A Fe-Nickel Based Amorphous Soft Magnetic Alloy Powder Core Material and Its Preparation Method

Through the combination of FeNibMcBdCeCuf's iron-nickel-based amorphous soft magnetic alloy magnetic powder core material, nano BaTiO3 layer and parylene film, the problems of high magnetic loss rate and insufficient mechanical performance in high frequency and high current applications are solved. , achieving the effect of high saturation magnetic induction strength and low magnetic loss rate.

CN112700940BActive Publication Date: 2024-11-12ANHUI SMAGNET MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011514402.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-21
Publication Date
2024-11-12
Estimated Expiration
2040-12-21

AI Technical Summary

Technical Problem

The existing iron-nickel-based amorphous soft magnetic alloy magnetic powder core materials have problems such as high magnetic loss rate, insufficient saturation magnetic induction strength, insufficient mechanical strength and toughness in high frequency, high current, miniaturization and integrated applications, which are difficult to meet the needs of high-tech Strict requirements in the technical field.

Method used

The molecular iron-nickel-based amorphous soft magnetic alloy magnetic powder core material of FeaNibMcBdCeCuf is used to encapsulate nano BaTiO3 layer and cover the parylene film. It is prepared by spraying fast quenching method and chemical vapor deposition method to ensure the mechanical strength, toughness and insulation of the material. sex.

Benefits of technology

It achieves a saturated magnetic induction strength of 0.8T to 1.2T, high initial and maximum magnetic permeability, low magnetic loss rate, excellent mechanical properties and good insulation, which can resist corrosion and oxidation, and is suitable for medium and low frequency applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides an iron-nickel-based amorphous soft magnetic alloy powder core material and a preparation method thereof. The core material has the following molecular formula: Fe a Ni b M c B d C e Cu f , a+b+c+d+f=100, M element is one or more of Nb, Co, Cr, La, and the core material also has nano BaTiO 3 layer, the nano-BaTiO 3 A layer of polyparaxylene film is deposited outside the layer by chemical vapor deposition. 3 Nano-BaTiO in the layer 3 The particle size of the nano BaTiO 3 The thickness of the layer is 5mm to 10mm. The magnetic powder core material provided by the present invention has a saturation magnetic induction intensity of 0.8T to 1.2T, a high initial magnetic permeability, and excellent maximum magnetic permeability, mechanical strength and toughness; has a low magnetic loss rate at medium and low frequencies; does not oxidize when heat treated in the air, and has good insulation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnetic materials, and in particular relates to an iron-nickel based amorphous soft magnetic alloy magnetic powder core material and a preparation method thereof. Background Art

[0002] Magnetism is one of the most basic physical properties of matter. It is ubiquitous among various substances and is diverse. Therefore, magnetic materials have been widely studied and applied in various fields. Magnetic materials are divided into soft magnetic materials, permanent magnetic materials and functional magnetic materials according to their use, and soft magnetic materials are divided into traditional soft magnetic materials and new soft magnetic materials. Traditional soft magnetic materials include pure iron, silicon steel, Permalloy and soft ferrite; new soft magnetic materials include amorphous soft magnetic alloys, nanocrystalline soft magnetic alloys and soft magnetic composite materials. Amorphous nanocrystalline soft magnetic materials have very excellent comprehensive soft magnetic properties, including high saturation magnetization, low coercive force, high magnetic permeability and low loss. They meet the needs of today's society for green, energy-saving, environmental protection and high efficiency. They are one of the emerging industries with strategic sustainable development in my country. They are widely used in all walks of life in society, mainly in high-tech fields such as power electronics and electronic information. With the development and progress of these high-tech fields, more stringent requirements are put forward for soft magnetic materials, requiring materials to be high-frequency, high-current, miniaturized, integrated and low-cost. Therefore, there is an urgent need for an iron-nickel based amorphous soft magnetic alloy powder core material with low magnetic loss rate, strong saturation magnetic induction, good insulation and mechanical strength and toughness. Summary of the invention

[0003] In view of the above defects, the present invention provides an iron-nickel based amorphous soft magnetic alloy powder core material having a saturation magnetic induction intensity of 0.8T to 1.2T, a relatively high initial magnetic permeability, and excellent maximum magnetic permeability, mechanical strength and toughness, and a preparation method thereof.

[0004] The present invention provides the following technical solution: an iron-nickel-based amorphous soft magnetic alloy powder core material, wherein the core material has the following molecular formula: Fe a Ni b M c B d C e Cu f , a+b+c+d+f=100, the M element is one or more of Nb, Co, Cr, and La, the magnetic core material also has a nano BaTiO3 layer outside, and a layer of polyparaxylene film with a thickness of 3μm to 7μm is deposited by chemical vapor deposition outside the nano BaTiO3 layer.

