A kind of polymethyl methacrylate production device and process

Through the tower reactor and condenser combination device, the problems of energy consumption and product optical performance of the traditional multi-stage fully mixed tank reactor are solved, and the low energy consumption production and high light transmittance products of polymethyl methacrylate are realized. , meeting the requirements of optical grade PMMA materials.

CN112717869BActive Publication Date: 2024-10-25TOPOLEFIN TECHNOLOGY (QUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011558530.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-25
Publication Date
2024-10-25
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

The existing polymethyl methacrylate production process has problems such as high energy consumption and poor optical properties of the product. In particular, the traditional multi-stage fully mixed tank reactor is inefficient in removing unreacted monomers and oligomer impurities, resulting in Poor energy efficiency and low product quality.

Method used

Using a tower reactor and condenser combination device, through multi-stage tray and condenser partition design, gradient feeding and partition reaction of reaction monomers and additives are realized, combined with condensation reflux and devolatilization extruder, to control the reaction temperature and Molecular weight distribution, ensuring narrow molecular weight distribution and high purity of the polymer.

Benefits of technology

The energy consumption of the production process is reduced, the equipment is simplified, and the molecular weight distribution index of the polymethyl methacrylate product is ≤2.0, and the light transmittance is ≥90%, which meets the requirements of optical grade PMMA materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112717869B_ABST
    Figure CN112717869B_ABST
Patent Text Reader

Abstract

The present invention discloses a polymethyl methacrylate production device, comprising a tower reactor, a condenser and a reflux tank. The side line inlet of the tower reactor comprises three feed ports arranged at intervals from top to bottom, each feed port is respectively connected to an auxiliary agent feeding pipeline, and the gas phase inlet of the condenser is connected to the gas phase outlet of the tower reactor; the reflux tank has a first liquid phase inlet connected to the liquid phase outlet of the condenser and a second liquid phase inlet for feeding reaction monomers, a first liquid phase outlet for discharging heavy components and a second liquid phase outlet for discharging light components, and the first liquid phase outlet is connected to the reflux inlet and each feed port of the tower reactor. The present invention also discloses a polymethyl methacrylate production process using the polymethyl methacrylate production device. Compared with the prior art, the polymethyl methacrylate production device of the present invention has low energy consumption and the optical properties of the product obtained are good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer preparation, in particular to a polymethyl methacrylate production device and process. Background Art

[0002] Polymethyl methacrylate (PMMA) is a copolymer composed of methyl methacrylate (MMA) and a small amount of acrylic ester monomers. It has good light transmittance, electrical insulation, acid and alkali resistance, heat resistance and cold resistance. It has a wide range of applications in the field of optical materials and daily use, and can be used in liquid crystal light guide plate films, optical fiber materials, LED materials, etc.

[0003] For the optical properties of PMMA, molecular weight distribution is a very important parameter. The smaller the molecular weight distribution index, the less light transmission loss in PMMA, and the better the light transmittance of PMMA. Free radical polymerization is mostly used in the current PMMA production process. Traditional free radical polymerization methods include solution polymerization, suspension polymerization and bulk polymerization. Free radical polymerization has the advantages of a wide variety of polymerizable monomers, mild reaction conditions, and easy control. However, free radical polymerization also has the problem that active chain free radicals are easy to couple or disproportionately terminate, resulting in the difficulty in controlling the molecular weight and molecular weight distribution of the polymerization product. The resulting PMMA often has a wider molecular weight and cannot meet the growing demand for high-performance PMMA. For PMMA with a narrower distribution and more regularity, it is necessary to obtain it through process control or active polymerization. The following introduces two publicly available methods for preparing optical-grade PMMA:

