance.

[0003] Generally, it is necessary to make the memory compatible with the embedded standard logic device. For embedded semiconductor devices, they are usually divided into a logic area and a memory. The logic area usually includes logic devices, and the memory area includes memory devices. With the development of storage technology, various types of semiconductor memories have emerged, such as static random access memory (SRAM), dynamic random access memory (DRAM), erasable programmable read-only memory (EOROM), and flash memory. Due to the advantages of low power consumption and fast operating speed, static random access memory and its formation method have attracted more and more attention.

[0004] In semiconductor device manufacturing methods, there are two common methods for adjusting the alpha, beta, and gamma ratios of static random access memory (SRAM) to achieve better device performance. One method involves using different numbers of fins for the pull-up transistor (PU), pass transistor (PG), and pull-down transistor (PD), such as 1, 1, 1, or 1, 1, 2, or 1, 2, 3, respectively. Another method involves using fin structures of varying heights to adjust the alpha, beta, and gamma ratios of the SRAM.

[0005] When adjusting the alpha ratio, beta ratio, and gamma ratio of a static random access memory (SRAM) by selecting different numbers of fins for the pull-up transistor (PU), pass transistor (PG), and pull-down transistor (PD), the beta ratio cannot be changed. Adjusting the beta ratio requires forming different mask layers for the pass transistor (PG) and the pull-down transistor (PD) and changing the beta ratio through threshold voltage adjustment injection. However, due to the continuous shrinking size of the static random access memory, it is difficult to adjust the beta ratio by forming different mask layers for the pass transistor (PG) and the pull-down transistor (PD). Summary of the Invention

[0006] The problem solved by the present invention is to provide a semiconductor device and a method for forming the same, which facilitates the adjustment of the β ratio, improves the write redundancy of the static random access memory, and thus improves the overall performance of the formed semiconductor device.

[0007] To solve the above problems, the present invention provides a method for forming a semiconductor device, comprising: providing a substrate, the substrate comprising a pull-up transistor region, a pull-down transistor region, and a transfer transistor region; forming a plurality of discretely arranged fins on the substrate, the fins comprising a first fin located simultaneously in the transfer transistor region and the pull-down transistor region, a second fin located in the pull-down transistor region, and a third fin located in the pull-up transistor region; forming a mask layer on the substrate, the mask layer simultaneously exposing the surface of the second fin and the surface of the third fin, or the mask layer exposing the surface of the first fin; and adjusting the threshold voltage of the exposed surface of the fin by ion implantation.

[0008] Optionally, when the mask layer exposes the surface of the second fin and the surface of the third fin at the same time, N-type ion implantation is performed on the surface of the second fin and the surface of the third fin.

[0009] Optionally, the N-type ions include P, As or Sb.

[0010] Optionally, the parameters of the N-type ion implantation include: an implantation energy of 4keV to 15keV, an implantation dose of 1E12atom / cm 2 to 1E15atom / cm 2 , the injection angle is 0 degrees to 20 degrees, the twist angle is 24 degrees, and the number of injections is 5.

[0011] Optionally, when the mask layer exposes the surface of the first fin, P-type ion implantation is performed on the surface of the first fin.

[0012] Optionally, the P-type ions include B, Ga or In.

[0013] Optionally, the parameters of the P-type ion implantation include: an implantation energy of 2keV to 4keV, an implantation dose of 1E11atom / cm 2 to 1E13atom / cm 2 , the injection angle is 0 degrees to 10 degrees, the twist angle is 20 degrees, and the number of injections is 5.

[0014] Optionally, before forming the mask layer on the substrate, the method further includes: forming a sacrificial oxide layer on the substrate and the surface of the fin.

[0015] Optionally, after adjusting the threshold voltage of the surface exposed by the fin by ion implantation, the method further includes: removing the mask layer.

[0016] Optionally, a gate structure spanning the fin is formed on the substrate.

[0017] Optionally, the mask layer is removed by wet etching, dry etching or ashing process.

[0018] Correspondingly, using the above-mentioned formation method, the present invention also provides a semiconductor device, including: a substrate, the substrate including a pull-up transistor region, a pull-down transistor region and a transfer transistor region; a plurality of fins, discretely arranged on the substrate, including a first fin, a second fin, and a third fin, wherein: the first fin is located in the transfer transistor region and the pull-down transistor region at the same time, the second fin is located in the pull-down transistor region; the third fin is located in the pull-up transistor region; a mask layer, located on the substrate, simultaneously exposing the surface of the second fin and the surface of the third fin, or exposing the surface of the first fin; and implanted ions, located in the second fin and the third fin or in the first fin.

