A blast furnace tuyere small sleeve and its manufacturing method
By pouring copper water into the cast film in the tuyere sleeve of the blast furnace, the tuyere sleeve body and the three-dimensional tapered copper pipe water channel are combined, combined with the wear-resistant and high-temperature resistant ceramic layer and the copper-steel composite plate structure, to solve the problem of wear and overheating of the tuyere sleeve. The problem of poor melting and welding quality is eliminated, and the thermal conductivity efficiency and service life are improved.
Patent Information
- Application Number
- CN202110079477.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-21
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2041-01-21
AI Technical Summary
The existing blast furnace tuyere sleeves are prone to wear, melting and collapse due to high-speed coal injection and increased oxygen enrichment rate. Poor welding quality leads to water leakage and low thermal conductivity, resulting in frequent water jacket failures.
Copper water is poured into the cast film to form the main body of the tuyere sleeve. It has built-in three-dimensional tapered copper water channels and wear-resistant and high-temperature resistant ceramic layers. The sealing plate is welded by copper plates and steel plates. The water channel and the main body of the tuyere sleeve are integrated structures. The ceramic layer increases wear resistance. It is heated to 835-845℃ during welding to form a copper-steel composite plate structure.
It improves the wear resistance and thermal conductivity of the air outlet sleeve, avoids overheating, melting, collapse and water leakage of the water jacket, and enhances the overall service life and performance.
Smart Images

Figure CN112662829B
Abstract
Description
Technical Field
[0001] The invention relates to a blast furnace tuyere small sleeve and a manufacturing method thereof. Background Art
[0002] The main function of the blast furnace tuyere sleeve is to supply air to the blast furnace and provide the oxygen required for fuel combustion. At the outlet of the tuyere sleeve, oxygen, coal powder and coke burn violently, generating a large amount of heat. The temperature is very high, generally exceeding 1500℃. The tuyere sleeve is generally made of copper alloy with a copper content of not less than 99.5%, and its melting point is about 1050℃. In order to prevent the water jacket from burning, circulating water is passed inside the water jacket to cool the water jacket.
[0003] In recent years, with the increase of oxygen enrichment rate of blast furnace, the temperature at the outlet of tuyere sleeve has further increased, and some have exceeded 2000℃, making the outlet of tuyere sleeve more prone to overheating, melting and collapse; in addition, as the oxygen enrichment increases, the coal injection amount also increases, making the outlet channel of tuyere sleeve prone to wear and cracking.
[0004] The above reasons work together to make the water jacket prone to the following three faults:
[0005] (1) The small sleeve tuyere is easily worn by high-speed coal injection, which affects the ventilation of the water sleeve to the blast furnace, and even causes water leakage in serious cases;
[0006] (2) Dead corners are prone to appear in the water channel inside the water jacket, resulting in local high temperature, which can easily form local vacuum and local overheating, causing the front end of the tuyere jacket to melt and collapse due to high temperature;
[0007] (3) The weld is prone to water leakage after being heated.
[0008] At present, the structure of the traditional blast furnace tuyere sleeve is as follows Figure 1 As shown. All copper or copper alloys are cast in blocks and then welded into shape. This manufacturing method has the following problems in actual use:
[0009] (1) Easy to leak. Since copper has poor welding performance and welding quality is difficult to guarantee, it is easy to leak after welding, resulting in low manufacturing yield. Some water jackets leak after working for a period of time.
[0010] (2) The outlet of the water jacket is prone to overheating, melting and collapse. Because the internal water channel structure is too simple, there are internal dead corners in the water channel, which are prone to local overheating and low heat conduction efficiency. When encountering unstable combustion, the heat conduction will not be timely, making the outlet prone to overheating, melting and collapse. Summary of the invention
[0011] The technical problem to be solved by the present invention is to propose a blast furnace tuyere sleeve and a manufacturing method thereof in view of the faults of the existing tuyere sleeve, and the technical solution adopted is:
[0012] A blast furnace tuyere sleeve comprises a tuyere sleeve body, a water channel and a sealing plate. The tuyere sleeve body is formed by pouring molten copper into a casting film, the water channel is pre-buried in the casting film, and the tuyere sleeve body and the water channel are an integrated structure; the sealing plate is welded to the end face of the air outlet end of the tuyere sleeve body, and the water inlet and outlet of the water channel are both located at the air inlet end of the tuyere sleeve body.