[0004] The invention patent "Optical grade polymethyl methacrylate continuous solution polymerization process and equipment used" with patent application number CN200710043411.9 (publication number CN101338001A) discloses an optical grade polymethyl methacrylate continuous solution polymerization process and equipment used, which is divided into four steps: refining distillation, polymerization reaction, flash devolatilization and wire drawing granulation. The inhibitors of the monomers, residual impurities and water are removed by distillation refining; the unreacted monomers, solvents and impurities are removed by two-stage flash devolatilization; the molecular weight of PMMA is controlled by temperature control and the addition of additives, so that the prepared PMMA meets the optical grade requirements. This PMMA production process adopts a solvent method. Compared with the traditional suspension polymerization method, it does not need to introduce a suspending agent or emulsifier, so the products produced will not be affected by additives, but compared with the bulk polymerization method, the step of handling the solvent is added, and the solvent is difficult to completely remove, and a dry PMMA finished product cannot be obtained. This process can effectively remove monomers and additives from PMMA products and recycle them, but the polymerization kettle has poor heat removal capacity and is not easy to remove the reaction heat during the reaction. In addition, the use of a multi-stage devolatilization device consumes a lot of energy and is costly.

[0005] The invention patent "Production Process of Optical-Grade Polymethyl Methacrylate" with patent application number CN201310101962.1 (publication number CN103130947B) discloses a production process of optical-grade polymethyl methacrylate, which is based on continuous bulk polymerization and adopts a process of two-stage fully mixed kettle reactors in series. The polymerization process is controlled by adjusting the amount of comonomers, initiators and chain transfer agents added, and finally an optical-grade PMMA product is obtained. The process disclosed in this patent is simple and convenient, the production process is environmentally friendly and efficient, and it is suitable for large-scale industrial application production. It uses a two-stage series kettle reactor, which can effectively control the reaction conditions of different reaction stages and make the entire polymerization process more flexible, but it cannot avoid excessive monomer and oligomer impurities mixed in the polymer, which increases the burden of post-processing, has poor energy utilization, and low product quality.

[0006] It can be seen that most of the existing industrial optical-grade PMMA production processes use a multi-stage continuous fully mixed kettle reactor in series. This process realizes the spatial separation of different stages in the reaction process, making the reaction residence time, reaction temperature and feeding controllable at different stages of the reaction, making the production process more flexible. By adjusting the reaction temperature, residence time and the addition method of the additives in different reactors, and then regulating the entire polymerization process, PMMA products with different characteristics can be obtained. However, the kettle reactor has the following disadvantages: First, the polymerization reaction is carried out in the reactor, and the unreacted monomers and some oligomer impurities cannot be removed in time during the reaction process; second, the polymerization of PMMA is an exothermic reaction, and a large amount of heat is released during the polymerization process. However, it is difficult to remove heat in the kettle reactor, and the exothermic reaction is not easy to control, resulting in the temperature of the reaction system rising continuously, the reaction rate accelerating, the viscosity of the reaction system increasing continuously, and the gel effect. In addition, the increase in reaction temperature will also aggravate the side reactions, resulting in the generation of more impurities such as dimers, which not only destroys the stable reaction system, but also increases the burden on post-processing equipment and reduces energy utilization. Summary of the invention

[0007] The first technical problem to be solved by the present invention is to provide a polymethyl methacrylate production device with low energy consumption and good optical properties of the product produced, in view of the current status of the prior art.

[0008] The second technical problem to be solved by the present invention is to provide a polymethyl methacrylate production process using the polymethyl methacrylate production device.

[0009] The technical solution adopted by the present invention to solve the above-mentioned first technical problem is: a polymethyl methacrylate production device, characterized in that it includes:

[0010] A tower reactor, wherein the side line inlet comprises a first feed port, a second feed port and a third feed port which are arranged at intervals from top to bottom, wherein the first feed port, the second feed port and the third feed port are respectively connected to a first auxiliary agent feeding pipeline, a second auxiliary agent feeding pipeline and a third auxiliary agent feeding pipeline, and the inner cavity of the tower reactor is divided into a side line extraction zone, a first reaction zone, a second reaction zone and a third reaction zone which are arranged in sequence from top to bottom, the upper part of the tower reactor has a gas phase outlet, a reflux inlet and a side line extraction port which are connected to the side line extraction zone, and the lower part of the tower reactor has a reaction liquid outlet which is connected to the third reaction zone;