[0019] Optionally, the second fin and the third fin have the same type of implanted ions.

[0020] Compared with the prior art, the technical solution of the present invention has the following advantages:

[0021] A plurality of discretely arranged fins are formed on a substrate, the fins including a first fin located in both the transfer transistor region and the pull-down transistor region, a second fin located in the pull-down transistor region, and a third fin located in the pull-up transistor region. A mask layer is formed on the substrate, and the mask layer is used to simultaneously expose the surfaces of the second fin and the third fin or the surface of the first fin. When adjusting the threshold voltage of the exposed fin surfaces by ion implantation, the surfaces of the second fin and the third fin can be implanted with the same type of ions, so that the second fin has different electrical properties from the first fin, thereby The fin and the fin on the transfer transistor area have different electrical properties, so that the β ratio can be adjusted; at the same time, since the mask layer exposes the second fin and the third fin at the same time or exposes the first fin (that is, covers the second fin and the third fin at the same time), the β ratio can be adjusted by forming a mask layer, saving costs; in addition, the distance between the second fin and the third fin is large, and it is easy to form a mask layer with good coverage quality, which makes the formation process of the mask layer simple, thereby making it easy to adjust the β ratio, improving the write redundancy of the static random access memory, and improving the overall performance of the formed semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figures 1 to 9 is a structural schematic diagram of a semiconductor device forming process according to a first embodiment of the present invention;

[0023] Figures 10 to 14 It is a structural diagram of the semiconductor device forming process in the second embodiment of the present invention. DETAILED DESCRIPTION

[0024] Currently, a common method for adjusting the alpha ratio, beta ratio, and gamma ratio of static random access memory (SRAM) is to select different numbers of fins for the pull-up transistor (PU), pass transistor (PG), and pull-down transistor (PD). In this case, the beta ratio is equal to the ratio of the number of fins of the pull-down transistor (PD) to the number of fins of the pass transistor (PG).

[0025] The inventors discovered that the β ratio formed using this method is immutable. Therefore, when the β ratio needs to be adjusted, different mask layers need to be formed on the pull-down transistor (PD) and the transfer transistor (PG) to adjust the threshold voltage. However, as the size of the static random access memory decreases, it is difficult to adjust the threshold voltage by forming different mask layers on the pull-down transistor (PD) and the transfer transistor (PG). As a result, the write redundancy of the static random access memory cannot be improved, which limits the use of semiconductor devices.

[0026] The inventors have discovered that by using a mask layer to simultaneously expose the surfaces of the second fin and the third fin or to expose the surface of the first fin (i.e., simultaneously cover the second fin and the third fin), the surfaces of the second fin and the third fin can be implanted with the same type of ions, so that the second fin and the first fin have different electrical properties, and thus the fin on the pull-down transistor area and the fin on the transfer transistor area have different electrical properties, which can achieve the adjustment of the β ratio; at the same time, because the mask layer simultaneously exposes the second fin and the third fin or exposes the first fin (i.e., simultaneously covers the second fin and the third fin), the distance between the second fin and the third fin is larger, and the mask layer formation becomes easier, which simplifies the formation difficulty of the mask layer while adjusting the β ratio, improving the write redundancy of the static random access memory, and thereby improving the overall performance of the formed semiconductor device.

[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0028] First embodiment

[0029] Figures 1 to 9 It is a structural diagram of the semiconductor device forming process in the first embodiment of the present invention.

[0030] First reference Figure 1 , providing a substrate 100 , wherein the substrate 100 includes a pull-up transistor region 110 , a pull-down transistor region 120 and a transfer transistor region 130 .

[0031] The substrate 100 may be single crystal silicon, polycrystalline silicon or amorphous silicon; the substrate 100 may also be made of semiconductor materials such as silicon, germanium, silicon germanium, gallium arsenide, etc.; in this embodiment, the material of the substrate 100 is single crystal silicon.

[0032] refer to Figures 2 to 3 , a plurality of discretely arranged fins 200 are formed on the substrate 100, the fins 200 including a first fin 210 located in both the transfer transistor region 130 and the pull-down transistor region 120, a second fin 220 located in the pull-down transistor region 120, and a third fin 230 located in the pull-up transistor region 110.

[0033] Figure 2 yes Figure 3 Section view along section line AA, Figure 3 yes Figure 2 Top view of .