[0005] Furthermore, the Fe atomic percentage is 38≤a≤45.

[0006] Furthermore, the atomic percentage of Ni is 30≤a≤42.

[0007] Furthermore, the atomic percentage of M is 10≤c≤15.

[0008] Furthermore, the atomic percentage of B is 5≤d≤7.

[0009] Furthermore, the atomic percentage of C is 1≤e≤3.

[0010] Furthermore, the atomic percentage of Cu is 0.45≤f≤0.10.

[0011] Furthermore, the particle size of the nano-BaTiO3 in the nano-BaTiO3 layer is 15nm-30nm, and the thickness of the nano-BaTiO3 layer is 5mm-10mm.

[0012] Furthermore, the magnetic powder core material has a saturation magnetic induction intensity of 0.8T to 1.2T.

[0013] The present invention also provides a method for preparing the above-mentioned iron-nickel-based amorphous soft magnetic alloy magnetic powder core material, comprising the following steps:

[0014] 1) According to the molecular formula Fe a Ni b M c B d C e Cu f The iron-nickel-based amorphous soft magnetic alloy core components are batched, the batched mixture is smelted into molten steel, the temperature of the molten steel is adjusted to 180° C. to 350° C., and the liquid level of the molten steel is 700 mm to 800 mm;

[0015] 2) using a single copper roller to spray and quench at a rate of 25 m / s to 35 m / s to cool the molten steel obtained in step 1) to obtain an iron-nickel based amorphous alloy thin strip, wherein the distance between the spraying nozzle and the single copper roller is 150 μm to 180 μm;

[0016] 3) heating the iron-nickel-based amorphous alloy ribbon obtained in step 2) to 200° C. to 300° C., wrapping the heated iron-nickel-based amorphous alloy ribbon with the nano-BaTiO3, and using a mold to limit the thickness of the nano-BaTiO3 layer to obtain a magnetic core material having a nano-BaTiO3 layer;

[0017] 4) The magnetic core material with the nano BaTiO3 layer obtained in step 3) is subjected to coupling treatment using a silane coupling agent, and then a layer of polyparaxylene film with a thickness of 3 μm to 7 μm is deposited using a chemical vapor deposition method to form the iron-nickel based amorphous soft magnetic alloy powder core material with the nano BaTiO3 layer coated with the polyparaxylene insulating film.

[0018] The beneficial effects of the present invention are:

[0019] 1. The molecular formula provided by the present invention is Fe a Ni b M c B d C e Cu f The iron-nickel based amorphous soft magnetic alloy powder core material ensures that the atomic percentage of iron is 38-45 and the atomic percentage of Ni is 30-42. The content of iron and nickel is increased so that the final soft magnetic alloy powder core material has a saturation magnetic induction intensity of 0.8T-1.2T, a higher initial magnetic permeability, and excellent maximum magnetic permeability, mechanical strength and toughness.

[0020] 2. The nano BaTiO3 in the nano BaTiO3 layer wrapped outside the magnetic powder core material is a strong dielectric compound material with high dielectric constant and low dielectric loss. Therefore, the molecular formula Fe prepared by the present invention is a Ni b M c B d C e Cu f The magnetic powder core material has a lower magnetic loss rate at medium and low frequencies.

[0021] 3. The present invention wraps a polyparaxylene insulating layer on the outermost layer. The good penetrating power of the polyparaxylene active molecules can form a pinhole-free, uniformly thick transparent insulating coating inside, at the bottom and around the wrapped magnetic core material with the nano-BaTiO3 layer, providing a complete high-quality protective coating for the magnetic core material with the nano-BaTiO3 layer, which can resist the damage of acid, alkali, salt spray, mold and various corrosive gases, and can ensure that the final magnetic powder core material will not be oxidized during heat treatment in the air, and has good insulation properties.

[0022] Specific embodiment

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] This embodiment provides an iron-nickel based amorphous soft magnetic alloy powder core material, the core material has the following molecular formula: Fe 40 Ni 42Cr 10 B7C 0.9 Cu 0.1 The magnetic core material also has a 5nm thick nano-BaTiO3 layer outside, and a 3μm thick polyparaxylene film is deposited by chemical vapor deposition outside the nano-BaTiO3 layer.

[0026] The particle size of the nano-BaTiO3 in the nano-BaTiO3 layer is 15 nm.