[0011] a condenser, whose gas phase inlet is connected to the gas phase outlet of the tower reactor; and

[0012] A reflux tank has a first liquid phase inlet connected to the liquid phase outlet of the condenser and a second liquid phase inlet for feeding reaction monomers, a first liquid phase outlet for discharging heavy components and a second liquid phase outlet for discharging light components, wherein the first liquid phase outlet is connected to the reflux inlet through a reflux pipeline, connected to the first feed port through a first reaction monomer feeding pipeline, connected to the second feed port through a second reaction monomer feeding pipeline, and connected to the third feed port through a third reaction monomer feeding pipeline.

[0013] In order to ensure the full reaction of the materials inside the tower reactor, the tower reactor includes a tower body and a tower kettle connected to the bottom of the tower body. A plurality of tower plates arranged alternately from top to bottom are installed in the tower body.

[0014] In order to facilitate the movement of the reaction liquid in the tower body, the tower plates are arranged at an angle.

[0015] In order to reasonably partition the tower reactor, the first feed inlet, the second feed inlet and the third feed inlet are respectively located in the middle, the lower middle and the lower part of the tower body.

[0016] In order to ensure the removal effect of impurities at the side line production area, the side line production port is higher than the first feed port, and there are at least three tower plates in the area between the side line production port and the first feed port.

[0017] In order to conveniently adjust the flow rate of the reaction monomers and the auxiliary agent fed into the tower reactor, thereby controlling the monomer conversion rate of each reaction zone, the first auxiliary agent feeding pipeline is equipped with a first flow regulating valve capable of controlling the flow rate of the first auxiliary agent feeding pipeline, the second auxiliary agent feeding pipeline is equipped with a second flow regulating valve capable of controlling the flow rate of the second auxiliary agent feeding pipeline, and the third auxiliary agent feeding pipeline is equipped with a third flow regulating valve capable of controlling the flow rate of the third auxiliary agent feeding pipeline;

[0018] The first reaction monomer feeding pipeline is installed with a fourth flow regulating valve capable of controlling the flow of the first reaction monomer feeding pipeline, the second reaction monomer feeding pipeline is installed with a fifth flow regulating valve capable of controlling the flow of the second reaction monomer feeding pipeline, and the third reaction monomer feeding pipeline is installed with a sixth flow regulating valve capable of controlling the flow of the third reaction monomer feeding pipeline.

[0019] In order to facilitate the sufficient mixing of the reaction monomers and the auxiliary agents, the first auxiliary agent feeding pipeline and the first reaction monomer feeding pipeline at least partially share the same pipeline, the second auxiliary agent feeding pipeline and the second reaction monomer feeding pipeline at least partially share the same pipeline, and the third auxiliary agent feeding pipeline and the third reaction monomer feeding pipeline at least partially share the same pipeline.

[0020] In order to make the side line extraction zone and the first reaction zone have a temperature mutation point, to ensure that the reaction monomers after entering the reactor basically flow downward to participate in the polymerization reaction, and to ensure that the side line extraction zone achieves a better removal effect, a supercooler capable of cooling the material of the first reaction monomer feeding pipeline is installed on the first reaction monomer feeding pipeline.

[0021] In order to further purify the product, a devolatilizing extruder for removing residual monomers in the reaction liquid is also included, and the material inlet of the devolatilizing extruder is connected to the reaction liquid outlet of the tower reactor.

[0022] In order to facilitate the transportation of materials, the side line extraction port is connected to an intermediate product extraction pipeline, and the intermediate product extraction pipeline is installed with a first delivery pump capable of outputting materials from the side line extraction port of the tower reactor;

[0023] A second delivery pump capable of delivering materials from the reaction liquid outlet of the tower reactor to the material inlet of the devolatilizer extruder is installed between the material inlet of the devolatilizer extruder and the reaction liquid outlet of the tower reactor.