[0013] Furthermore, the sealing plate is welded by a copper plate and a steel plate, and the copper plate of the sealing plate is welded to the end face of the air outlet end of the air outlet small sleeve body.
[0014] A wear-resistant and high-temperature resistant ceramic layer is arranged on the inner wall of the air duct of the air outlet of the air outlet small sleeve body, the depth of the wear-resistant and high-temperature resistant ceramic layer to the air outlet is 220mm, and the thickness of the wear-resistant and high-temperature resistant ceramic layer is 0.5mm. The wear-resistant and high-temperature resistant ceramic layer increases the wear resistance of the air outlet of the air outlet small sleeve.
[0015] The wear-resistant and high-temperature resistant ceramic layer is manufactured by spraying or surfacing welding, which are both known processes and are known to those skilled in the art.
[0016] The waterway is made of a copper tube with a wall thickness of 3-5 mm. The waterway is in the shape of a three-dimensional cone as a whole. The copper tube is bent multiple times and then rolled into a cone along the vertical axis.
[0017] The present invention also provides a method for manufacturing a blast furnace tuyere sleeve, comprising the following steps:
[0018] Step 1, casting a casting film according to the size of the existing blast furnace tuyere small sleeve;
[0019] Step 2: Make waterway;
[0020] Step 3: Wax the waterway. The specific method is as follows:
[0021] Wrap plastic tape on the outer surface of the water channel, put the water channel into a 100-120℃ paraffin solution, let it stand until the temperature is constant, then quickly take it out; wait for 1-5 seconds, then quickly pour out the remaining paraffin from one end, so that a paraffin layer with a thickness of 0.3-1.5mm is attached to the inner surface of the water channel;
[0022] Step 4: Make sand filling. The specific method is as follows:
[0023] Mix the casting sand and expandable polyester beads in a volume ratio of 1: (0.1-0.2) and stir evenly;
[0024] Step 5, pouring the filling sand in step 4 into the waterway in step 2 and compacting it, and sealing the water inlet and outlet of the waterway;
[0025] Step 6: Place the water channel in step 5 in the casting film in step 1, pour molten copper at 1110-1140°C into the casting film, wait for tens of seconds until the temperature of the molten copper drops by 100°C, and quickly open the water inlet and outlet of the water channel, and slowly cool for more than three hours;
[0026] Step 7: Clean the sand filling. The specific method is as follows:
[0027] Put the blast furnace tuyere small sleeve cast in step 6 on a vibrating workbench and vibrate for more than 15 minutes, so that the filling sand poured into the water channel falls out; then insert a compressed air nozzle from one end of the water channel, quickly introduce compressed air, clean the filling sand in the water channel, and form a blast furnace tuyere small sleeve casting with a processing allowance;
[0028] Step 8: Weld a sealing plate onto the end surface of the air outlet of the casting in step 7 to form a welded part with a processing allowance;
[0029] Step 9: machining the welded parts in step 8;
[0030] Step 10, pressure test, the specific method is as follows: pass 2MPa water pressure test from the inlet and outlet of the waterway, maintain the pressure for 5-20 minutes without leakage, it is qualified, otherwise, it is unqualified;
[0031] In step 11 and step 10, the qualified parts are processed into a wear-resistant and high-temperature resistant ceramic layer, and polished until the thickness of the wear-resistant and high-temperature resistant ceramic layer is 0.5 mm.
[0032] In a further embodiment of the method of the present invention, in step 2, the water channel is a copper tube with a wall thickness of 3-5 mm, and the specific method of the water channel is as follows:
[0033] A copper tube with a wall thickness of 3-5 mm is selected, and the openings at both ends of the copper tube are respectively a water inlet and a water outlet; the copper tube is formed from the water inlet to the front section as the first water inlet section, and the first bend is performed at the end of the first water inlet section. After the first bend, the water outlet of the copper tube faces the side where the water inlet is located, and the first bending arc is formed at the first bending point;
[0034] After the first bend, the copper tube moves forward a section as the second water inlet section. The water flow direction of the second water inlet section is opposite to that of the first water inlet section. A second bend is performed at the end of the second water inlet section. After the second bend, the water outlet of the copper tube faces the side away from the water inlet, and a second bending arc is formed at the second bend.
