Low-temperature roasting, leaching and recycling iron removal process of sodium ferroaluminate

Through the low-temperature roasting and leaching cycle iron removal process of yellow sodium iron alum, the problems of large slag volume and low iron grade of iron removal process in hydrometallurgy are solved, and the resource processing and energy consumption of iron slag removal are achieved, which improves the removal of iron slag Iron effect and recovery rate.

CN112593074BActive Publication Date: 2024-11-15ANHUI TONGGUAN NONFERROUS METALS (CHIZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011274977.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-16
Publication Date
2024-11-15
Estimated Expiration
2040-11-16

AI Technical Summary

Technical Problem

The iron removal process in the existing hydrometallurgy has problems such as large slag volume, low iron grade, high sulfuric acid consumption, high equipment requirements, and high energy consumption, especially the difficulty in applying the yellow sodium iron alum method.

Method used

The low-temperature roasting and leaching cycle iron removal process is adopted to generate pre-liquid reaction of yellow sodium iron alum, and the roasting and decomposition are used to generate iron sulfate and iron oxide. The slurry leaching and water washing cycle are used to recover valuable elements, so as to achieve the resource of iron slag removal .

Benefits of technology

The reduction and resource utilization of iron slag removal has been achieved, energy consumption and environmental pollution have been reduced, the grade and recovery rate of iron slag removal have been improved, and costs and environmental protection have been saved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112593074B_ABST
    Figure CN112593074B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of iron removal in hydrometallurgy, and discloses a sodium ferroaluminate low-temperature roasting leaching cycle iron removal process, comprising the following steps: S1, pre-liquid reaction: collect the pre-liquid of alum precipitation and adjust the pH value to 1.5-2.0, mix it with the roasting slag leachate, control the temperature to 90-100°C, react for 4-6h, react the sodium ions and iron ions therein to generate sodium ferroaluminate precipitation, and adopt sedimentation or filter pressing to separate solid and liquid after the reaction is completed, the liquid after alum precipitation returns to the main system, and the ferroaluminate slag is transported to the roasting process; S2, roasting decomposition: roasting and decomposing the ferroaluminate slag in a roasting furnace at 450-480°C to produce ferric sulfate, ferric oxide, sodium sulfate solid and water vapor, and the generated water vapor is discharged after being treated by a dynamic wave dust collector to obtain dust collection ash. The present invention has the advantages of less auxiliary material consumption, high comprehensive recovery rate, no need for desulfurization and denitrification of roasting tail gas, and high degree of resource utilization of iron removal slag, and is environmentally friendly and cost-saving.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrometallurgical iron removal, in particular to a low-temperature roasting, leaching and circulating iron removal process of natantrolite. Background Art

[0002] In the hydrometallurgical process, acidic solutions are often used to leach ores, and the iron in the minerals often enters the leachate in the form of trivalent or divalent iron ions. Since iron is very harmful in subsequent processes such as electrodeposition, iron removal is the most common and important process in hydrometallurgy.

[0003] The problem of precipitation and iron removal in the process of hydrometallurgy is the most representative in hydrometallurgy. Zinc ore generally contains 5%-15% iron. When zinc and other nonferrous metals enter the solution during the leaching process, iron also enters the solution to varying degrees. In order to precipitate iron from the solution with high iron content, the jarosite method, goethite method, and hematite method have been applied in industry as new iron precipitation methods since the late 1960s.

[0004] Although these methods basically solve the problem of iron removal from leaching solution in hydrometallurgy, they all have their own shortcomings:

[0005] The disadvantages of the ferroalloy method are large slag volume, low iron grade, high sulfuric acid consumption, and ferroalloy slag is listed in the list of hazardous wastes, with high disposal costs;

[0006] The key point of the goethite method is to keep the concentration of trivalent iron ions in the solution at a low level during the precipitation process. The efficiency is low, and the slag contains a high zinc content, which requires further pyrometallurgical treatment, and there are many subsequent problems.

[0007] Although the hematite method removes iron in small amounts and has a high iron content, it requires high temperatures and pressures, high equipment requirements, and high energy consumption, investment, and operating costs.