[0024] The technical solution adopted by the present invention to solve the above second technical problem is: a polymethyl methacrylate production process using the above polymethyl methacrylate production device comprises the following steps:

[0025] (1) continuously feeding the reaction monomers into a reflux tank, mixing the initiator and the reaction monomers and feeding them into a tower reactor through a first feed port, and starting polymerization in a first reaction zone;

[0026] (2) When the conversion rate reaches 30-40%, the reaction monomer is fed into the tower reactor through the second feed port, mixed with the reaction liquid preliminarily polymerized in the first reaction zone, and repolymerized in the second reaction zone;

[0027] (3) When the conversion rate reaches 60-80%, a chain transfer agent is fed into the tower reactor through the second feed port to control the molecular weight of the polymer in the reaction system;

[0028] (4) When the reaction liquid enters the third reaction zone, the chain transfer agent and the reaction monomer are mixed and fed into the tower reactor through the third feed port, mixed with the reaction liquid that has undergone repolymerization in the second reaction zone, and final polymerization is carried out in the third reaction zone;

[0029] (5) The volatilized monomers in the tower reactor are discharged from the gas phase outlet, condensed in the condenser, and then enter the reflux tank. After the stratification in the reflux tank, the monomers are recombined into four streams, one of which is returned to the tower reactor through the reflux inlet as reflux, and the other three streams are respectively fed into the tower reactor through the first feed inlet, the second feed inlet, and the third feed inlet;

[0030] (6) The intermediate product in the tower reactor is discharged through the side line outlet.

[0031] In order to control the reaction process and obtain optical grade PMMA with narrow molecular weight,

[0032] In step (1), the monomer flow rate is controlled to be 1000-1550 kg / h, and the initiator flow rate is controlled to be 0.4-0.71 kg / h;

[0033] In step (2), the monomer flow rate is controlled to be 800-1600 kg / h;

[0034] In step (3), the chain transfer agent flow rate is controlled to be 2 to 4.5 kg / h;

[0035] In step (4), the monomer flow rate is controlled to be 600-1500 kg / h, and the chain transfer agent flow rate is controlled to be 1.5-4 kg / h.

[0036] Compared with the prior art, the advantages of the present invention are: a tower reactor is used to replace the traditional process of multi-stage fully mixed kettle reactors in series, which simplifies the process equipment and reduces the energy consumption in the production process. The PMMA product produced meets the requirements of optical grade PMMA materials, with a molecular weight distribution index of ≤2.0 and a light transmittance of ≥90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a schematic structural diagram of an embodiment of a polymethyl methacrylate production device of the present invention;

[0038] Figure 2 for Figure 1 Schematic diagram of the structure of the mid-tower reactor. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below with reference to the accompanying drawings.

[0040] like Figure 1 and Figure 2 FIG. 1 is a preferred embodiment of the polymethyl methacrylate production device of the present invention. The polymethyl methacrylate production device comprises a tower reactor 1 , a condenser 2 , a reflux tank 3 and a devolatilization extruder 4 .

[0041] The tower reactor 1 includes a tower body 11 and a tower kettle 12 connected to the bottom of the tower body 11 .

[0042] A plurality of tower plates 111 are installed in the tower body 11 , which are staggered from top to bottom, and the tower plates 111 are arranged at an angle, which is beneficial for the movement of the reaction liquid in the tower body 11 .