[0027] This embodiment also provides a method for preparing an iron-nickel based amorphous soft magnetic alloy powder core material, comprising the following steps:

[0028] 1) According to the molecular formula Fe 40 Ni 42 Cr 10 B7C 0.9 Cu 0.1 The iron-nickel-based amorphous soft magnetic alloy core components are batched, the batched mixture is smelted into molten steel, the temperature of the molten steel is adjusted to 180° C., and the liquid level of the molten steel is 700 mm;

[0029] 2) using a single copper roller to perform a spraying rapid quenching method at a rate of 25 m / s to cool the molten steel obtained in step 1) to obtain an Fe-Ni-based amorphous alloy thin strip, wherein the distance between the spraying nozzle and the single copper roller is 150 μm;

[0030] 3) heating the iron-nickel-based amorphous alloy ribbon obtained in step 2) to 200° C., wrapping the heated iron-nickel-based amorphous alloy ribbon with nano-BaTiO3, and using a mold to limit the thickness of the nano-BaTiO3 layer to 5 mm, to obtain a magnetic core material having a nano-BaTiO3 layer;

[0031] 4) The magnetic core material with the nano BaTiO3 layer obtained in step 3) is subjected to coupling treatment using a silane coupling agent, and then a layer of 3 μm thick polyparaxylene film is deposited using a chemical vapor deposition method to form an iron-nickel based amorphous soft magnetic alloy powder core material with a nano BaTiO3 layer coated with a polyparaxylene insulating film.

[0032] According to the test, the magnetic powder core material provided in this embodiment has a saturation magnetic induction intensity of 0.8T, a maximum magnetic permeability of 195mH / m, and a resistivity of 120×10 -8 Ω·m, mechanical strength is 47 Shore A, and elongation at break is 12.4%.

[0033] Example 2

[0034] This embodiment provides an iron-nickel based amorphous soft magnetic alloy powder core material, the core material has the following molecular formula: Fe 45 Ni 30 (Nb0.3 La 0.7 ) 15 B7C 2.55 Cu 0.45 The core material also has a nano BaTiO3 layer outside, the thickness of the nano BaTiO3 layer is 8mm, and a 5μm thick polyparaxylene film is deposited by chemical vapor deposition outside the nano BaTiO3 layer. The particle size of the nano BaTiO3 in the nano BaTiO3 layer is 22nm.

[0035] This embodiment also provides a method for preparing the above-mentioned iron-nickel based amorphous soft magnetic alloy powder core material, comprising the following steps:

[0036] 1) According to the molecular formula Fe 45 Ni 30 (Nb 0.3 La 0.7 ) 15 B7C 2.55 Cu 0.45 The iron-nickel-based amorphous soft magnetic alloy core components are batched, the batched mixture is smelted into molten steel, the temperature of the molten steel is adjusted to 260° C., and the liquid level of the molten steel is 750 mm;

[0037] 2) using a single copper roller to perform a spraying rapid quenching method at a rate of 30 m / s to cool the molten steel obtained in step 1) to obtain an Fe-Ni-based amorphous alloy thin strip, and the distance between the spraying nozzle and the single copper roller is 165 μm;

[0038] 3) heating the iron-nickel-based amorphous alloy ribbon obtained in step 2) to 250° C., wrapping the heated iron-nickel-based amorphous alloy ribbon with nano-BaTiO3, and using a mold to limit the thickness of the nano-BaTiO3 layer to 8 mm, to obtain a magnetic core material having a nano-BaTiO3 layer;

[0039] 4) The magnetic core material with the nano-BaTiO3 layer obtained in step 3) is subjected to coupling treatment using a silane coupling agent, and then a layer of 5 μm thick polyparaxylene film is deposited using a chemical vapor deposition method to form an iron-nickel based amorphous soft magnetic alloy powder core material with a nano-BaTiO3 layer coated with a polyparaxylene insulating film.

[0040] After testing, the magnetic powder core material provided in this embodiment has a saturation magnetic induction intensity of 1.05T, a maximum magnetic permeability of 213mH / m, and a resistivity of 132×10 -8 Ω·m, mechanical strength is 52 Shore A, and elongation at break is 12.6%.

[0041] Example 3

[0042] An iron-nickel-based amorphous soft magnetic alloy powder core material, characterized in that the core material has the following molecular formula: Fe 41.5 Ni 38 (Nb 0.5 Co 0.5 ) 12.5 B5C 2.725 Cu 0.275 The core material also has a 10 mm thick nano BaTiO3 layer outside, and a 7 μm thick polyparaxylene film is deposited by chemical vapor deposition outside the nano BaTiO3 layer.

[0043] The particle size of the nano-BaTiO3 in the nano-BaTiO3 layer is 17.5 nm.