[0008] Therefore, we proposed a low-temperature roasting and leaching cycle iron removal process of sodium ferroaluminate to solve the above problems. Summary of the invention

[0009] The purpose of the present invention is to solve the disadvantages of the prior art such as the difficulty in application of diamond powder, and to propose a low-temperature roasting, leaching and circulating iron removal process of sodium ferroaluminate.

[0010] The low-temperature roasting, leaching and circulating iron removal process of sodium ferroaluminate comprises the following steps:

[0011] S1, pre-liquid reaction: collect the pre-liquid of alum precipitation and adjust the pH value to 1.5-2.0, mix it with the roasting slag leaching solution, control the temperature to 90-100°C, react for 4-6h, so that the sodium ions react with the iron ions to form yellow sodium ferroaluminate precipitation, and after the reaction is completed, use sedimentation or filter press to separate the solid and liquid, return the pre-liquid of alum precipitation to the main system, and transport the ferroaluminate slag to the roasting process;

[0012] S2, roasting and decomposition: roasting and decomposing the iron alum slag in a roasting furnace at 450-480°C to produce iron sulfate, iron oxide, sodium sulfate solid and water vapor. The produced water vapor is treated by a dynamic wave dust collector and then discharged to obtain dust collection ash;

[0013] S3, slurry leaching: the calcined slag and dust ash of the generated iron sulfate, iron oxide and sodium sulfate solids are added with neutral leachate or weak acid leachate for slurry leaching, the liquid-solid ratio is controlled at 2-4:1, the temperature is 70-80°C, the reaction time is 0.8-1.2h, the sodium sulfate therein is fully dissolved into the leachate, and after the reaction is completed, the solid-liquid separation is carried out, the leachate is returned to the alum precipitation process, and the leached slag is sent to the water washing process;

[0014] S4, water washing cycle: add water to the leached residue to make it slurry, control the liquid-solid ratio to 3-5:1, the temperature to 50-70℃, the reaction time to 0.8-1.2h, fully dissolve the soluble salts of the valuable elements remaining in the residue, and perform solid-liquid separation after the reaction is completed. The solid product is the final iron-removing residue, and the solution is enriched and circulated or circulated after adding alkali to precipitate zinc to recover the valuable elements therein.

[0015] Preferably, in S1, if the iron ion concentration is high, a neutralizing agent such as ammonium bicarbonate, sodium bicarbonate or zinc oxide is added during the reaction.

[0016] Preferably, in S1, the reaction chemical formula for generating yellow sodium iron alum precipitate is: Na2SO4+3Fe2(SO4)3+12H2O→2NaFe3(SO4)2(OH)6+6H2SO4.

[0017] Preferably, in S2, the chemical formula of the reaction occurring during calcination and decomposition is: 2NaFe3(SO4)2(OH)6→Na2SO4+Fe2(SO4)3+2Fe2O3+6H2O.

[0018] Preferably, in S4, the reaction chemical formula of adding alkali to precipitate zinc is: 3ZnSO4+3Na2CO3+H2O→ZnCO3·2Zn(OH)2·H2O+2CO2+3Na2SO4.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention organically combines wet iron removal with pyrometallurgical slag treatment, utilizes the difference in water solubility of the primary decomposition products of low-temperature roasting of sodium iron alum, and realizes the recycling of valuable elements and the improvement of the grade of iron removal slag through a washing method, so as to achieve the purpose of reducing and recycling the iron removal slag. Compared with the traditional process, the sulfur, sodium and other valuable elements in the iron removal slag are fully recycled, and the iron is enriched in the slag, which can be used as a raw material for steel smelting or other metallurgical processing, which is convenient for resource processing; low-temperature roasting and decomposition do not produce harmful gases, the energy consumption is low and there is no tail gas treatment burden. The iron removal method of the present invention has the advantages of low auxiliary material consumption, high comprehensive recovery rate, no need for desulfurization and denitrification of roasting tail gas, and high degree of resource utilization of iron removal slag, which is environmentally friendly and cost-saving. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention provides a schematic diagram of the process structure of the low-temperature roasting, leaching and circulating iron removal process of sodium ferroaluminate. DETAILED DESCRIPTION

[0022] The present invention will be further explained below in conjunction with specific embodiments.