[0034] In this embodiment, Fin121 SRAM is used as an example. In other embodiments, Fin131 SRAM or Fin132 SRAM may also be used. Fin121 SRAM indicates that the SRAM has one fin on the pull-up transistor area, two fins on the pull-down transistor area, and one fin on the transfer transistor area. The meaning of Fin131 SRAM or Fin132 SRAM is similar.

[0035] In this embodiment, the method for forming the fin 200 is: first forming a photoresist layer on the substrate 100; after exposure and development processes, forming a photoresist pattern in the photoresist layer; then etching the substrate 100 using the patterned photoresist layer as a mask, thereby forming the fin 200 on the substrate 100.

[0036] In other embodiments, the method for forming the fin 200 may also be: forming a fin material layer on the substrate 100, and forming a photoresist layer on the fin material layer; after exposure and development processes, forming a photoresist pattern in the photoresist layer; and then etching the fin material layer using the patterned photoresist layer as a mask, thereby forming the fin 200 on the substrate 100.

[0037] refer to Figures 4 and 5 , a mask layer 300 is formed on the substrate 100 , and the mask layer 300 exposes the surface of the second fin 220 and the surface of the third fin 230 at the same time.

[0038] Figure 4 yes Figure 5 Section view along section line AA, Figure 5 yes Figure 4 Top view of .

[0039] In this embodiment, the material of the mask layer 300 is krypton fluoride (KrF); in other embodiments, the material of the mask layer 300 may also be argon fluoride (ArF).

[0040] In this embodiment, since the mask layer 300 simultaneously exposes the surface of the second fin 220 and the surface of the third fin 230, during subsequent ion implantation, the second fin 220 and the first fin 210 have different electrical properties, thereby changing the β ratio; in addition, the mask layer 300 simultaneously exposes the second fin 220 and the third fin 230. Since the distance between the second fin 220 and the third fin 230 is large, the opening of the mask layer 300 formed in this way is large, and the mask layer 300 is easy to form, which simplifies the process of forming the mask layer 300; at the same time, since the mask layer 300 simultaneously exposes the second fin 220 and the third fin 230, it is possible to achieve different electrical properties between the first fin 210 and the second fin 220, without the need for an additional mask layer, thereby saving costs.

[0041] refer to Figure 6 , the threshold voltage of the surface exposed to the fin 200 is adjusted by ion implantation.

[0042] The arrowed lines in the figure indicate the direction of ion flow.

[0043] In this embodiment, the threshold voltage of the surface exposed by the second fin 220 and the surface exposed by the third fin 230 is adjusted by ion implantation.

[0044] In this embodiment, N-type ion implantation is performed on the surface of the second fin 220 and the surface of the third fin 230 .

[0045] In this embodiment, the N-type ion is As; in other embodiments, the N-type ion may also be P or Sb.

[0046] In this embodiment, the same type of ions are implanted into the second fin 220 and the third fin 230 .

[0047] In this embodiment, the parameters of the N-type ion implantation include: an implantation energy of 4keV to 15keV, an implantation dose of 1E12atom / cm 2 to 1E15atom / cm 2 , the injection angle is 0 degrees to 20 degrees, the twist angle is 24 degrees, and the number of injections is 5.

[0048] In this embodiment, since the surface of the second fin 220 and the surface of the third fin 230 are exposed at the same time and are both injected with N-type ions, when the threshold voltage of the first fin 210 is subsequently adjusted, the type of ions injected into the first fin 210 is different from the type of ions injected into the second fin 220. In this way, the first fin 210 and the second fin 220 have different electrical properties, thereby realizing the adjustment of the β ratio, improving the write redundancy of the static random access memory, and improving the overall performance of the formed semiconductor device.

[0049] refer to Figure 7 , remove the mask layer 300.

[0050] In this embodiment, dry etching is used to remove the mask layer 300 ; in other embodiments, wet etching or ashing processes may be used to remove the mask layer 300 .

[0051] In this embodiment, the process parameters of the dry etching include: the etching gas includes HCl, the dilution gas includes N2, the molar percentage of the etching gas in the total gas is 10% to 20%, and the temperature is 80 degrees Celsius to 100 degrees Celsius.

[0052] refer to Figures 8 and 9 , a gate structure 400 is formed on the substrate 100 and spans the fin 200 .

[0053] Figure 9 yes Figure 8 In the cross-sectional view along section line AA, Figure 8 yes Figure 9 Top view of .

[0054] In this embodiment, the gate structure 400 includes a gate oxide layer (not shown in the figure) located on the surface of the fin 200 and a gate dielectric layer located on the gate oxide layer.