[0035] After the second bend, the copper tube moves forward one section as the third water inlet section. The water flow direction of the third water inlet section is the same as that of the first water inlet section. The third bend is made at the end of the third water inlet section. After the third bend, the water outlet of the copper tube faces the side where the water inlet is located, and the third bending arc is formed at the third bend.
[0036] After the third bend, the copper tube moves forward one section as the fourth water inlet section. The water flow direction of the fourth water inlet section is the same as that of the second water inlet section. The fourth bend is made at the end of the fourth water inlet section. After the fourth bend, the water outlet of the copper tube faces the side away from the water inlet, and the fourth bend forms a fourth curved arc.
[0037] After the fourth bend, the copper tube moves forward one section as the fifth water inlet section. The water flow direction of the fifth water inlet section is the same as that of the first water inlet section. The fifth bend is made at the end of the fifth water inlet section. After the fifth bend, the water outlet of the copper tube faces the side where the water inlet is located, and the fifth bending arc is formed at the fifth bend.
[0038] After the fifth bend, the copper tube moves forward a section as the sixth water inlet section, and the end of the sixth water inlet section is the water outlet of the copper tube;
[0039] The copper tube is bent to form a curved tube. After the bending, the water outlet and the water inlet of the copper tube are located on the same side and are substantially flush with each other. The second bending arc and the fourth bending arc on the same side of the curved tube are lower than the water outlet and the water inlet of the copper tube. The first bending arc, the third bending arc and the fifth bending arc on the other side of the curved tube are substantially flush with each other.
[0040] Keeping the height shape of the bent pipe unchanged, the bent pipe is rolled into a cone along the vertical axis to form a three-dimensional conical water channel. The large end of the three-dimensional conical water channel is the side where the water outlet, water inlet, second bending arc and fourth bending arc of the copper pipe are located, and the small end of the three-dimensional conical water channel is the side where the first bending arc, third bending arc and fifth bending arc are located.
[0041] In a further scheme of the method of the present invention, in step 8, before welding, a welding plane perpendicular to the central cone hole of the casting is processed on the end face of the air outlet of the casting, and a groove is opened on the welding plane and the copper plate of the sealing plate; when welding, the casting and the sealing plate are heated to 835-845°C and welded together to form a welded part with a processing allowance.
[0042] In a further embodiment of the method of the present invention, in step 6, the molten copper is casting copper having a copper content of 98% to 99%.
[0043] In a further embodiment of the method of the present invention, the water inlet and the water outlet of the water channel are sealed with rubber plugs or copper covers.
[0044] The beneficial effects of the present invention compared with the prior art are:
[0045] In the present invention, the water channel is integrally cast by burying the copper tube. After the casting is completed, the water channel and the water jacket are in seamless contact as a whole, with low thermal resistance, good heat conduction effect, and smooth flow without dead angles. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1It is a cross-sectional view of a blast furnace tuyere small sleeve of the present invention.
[0047] Figure 2 It is a side view of the blast furnace tuyere small sleeve of the present invention.
[0048] Figure 3 This is the plan view of the curved pipe of the waterway.
[0049] Figure 4 It is a three-dimensional schematic diagram of a three-dimensional conical waterway.
[0050] Figure 5 It is a side view of a three-dimensional conical waterway.
[0051] Figure 6 This is a schematic diagram of the tuyere sleeve of the buried pipe casting. DETAILED DESCRIPTION
[0052] The technical solution of the present invention is described in detail below, but the protection scope of the present invention is not limited to the embodiments.
[0053] To make the content of the present invention more clearly understood, the following Figure 1-Figure 6 The specific implementation manner is further described.
[0054] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0055] like Figure 1 and 2 As shown, a blast furnace tuyere sleeve comprises a tuyere sleeve body 1, a water channel 2 and a sealing plate 3. The tuyere sleeve body 1 is formed by pouring molten copper into a casting film, the water channel 2 is pre-buried in the casting film, and the tuyere sleeve body 1 and the water channel 2 are an integral structure; the sealing plate 3 is welded to the end face of the air outlet end of the tuyere sleeve body 1, and the water inlet 21 and the water outlet 22 of the water channel 2 are both located at the air inlet end of the tuyere sleeve body 1.
[0056] like Figure 3 and 4 As shown, in this embodiment, the water channel 2 is made of a copper tube with a wall thickness of 3-5 mm, and the water channel 2 is in a three-dimensional cone shape as a whole, which is formed by bending the copper tube multiple times and rolling it into a cone along the vertical axis. During the bending process, the copper tube is ensured not to have wrinkles, damage, or local deformation.