[0044] This embodiment also provides a method for preparing the above-mentioned iron-nickel based amorphous soft magnetic alloy powder core material, comprising the following steps:

[0045] 1) According to the molecular formula Fe 41.5 Ni 38 (Nb 0.5 Co 0.5 ) 12.5 B5C 2.725 Cu 0.275 The iron-nickel-based amorphous soft magnetic alloy core components are batched, the batched mixture is smelted into molten steel, the temperature of the molten steel is adjusted to 350° C., and the liquid level of the molten steel is 800 mm;

[0046] 2) using a single copper roller to spray and quench at a rate of 35 m / s to cool the molten steel obtained in step 1) to obtain an iron-nickel based amorphous alloy thin strip, and the distance between the nozzle used for spraying and the single copper roller is 180 μm;

[0047] 3) heating the iron-nickel-based amorphous alloy ribbon obtained in step 2) to 300° C., wrapping the heated iron-nickel-based amorphous alloy ribbon with nano-BaTiO3, and using a mold to limit the thickness of the nano-BaTiO3 layer to 10 mm, thereby obtaining a magnetic core material having a nano-BaTiO3 layer;

[0048] 4) The magnetic core material with the nano-BaTiO3 layer obtained in step 3) is subjected to coupling treatment using a silane coupling agent, and then a layer of 5 μm thick polyparaxylene film is deposited using a chemical vapor deposition method to form an iron-nickel based amorphous soft magnetic alloy powder core material with a nano-BaTiO3 layer coated with a polyparaxylene insulating film.

[0049] According to the test, the magnetic powder core material provided in this embodiment has a saturation magnetic induction intensity of 1.2T, a maximum magnetic permeability of 241mH / m, and a resistivity of 136×10 -8Ω·m, mechanical strength is 57 Shore A, and elongation at break is 13.5%.

[0050] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may still be modified, or some or all of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

[0051] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present invention and to form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present invention and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. An iron-nickel based amorphous soft magnetic alloy powder core material, characterized in that: The powder core material has the following molecular formula: Fe a Ni b M c B d C e Cu f , a+b+c+d+f=100, the M element is one or more of Nb, Co, Cr, and La, the magnetic powder core material further has a nano-BaTiO3 layer, and a layer of polyparaxylene film with a thickness of 3μm to 7μm is deposited on the outside of the nano-BaTiO3 layer by chemical vapor deposition; the Fe atomic percentage is 38≤a≤45; the Ni atomic percentage is 30≤a≤42.

2. The iron-nickel based amorphous soft magnetic alloy powder core material according to claim 1, characterized in that: The atomic percentage of M is 10≤c≤15.

3. The iron-nickel based amorphous soft magnetic alloy powder core material according to claim 1, characterized in that: The atomic percentage of B is 5≤d≤7.

4. The iron-nickel based amorphous soft magnetic alloy powder core material according to claim 1, characterized in that: The atomic percentage of C is 1≤e≤3.

5. The iron-nickel based amorphous soft magnetic alloy powder core material according to claim 1, characterized in that: The atomic percentage of Cu is 0.45≤f≤0.

10.

6. The iron-nickel based amorphous soft magnetic alloy powder core material according to claim 1, characterized in that: The particle size of the nano-BaTiO3 in the nano-BaTiO3 layer is 15nm-30nm, and the thickness of the nano-BaTiO3 layer is 5mm-10mm.

7. The iron-nickel based amorphous soft magnetic alloy powder core material according to claim 1, characterized in that: The magnetic powder core material has a saturation magnetic induction intensity of 0.8T to 1.2T.

8. The method for preparing the iron-nickel based amorphous soft magnetic alloy powder core material according to any one of claims 1 to 7, characterized in that: The following steps are involved: 1) According to the molecular formula Fe a Ni b M c B d C e Cu f The iron-nickel based amorphous soft magnetic alloy core components are prepared, the prepared mixture is smelted into molten steel, the temperature of the molten steel is adjusted to 180° C. to 350° C., and the liquid level of the molten steel is 700 mm to 800 mm; 2) using a single copper roller to perform a spraying rapid quenching method at a rate of 25 m / s to 35 m / s to cool the molten steel obtained in step 1) to obtain an iron-nickel based amorphous alloy thin strip, wherein the distance between the spraying nozzle and the single copper roller is 150 μm to 180 μm; 3) heating the iron-nickel based amorphous alloy ribbon obtained in step 2) to 200° C. to 300° C., wrapping the heated iron-nickel based amorphous alloy ribbon with the nano-BaTiO3 layer, and using a mold to limit the thickness of the nano-BaTiO3 layer to obtain a magnetic core material having a nano-BaTiO3 layer; 4) The magnetic core material with the nano BaTiO3 layer obtained in step 3) is subjected to coupling treatment using a silane coupling agent, and then a layer of polyparaxylene film with a thickness of 3 μm to 7 μm is deposited by chemical vapor deposition to form an iron-nickel based amorphous soft magnetic alloy powder core material with a nano BaTiO3 layer coated with a polyparaxylene insulating film.