[0055] In this embodiment, the gate structure 400 is formed by a conventional method, which will not be further described here.

[0056] Correspondingly, the present invention also provides a semiconductor device formed using the above method, including: a substrate 100, the substrate 100 including a pull-up transistor region 110, a pull-down transistor region 120 and a transfer transistor region 130; a plurality of fins 200, located on the substrate 100, including a first fin 210, a second fin 220, and a third fin 230, wherein: the first fin 210 is located in both the transfer transistor region 130 and the pull-down transistor region 120; the second fin 220 is located in the pull-down transistor region 120; the third fin 230 is located in the pull-up transistor region 110; a mask layer 300, located on the substrate 100, simultaneously exposing the surface of the second fin 220 and the surface of the third fin 230; implanted ions, located in the second fin 220 and the third fin 230; a gate structure 400, located on the substrate 100 and spanning the fins 200.

[0057] In this embodiment, the second fin 220 and the third fin 230 have the same type of implanted ions.

[0058] Second embodiment

[0059] Figures 10 to 14 It is a structural diagram of the semiconductor device forming process in the second embodiment of the present invention.

[0060] In this embodiment, the process from providing a substrate to forming a plurality of discretely arranged fins on the substrate is the same as that of the first embodiment, and the specific reference is made to Figures 1 to 3 .

[0061] refer to Figure 10 A sacrificial oxide layer 500 is formed on the surfaces of the substrate 100 and the fin 200 .

[0062] In this embodiment, before forming a mask layer on the substrate, a sacrificial oxide layer 500 is formed on the substrate and the surface of the fin; in other embodiments, before forming a mask layer on the substrate, a sacrificial oxide layer 500 may not be formed on the substrate and the surface of the fin.

[0063] In this embodiment, the formation of the sacrificial oxide layer 500 can prevent the threshold voltage ion injection tunneling effect, isolate the substrate 100 and the subsequently formed mask layer, prevent the organic matter in the mask layer from contacting the substrate 100 and contaminating the substrate 100, and can also capture the defects on the surface of the substrate 100 and improve the interface state of the surface of the substrate 100. At the same time, the growth of the sacrificial oxide layer 500 can improve the influence of the white band effect on the device.

[0064] refer to Figures 11 to 12, a mask layer 600 is formed on the substrate 100 , and the mask layer 600 exposes the surface of the first fin 210 .

[0065] Figure 11 yes Figure 12 Section view along section line AA, Figure 12 yes Figure 11 Top view of .

[0066] In this embodiment, the mask layer 600 exposes the mask layer 600 on the surface of the first fin 210 .

[0067] In this embodiment, the material of the mask layer 600 is argon fluoride (ArF).

[0068] In this embodiment, the mask layer 600 is used to expose the surface of the first fin 210, that is, to cover the surfaces of the second fin 220 and the third fin 230. In this way, when the threshold voltage is adjusted by subsequent ion implantation of the first fin 210, the first fin 210 and the second fin 220 have different electrical properties, thereby achieving a change in the β ratio, and the change in the β ratio can be achieved without an additional mask layer, saving costs. In addition, since the distance between the second fin 220 and the third fin 230 is large, the mask layer 600 is easy to form, and the characteristic size and coverage range of the mask layer 600 are easy to control, which simplifies the formation process of the mask layer 600.

[0069] refer to Figure 13 , the threshold voltage of the exposed fin 200 is adjusted by ion implantation.

[0070] The arrowed lines in the figure indicate the direction of ion flow.

[0071] In this embodiment, P-type ion implantation is performed on the exposed first fin 210 by ion implantation.

[0072] In this embodiment, the P-type ion is B; in other embodiments, the P-type ion may also be Ga or In.

[0073] In this embodiment, the parameters of the P-type ion implantation include: an implantation energy of 2keV to 4keV, an implantation dose of 1E11atom / cm 2 to 1E13atom / cm 2 , the injection angle is 0 degrees to 10 degrees, the twist angle is 20 degrees, and the number of injections is 5.

[0074] In this embodiment, since the second fin 220 and the third fin 230 are covered at the same time, the first fin 210 is exposed and P-type ions are injected, which subsequently results in different types of injected ions in the first fin 210 and the second fin 220. In this way, the first fin 210 and the second fin 220 have different electrical properties, thereby achieving the adjustment of the β ratio, thereby improving the write redundancy of the static random access memory and improving the overall performance of the formed semiconductor device.