[0057] In this embodiment, the water channel is integrally cast by burying copper tubes. After casting, the water channel and the water jacket are in seamless contact as a whole, with low thermal resistance, good thermal conductivity, and smooth flow without dead angles.
[0058] like Figure 1As shown, the sealing plate 3 is welded by copper plate and steel plate to form a copper-steel composite plate structure. The steel layer adopts high-temperature heat-resistant steel. The copper plate of the sealing plate 3 is welded to the end face of the air outlet end of the air outlet small sleeve body 1.
[0059] like Figure 1 As shown, a wear-resistant and high-temperature resistant ceramic layer is arranged on the inner wall of the air duct of the air outlet of the air outlet small sleeve body 1, the depth of the wear-resistant and high-temperature resistant ceramic layer to the air outlet is 220mm, and the thickness of the wear-resistant and high-temperature resistant ceramic layer is 0.5mm. The wear-resistant and high-temperature resistant ceramic layer is made by spraying or surfacing process. Spraying or surfacing process are both known processes, known to those skilled in the art.
[0060] A method for manufacturing a blast furnace tuyere sleeve comprises the following steps:
[0061] Step 1, casting a casting film according to the size of the existing blast furnace tuyere small sleeve;
[0062] Step 2: Make waterway 2;
[0063] Step 3, wax dipping of the water channel 2, the specific method is as follows: wrap plastic tape on the outer surface of the water channel 2, put the water channel 2 into a 100-120°C paraffin solution, let it stand until the temperature is constant, and then quickly take it out; wait for 1-5 seconds, and then quickly pour out the remaining paraffin from one end, so that a paraffin layer with a thickness of 0.3-1.5mm is attached to the inner surface of the water channel 2;
[0064] Step 4: Prepare filling sand. The specific method is as follows: Mix the casting sand and expandable polyester beads in a volume ratio of 1: (0.1-0.2) and stir evenly;
[0065] Step 5, pouring the filling sand in step 4 into the waterway 2 in step 2 and compacting it, and closing the water inlet 21 and the water outlet 22 of the waterway 2;
[0066] Step 6, place the water channel 2 in step 5 in the casting film of step 1, pour molten copper at 1110-1140°C into the casting film, wait for tens of seconds until the temperature of the molten copper drops by 100°C, and quickly open the water inlet 21 and the water outlet 22 of the water channel 2, and slowly cool for more than three hours;
[0067] Step 7: Clean the sand filling. The specific method is as follows:
[0068] The blast furnace tuyere small sleeve cast in step 6 is placed on a vibrating workbench and vibrated for more than 15 minutes, and the filling sand poured into the water channel 2 falls out; then a compressed air nozzle is inserted into one end of the water channel 2, and compressed air is quickly introduced to clean the filling sand in the water channel 2, thereby forming a blast furnace tuyere small sleeve casting with a processing allowance;
[0069] Step 8: In step 7, a sealing plate 3 is welded on the end surface of the air outlet of the casting to form a welded part with a processing allowance;
[0070] Step 9: machining the welded parts in step 8;
[0071] Step 10, pressure test, the specific method is as follows: pass 2MPa water through the inlet and outlet of waterway 2 for pressure test, maintain the pressure for 5-20 minutes without leakage, it is qualified, otherwise, it is unqualified;
[0072] In step 11 and step 10, the qualified parts are processed into a wear-resistant and high-temperature resistant ceramic layer, and polished until the thickness of the wear-resistant and high-temperature resistant ceramic layer is 0.5 mm.
[0073] like Figure 1 As shown, in the method of this embodiment, in step 1, a casting film is cast according to the size of the existing blast furnace tuyere small sleeve. The casting film mentioned here is a known process and is known to people in this technical field.
[0074] like Figure 3 , 4 As shown in Figure 5, in step 2, the water channel 2 selects a copper tube with a wall thickness of 3-5 mm. The specific method of the water channel 2 is as follows:
[0075] A copper tube with a wall thickness of 3-5 mm is selected, and the openings at both ends of the copper tube are respectively a water inlet and a water outlet; the two ends of the copper tube are also the water inlet 21 and the water outlet 22 of the waterway 2.
[0076] The copper tube is extended forward from the water inlet as the first water inlet section 23, and is bent for the first time at the end of the first water inlet section 23. After the first bending, the water outlet of the copper tube faces the side where the water inlet is located, and the first bending arc a is formed at the first bending point.