[0023] Reference Figure 1 The low-temperature roasting and leaching cycle iron removal process of sodium ferroaluminate proposed by the present invention comprises the following steps:

[0024] S1. Yellow sodium ferroalum method for iron removal

[0025] The pre-alum precipitation liquid is adjusted to a pH value of 1.5-2.0, mixed with the roasting slag leaching liquid, and the temperature is controlled at 90-100°C. The reaction is carried out for 4-6 hours to make the sodium ions react with the iron ions to form yellow sodium iron alum precipitation; if the iron ion concentration is high, a small amount of neutralizing agent such as ammonium bicarbonate, sodium bicarbonate or zinc oxide needs to be added during the reaction. After the reaction is completed, solid-liquid separation is carried out by sedimentation, filter pressing, etc. The post-alum precipitation liquid is returned to the main system, and the iron alum slag is sent to the roasting process;

[0026] The main chemical reactions of alum precipitation and iron removal are as follows:

[0027] Na2SO4+3Fe2(SO4)3+12H2O→2NaFe3(SO4)2(OH)6+6H2SO4

[0028] S2, low temperature roasting of iron alum slag

[0029] The iron alum residue is roasted in a roasting furnace at 450-480°C to allow the yellow sodium iron alum to undergo sufficient primary decomposition without secondary decomposition, producing iron sulfate, iron oxide, sodium sulfate solids and water vapor. The water vapor is discharged after being treated by a dynamic wave dust collector, and the other iron sulfate, iron oxide, sodium sulfate solids are sent to the leaching process as roasted residue;

[0030] The main chemical reactions that occur during low temperature calcination are as follows:

[0031] 2NaFe3(SO4)2(OH)6→Na2SO4+Fe2(SO4)3+2Fe2O3+6H2O

[0032] S3, leaching process

[0033] The roasted slag and dust collection ash are added with neutral leachate or weak acid leachate for slurry leaching, the liquid-solid ratio is controlled at 2-4:1, the temperature is 70-80°C, the reaction time is about 1 hour, the sodium sulfate therein is fully dissolved in the leachate, and after the reaction is completed, the solid-liquid separation is performed, the leachate is returned to the alum precipitation process, and the leached slag is sent to the water washing process;

[0034] S4, washing process

[0035] The leached residue is slurried with water, and the liquid-solid ratio is controlled at 3-5:1, the temperature is 50-70°C, and the reaction time is about 1 hour. The soluble salts of the valuable elements remaining in the residue are fully dissolved. After the reaction is completed, solid-liquid separation is performed. The solid product is the final iron-removing residue. The solution is enriched and circulated or circulated after adding alkali to precipitate zinc to recover the valuable elements. The circulation mode of the water washing liquid depends on the precocity of the iron alum in the main system. The precocity is higher and the zinc precipitation cycle is preferred. The zinc precipitation residue can be used as a neutralizer for the alum precipitation reaction in S1. The zinc precipitation solution is circulated and enriched and returned to the main system to supplement the sodium loss caused by precocity.

[0036] The main chemical reactions of alkali zinc precipitation are as follows:

[0037] 3ZnSO4+3Na2CO3+H2O→ZnCO3·2Zn(OH)2·H2O+2CO2+3Na2SO4

[0038] Example:

[0039] The main components of yellow sodium iron alum slag are calculated by weight percentage (%): Fe 23.53, Zn 3.25, Cu 0.17, S10.65, Si 1.13. The iron alum slag is placed in a calcining furnace at 450°C for 1 hour, and after cooling, a neutral leaching solution is added at a liquid-solid ratio of 2:1 for slurrying, the reaction temperature is controlled at 75°C and stirred for 1 hour, and a vacuum filtration method is used for solid-liquid separation. The filtrate can be returned to the alum precipitation process as an alum precipitation agent, and the filter residue is slurried with water at a liquid-solid ratio of 3:1, and the temperature is controlled at 60 degrees Celsius and stirred for 1 hour. A vacuum filtration method is used for solid-liquid separation and water is added for leaching. The filtrate is returned to the main system for recycling after cyclic enrichment. The filter residue is the final iron removal slag. The main components are calculated by weight percentage (%): Fe 44.91, Zn 0.40, Cu 0.10, S 1.71, Si 4.20.