[0075] refer to Figure 14 After adjusting the threshold voltage of the exposed fin 200 by ion implantation, the mask layer 600 and the sacrificial oxide layer 500 are removed.

[0076] After removing the mask layer 600, the process of forming the gate structure 400 across the fin on the substrate is the same as that of the first embodiment, for details, refer to Figures 8 and 9 .

[0077] Accordingly, the present invention also provides a semiconductor device formed using the above method, comprising: a substrate 100, the substrate 100 including a pull-up transistor region 110, a pull-down transistor region 120 and a transfer transistor region 130; a plurality of fins 200, located on the substrate 100, including a first fin 210, a second fin 220, and a third fin 230, wherein: the first fin 210 is located at both the transfer transistor region 130 and the pull-down transistor region 120; the second fin 220 is located at the pull-down transistor region 120; the third fin 230 is located at the pull-up transistor region 110; a sacrificial oxide layer 500, located on the substrate 100 and on the surface of the fin 200; a mask layer 600, located on the substrate 100, while exposing the surface of the first fin 210; implanted ions, located in the first fin 210; and a gate structure 400, located on the substrate 100 and spanning the fin 200.

[0078] In this embodiment, the second fin 220 and the third fin 230 have the same type of implanted ions.

[0079] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the scope defined by the claims.

Claims

1. A method for forming a semiconductor device, characterized in that: include: providing a substrate, the substrate comprising a pull-up transistor region, a pull-down transistor region, and a transfer transistor region; forming a plurality of discretely arranged fins on the substrate, the fins comprising a first fin located in both the transfer transistor region and the pull-down transistor region, a second fin located in the pull-down transistor region, and a third fin located in the pull-up transistor region; forming a mask layer on the substrate, wherein the mask layer simultaneously exposes a surface of the second fin and a surface of the third fin, or the mask layer exposes a surface of the first fin; The threshold voltage of the surface where the fin is exposed is adjusted by ion implantation.

2. The forming method according to claim 1, characterized in that: When the mask layer exposes the surface of the second fin and the surface of the third fin at the same time, N-type ion implantation is performed on the surface of the second fin and the surface of the third fin.

3. The forming method according to claim 2, characterized in that: The N-type ions include P, As or Sb.

4. The forming method according to claim 3, characterized in that: The parameters of the N-type ion implantation include: the implantation energy is 4keV to 15keV, the implantation dose is 1E12atom / cm 2 To 1E15atom / cm 2 , the injection angle is 0 degrees to 20 degrees, the twist angle is 24 degrees, and the number of injections is 5.

5. The forming method according to claim 1, characterized in that: When the mask layer exposes the surface of the first fin, P-type ions are implanted into the surface of the first fin.

6. The forming method according to claim 5, characterized in that: The P-type ions include B, Ga or In.

7. The forming method according to claim 6, characterized in that: The parameters of the P-type ion implantation include: the implantation energy is 2keV to 4keV, the implantation dose is 1E11atom / cm 2 to 1E13atom / cm 2 , the injection angle is 0 degrees to 10 degrees, the twist angle is 20 degrees, and the number of injections is 5.

8. The forming method according to claim 1, characterized in that: Before forming the mask layer on the substrate, the method further includes: forming a sacrificial oxide layer on the substrate and the surface of the fin.

9. The forming method according to claim 1, characterized in that: After adjusting the threshold voltage of the surface of the exposed fin by ion implantation, the method further includes: removing the mask layer.

10. The forming method according to claim 9, characterized in that: A gate structure is formed on the substrate and spans the fin.

11. The forming method according to claim 9, characterized in that: The mask layer is removed by wet etching, dry etching or ashing process.

12. A semiconductor device formed by the forming method according to any one of claims 1 to 11, characterized in that: include: a substrate, the substrate comprising a pull-up transistor region, a pull-down transistor region, and a transfer transistor region; A plurality of fins are separately arranged on the substrate, including a first fin, a second fin, and a third fin, wherein: the first fin is located in both the transfer transistor region and the pull-down transistor region; The second fin is located in the pull-down transistor region; The third fin is located in the pull-up transistor region; a mask layer, located on the substrate, exposing a surface of the second fin and a surface of the third fin at the same time, or exposing a surface of the first fin; The implanted ions are located in the second fin and the third fin or in the first fin.

13. The semiconductor device according to claim 12, wherein: The second fin and the third fin have the same type of implanted ions.

Citation Information

Patent Citations

  • Semiconductor structure forming method

    CN105097495A

  • Semiconductor device and manufacturing method thereof, and electronic apparatus

    CN105206577A