[0077] After the first bend, the copper tube moves forward a section as the second water inlet section 24. The water flow direction of the second water inlet section 24 is opposite to that of the first water inlet section 23. A second bend is made at the end of the second water inlet section 24. After the second bend, the water outlet of the copper tube faces the side away from the water inlet, and a second bending arc b is formed at the second bend.
[0078] After the second bend, the copper tube moves forward one section further as the third water inlet section 25. The water flow direction of the third water inlet section 25 is the same as that of the first water inlet section 23. The third bend is made at the end of the third water inlet section 25. After the third bend, the water outlet of the copper tube faces the side where the water inlet is located, and the third bending arc c is formed at the third bend.
[0079] After the third bend, the copper tube moves forward one section further as the fourth water inlet section 26. The water flow direction of the fourth water inlet section 26 is the same as that of the second water inlet section 24. The fourth bend is made at the end of the fourth water inlet section 26. After the fourth bend, the water outlet of the copper tube faces the side away from the water inlet, and the fourth bending arc d is formed at the fourth bend.
[0080] After the fourth bend, the copper tube moves forward one section further as the fifth water inlet section 27. The water flow direction of the fifth water inlet section 27 is the same as that of the first water inlet section 23. The fifth bend is made at the end of the fifth water inlet section 27. After the fifth bend, the water outlet of the copper tube faces the side where the water inlet is located, and the fifth bending arc e is formed at the fifth bend.
[0081] After the fifth bend, the copper tube moves forward one section further to serve as the sixth water inlet section 28, and the end of the sixth water inlet section 28 is the water outlet of the copper tube.
[0082] like Figure 3 As shown, the first water inlet section 23 and the sixth water inlet section 28 take into account that the size of the air inlet end of the blast furnace tuyere sleeve is larger than the size of the air outlet end, and also take into account the wall thickness of the air inlet end of the blast furnace tuyere sleeve. Therefore, there are two inflection points 29 on the first water inlet section 23. The setting of the two inflection points 29 is to ensure uniform cooling of the tuyere sleeve body 1 of the blast furnace tuyere sleeve.
[0083] like Figure 3 and 5 As shown, the bending of the copper tube is completed to form a bent tube. After the bending, the water outlet and the water inlet of the copper tube are located on the same side and are basically flush. The second bending arc b and the fourth bending arc d on the same side of the bent tube are lower than the water outlet and the water inlet of the copper tube. The first bending arc a, the third bending arc c and the fifth bending arc e on the other side of the bent tube are basically flush.
[0084] like Figure 4 As shown, the shape of the bent pipe in the height direction is kept unchanged, and then the bent pipe is rolled into a cone along the vertical axis direction to form a three-dimensional conical waterway 2. The large end of the three-dimensional conical waterway 2 is the side where the water outlet, water inlet, second bending arc b and fourth bending arc d of the copper pipe are located, and the small end of the three-dimensional conical waterway 2 is the side where the first bending arc a, third bending arc c and fifth bending arc e are located.
[0085] In this specific embodiment, in the method, in step 3, the water channel 2 is dipped in wax, and the length of waiting time after the water channel 2 is taken out of the paraffin solution can be determined according to the temperature. The higher the temperature, the shorter the waiting time, and the lower the temperature, the longer the waiting time.
[0086] In this specific embodiment, in the method, in step 4, the foundry sand and expandable polyester beads are known products and are directly purchased. When used, the foundry sand and expandable polyester beads are mixed in a volume ratio of 1: (0.1-0.2) and stirred evenly to complete the sand filling production.
[0087] In this specific embodiment, in the method, in step 5, the water inlet 21 and the water outlet 22 of the waterway 2 are sealed with rubber plugs or copper covers to prevent the filling sand from flowing out.
[0088] In this specific embodiment, in the method, in step 6, a casting mold is cast, and the prepared copper tube is placed in an appropriate position of the mold, and the design parameters are determined to ensure uniform water cooling of the tuyere sleeve body 1. The copper water is casting copper with a copper content of 98%-99%.
[0089] In this specific embodiment, in the method, after step 7 is completed, a small tuyere sleeve casting with machining allowance is formed. Figure 6 shown.