[0040] The sodium ferroaluminate low-temperature roasting leaching cycle iron removal method of the present invention is to form sodium ferroaluminate by using the precipitation alum iron removal method to remove iron ions in the leachate, and then roast at a relatively low temperature after solid-liquid separation to decompose the sodium ferroaluminate into ferric sulfate, sodium sulfate and ferric oxide. The roasted slag is washed with a neutral leachate or a weak acid leachate, and the sulfate radical and sodium ion therein are recycled and utilized, so that they continue to participate in the precipitation alum iron removal reaction. The washed slag is then washed with water to recover the valuable metals therein. The main component of the iron slag after washing is ferric oxide, and the iron content is about twice that of the ferroaluminate slag, which can be used as a raw material for steel smelting or other metallurgical processes. The essence of the present invention is to utilize the water solubility difference of the primary decomposition product of the sodium ferroaluminate low-temperature roasting to realize the recycling of valuable elements and the improvement of the grade of the iron removal slag through the washing method, so as to achieve the purpose of reducing the amount of the iron removal slag and recycling it.

[0041] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A low-temperature roasting, leaching and circulating iron removal process of sodium ferroaluminate, characterized in that: The following steps are involved: S1, pre-liquid reaction: collect the pre-liquid of alum precipitation and adjust the pH value to 1.5-2.0, mix it with the roasting slag leaching solution, control the temperature to 90-100°C, react for 4-6h, so that the sodium ions react with the iron ions to form yellow sodium ferroaluminate precipitation, and after the reaction is completed, use sedimentation or filter press to separate the solid and liquid, return the pre-liquid of alum precipitation to the main system, and transport the ferroaluminate slag to the roasting process; S2, roasting and decomposition: roasting and decomposing the iron alum slag in a roasting furnace at 450-480°C to produce iron sulfate, iron oxide, sodium sulfate solid and water vapor. The produced water vapor is treated by a dynamic wave dust collector and then discharged to obtain dust collection ash; S3, slurry leaching: the calcined slag and dust ash of the generated iron sulfate, iron oxide and sodium sulfate solids are added with neutral leachate or weak acid leachate for slurry leaching, the liquid-solid ratio is controlled at 2-4:1, the temperature is 70-80°C, the reaction time is 0.8-1.2h, the sodium sulfate therein is fully dissolved into the leachate, and after the reaction is completed, the solid-liquid separation is carried out, the leachate is returned to the alum precipitation process, and the leached slag is sent to the water washing process; S4, water washing cycle: add water to the leached slag to make it slurry, control the liquid-solid ratio to 3-5:1, the temperature to 50-70℃, the reaction time to 0.8-1.2h, fully dissolve the soluble salts of the valuable elements remaining in the slag, and perform solid-liquid separation after the reaction is completed. The solid product is the final iron-removing slag, and the solution is enriched and circulated or circulated after adding alkali to precipitate zinc to recover the valuable elements. The reaction formula of adding alkali to precipitate zinc is: 3ZnSO4+3Na2CO3+H2O→ZnCO3·2Zn(OH)2·H2O+2CO2+3Na2SO4.

2. The process for removing iron from yellow sodium ferroaluminate by low temperature roasting, leaching and circulation according to claim 1, characterized in that: In S1, if the iron ion concentration is high, a neutralizing agent such as ammonium bicarbonate, sodium bicarbonate or zinc oxide is added during the reaction.

3. The low-temperature roasting, leaching and circulating iron removal process of yellow sodium ferroaluminate according to claim 1, characterized in that: In S1, the reaction chemical formula for generating yellow sodium iron alum precipitate is: Na2SO4+3Fe2(SO4)3+12H2O→2NaFe3(SO4)2(OH)6+6H2SO4.

4. The low-temperature roasting, leaching and circulating iron removal process of yellow sodium ferroaluminate according to claim 1, characterized in that: In the S2, the reaction chemical formula of the calcination decomposition is: 2NaFe3(SO4)2(OH)6→Na2SO4+Fe2(SO4)3+2Fe2O3+6H2O.