[0090] In this specific embodiment, in the method, in step 8, before welding, a welding plane perpendicular to the central cone hole of the casting is processed on the end face of the air outlet of the casting, and a groove is opened on the welding plane and the copper plate of the sealing plate 3; when welding, the casting and the sealing plate 3 are heated to 835-845°C and welded together to form a welded part with a processing allowance.
[0091] In this specific implementation manner, in the method, step 9, according to the design parameter requirements, the welded parts with machining allowance in step 8 are machined and formed.
[0092] In this specific embodiment, in the method, step 10 is to perform a pressure test on the waterway, and this pressure test method is a known method.
[0093] In this specific embodiment, in the method, in step 11, the wear-resistant and high-temperature resistant ceramic layer can be made by spraying or surfacing. In this embodiment, surfacing is preferred. Spraying or surfacing are both known processes and are known to those skilled in the art.
[0094] The above embodiments are only for illustrating the technical idea of the present invention, and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the present invention.
Claims
1. A blast furnace tuyere small sleeve, Features: The tuyere sleeve body (1) comprises a tuyere sleeve body, a water channel (2) and a sealing plate (3); the tuyere sleeve body (1) is formed by pouring molten copper into a casting mold; the water channel (2) is pre-buried in the casting mold; the tuyere sleeve body (1) and the water channel (2) are an integral structure; the sealing plate (3) is welded to the end surface of the air outlet end of the tuyere sleeve body (1); the water inlet (21) and the water outlet (22) of the water channel (2) are both located at the air inlet end of the tuyere sleeve body (1); The sealing plate (3) is welded from a copper plate and a steel plate, and the copper plate of the sealing plate (3) is welded to the end face of the air outlet end of the air outlet sleeve body (1); the water channel (2) is made of a copper tube with a wall thickness of 3-5 mm, and the water channel (2) is in a three-dimensional cone shape as a whole, and is formed by bending the copper tube multiple times and rolling it into a cone along the vertical axis direction; The specific method of the waterway (2) is as follows: A copper tube with a wall thickness of 3-5 mm is selected, and the openings at both ends of the copper tube are respectively a water inlet and a water outlet; the copper tube is formed from the water inlet to the front section as a first water inlet section (23), and a first bend is performed at the end of the first water inlet section (23). After the first bend, the water outlet of the copper tube faces the side where the water inlet is located, and a first bending arc (a) is formed at the first bend; the first water inlet section (23) is provided with two inflection points (29); After the first bend, the copper tube is further forwarded to serve as a second water inlet section (24). The water flow direction of the second water inlet section (24) is opposite to that of the first water inlet section (23). A second bend is performed at the end of the second water inlet section (24). After the second bend, the water outlet of the copper tube faces the side away from the water inlet. A second bending arc (b) is formed at the second bend. After the second bend, the copper tube is further forwarded to serve as a third water inlet section (25). The water flow direction of the third water inlet section (25) is the same as that of the first water inlet section (23). A third bend is performed at the end of the third water inlet section (25). After the third bend, the water outlet of the copper tube faces the side where the water inlet is located. A third bending arc (c) is formed at the third bend. After the third bend, the copper tube is further forwarded to serve as a fourth water inlet section (26). The water flow direction of the fourth water inlet section (26) is the same as that of the second water inlet section (24). A fourth bend is performed at the end of the fourth water inlet section (26). After the fourth bend, the water outlet of the copper tube faces a side away from the water inlet. A fourth bending arc (d) is formed at the fourth bend. After the fourth bend, the copper tube is further forwarded to serve as a fifth water inlet section (27). The water flow direction of the fifth water inlet section (27) is the same as that of the first water inlet section (23). A fifth bend is performed at the end of the fifth water inlet section (27). After the fifth bend, the water outlet of the copper tube faces the side where the water inlet is located. A fifth bending arc (e) is formed at the fifth bend. After the fifth bend, the copper tube is further forwarded to serve as the sixth water inlet section (28), and the end of the sixth water inlet section (28) is the water outlet of the copper tube; the sixth water inlet section (28) is provided with two inflection points (29); The copper tube is bent to form a curved tube. After the bending, the water outlet and the water inlet of the copper tube are located on the same side and are substantially flush with each other. The second bending arc (b) and the fourth bending arc (d) on the same side of the curved tube are lower than the water outlet and the water inlet of the copper tube. The first bending arc (a), the third bending arc (c) and the fifth bending arc (e) on the other side of the curved tube are substantially flush with each other. The shape of the bent pipe in the height direction is kept unchanged, and the bent pipe is rolled into a cone along the vertical axis direction to form a three-dimensional cone-shaped water channel (2). The large end of the three-dimensional cone-shaped water channel (2) is the side where the water outlet, the water inlet, the second bending arc (b) and the fourth bending arc (d) of the copper pipe are located, and the small end of the three-dimensional cone-shaped water channel (2) is the side where the first bending arc (a), the third bending arc (c) and the fifth bending arc (e) are located.
2. A blast furnace tuyere sleeve according to claim 1, Features: A wear-resistant and high-temperature resistant ceramic layer (4) is provided on the inner wall of the air duct of the air outlet of the air outlet small sleeve body (1), the depth of the wear-resistant and high-temperature resistant ceramic layer (4) from the air outlet inward is 220 mm, and the thickness of the wear-resistant and high-temperature resistant ceramic layer (4) is 0.5 mm.
3. A blast furnace tuyere sleeve according to claim 2, Features: The wear-resistant and high-temperature resistant ceramic layer is manufactured by spraying or surfacing process.
4. The method for manufacturing a blast furnace tuyere sleeve according to any one of claims 1 to 3, Features: The steps include: Step 1, casting a mold according to the size of the existing blast furnace tuyere small sleeve; Step 2: Make a waterway (2); Step 3: Wax the waterway (2). The specific method is as follows: Wrap plastic tape around the outer surface of the water channel (2), place the water channel (2) in a 100-120°C paraffin solution, let it stand until the temperature is constant, then quickly take it out; wait for 1-5 seconds, then quickly pour out the remaining paraffin from one end, so that a paraffin layer with a thickness of 0.3-1.5 mm is attached to the inner surface of the water channel (2); Step 4: Make sand filling. The specific method is as follows: Mix the foundry sand and expandable polyester beads in a volume ratio of 1: (0.1-0.2) and stir evenly; Step 5, pouring the filling sand in step 4 into the waterway (2) in step 2 and compacting it, and sealing the water inlet (21) and the water outlet (22) of the waterway (2); Step 6, placing the water channel (2) in step 5 in the casting mold of step 1, pouring molten copper at 1110-1140° C. into the casting mold, waiting for tens of seconds until the temperature of the molten copper drops by 100° C., and quickly opening the water inlet (21) and the water outlet (22) of the water channel (2), and slowly cooling for more than three hours; Step 7: Clean the sand filling. The specific method is as follows: The blast furnace tuyere small sleeve cast in step 6 is placed on a vibrating workbench and vibrated for more than 15 minutes, and the filling sand poured into the water channel (2) falls out; then a compressed air nozzle is inserted into one end of the water channel (2), and compressed air is quickly introduced to clean the filling sand in the water channel (2), thereby forming a blast furnace tuyere small sleeve casting with a processing allowance; Step 8: welding a sealing plate (3) to the end surface of the air outlet of the casting in step 7 to form a welded part with a processing allowance; Step 9: machining the welded parts in step 8; Step 10, pressure test, the specific method is as follows: 2MPa water is introduced into the inlet and outlet of the waterway (2) for pressure test, and if there is no leakage after maintaining the pressure for 5-20 minutes, it is qualified, otherwise it is unqualified; In step 11 and step 10, the qualified parts are processed into a wear-resistant and high-temperature resistant ceramic layer, and polished until the thickness of the wear-resistant and high-temperature resistant ceramic layer is 0.5 mm.
5. The method according to claim 4, Features: In step 8, before welding, a welding plane perpendicular to the central cone hole of the casting is processed on the end face of the air outlet of the casting, and grooves are cut on the welding plane and the copper plate of the sealing plate (3); when welding, the casting and the sealing plate (3) are heated to 835-845°C and welded together to form a welded part with a processing allowance.
6. The method according to claim 4, Features: In step 6, the molten copper is casting copper having a copper content of 98%-99%.
7. The method according to claim 4, Features: In step 5, the water inlet (21) and the water outlet (22) of the water channel (2) are sealed with rubber stoppers or copper covers.
Citation Information
Patent Citations
Stave cooler for blast furnace
CN101855369A
Blast-furnace tuyere manufacturing and inspecting method
CN104178592A
Copper water jacket and production method thereof
CN105423763A
Tiny sleeve for blast-furnace tuyere
CN202187018U
Filtering device in blast furnace pulverized coal injection tank