[0043] The side inlet of the tower reactor 1 includes a first feed port 112, a second feed port 113 and a third feed port 114 arranged at intervals from top to bottom. The first feed port 112, the second feed port 113 and the third feed port 114 are respectively located in the middle, the lower middle and the lower part of the tower body 11, and are respectively connected with the first auxiliary agent feeding pipeline 13, the second auxiliary agent feeding pipeline 14 and the third auxiliary agent feeding pipeline 15, and the inner cavity of the tower reactor 1 is divided into a side line extraction area 10a, a first reaction area 10b, a second reaction area 10c and a third reaction area 10d arranged in sequence from top to bottom. The material transported by the first auxiliary agent feeding pipeline 13 is an initiator, and the materials transported by the second auxiliary agent feeding pipeline 14 and the third auxiliary agent feeding pipeline 15 are chain transfer agents.

[0044] The upper part of the tower body 11 has a gas phase outlet 115, a reflux inlet 116 and a side line outlet 117 which are connected to the side line production area 10a. The gas phase outlet 115 is located at the bottom of the tower body 11. The side line outlet 117 is higher than the above-mentioned first feed port 112, and there are at least three tower plates 111 in the area between the side line outlet 117 and the first feed port 112. The side line outlet 117 is connected to the intermediate product production pipeline 16, and the intermediate product production pipeline 16 is installed with a first delivery pump 161 that can output materials from the side line outlet 117 of the tower reactor 1.

[0045] A stirrer 121 is installed in the tower kettle 12, and the bottom of the tower kettle 12 has a reaction liquid outlet 122 that is connected to the third reaction zone 10d. In this embodiment, the stirrer is a bottom-entry multi-stage propeller stirrer. The viscosity of the reaction system in the tower kettle 12 is relatively high, and the design of the stirrer 121 can ensure good mixing between the feed monomer and the high-viscosity monomer-polymer mixture in the kettle. In addition, the outside of the tower kettle 12 adopts a cooling coil structure, and the cooling coil structure is provided with a cooling water inlet and outlet.

[0046] The gas phase inlet of the condenser 2 is connected to the gas phase outlet 115 of the tower reactor 1 .

[0047] The side of the reflux tank 3 has a first liquid phase inlet connected to the liquid phase outlet of the condenser 2 and a second liquid phase inlet for feeding the reaction monomers, a first liquid phase outlet for discharging the heavy components at the bottom, and a second liquid phase outlet for discharging the light components (non-condensable gas or small molecule gas) at the top. The first liquid phase outlet is connected to the reflux inlet 116 through the reflux line 31, connected to the first feed port 112 through the first reaction monomer feed line 32, connected to the second feed port 113 through the second reaction monomer feed line 33, and connected to the third feed port 114 through the third reaction monomer feed line 34. In addition, a subcooler 322 capable of cooling the material of the first reaction monomer feed line 32 is installed on the first reaction monomer feed line 32, so that after the material passes through the subcooler 322 and enters the first feed port 112, the plate temperature at the first feed port 112 is at least 2°C higher than the temperature of the previous plate.

[0048] The material inlet of the devolatilizing extruder 4 is connected to the reaction liquid outlet 122 of the tower reactor 1, and the devolatilizing extruder 4 can remove the residual monomers in the reaction liquid. A second delivery pump 41 is installed between the material inlet of the devolatilizing extruder 4 and the reaction liquid outlet 122 of the tower reactor 1, which can deliver the material from the reaction liquid outlet 122 of the tower reactor 1 to the material inlet of the devolatilizing extruder 4. In this embodiment, the first delivery pump 161 and the second delivery pump 41 are both gear pumps.

[0049] In addition, in order to conveniently adjust the flow rate of the reaction monomers and auxiliary agents fed into the tower reactor 1, thereby controlling the monomer conversion rate of each reaction zone, the first auxiliary agent feeding pipeline 13 is equipped with a first flow regulating valve 131 capable of controlling the flow rate of the first auxiliary agent feeding pipeline 13, the second auxiliary agent feeding pipeline 14 is equipped with a second flow regulating valve 141 capable of controlling the flow rate of the second auxiliary agent feeding pipeline 14, and the third auxiliary agent feeding pipeline 15 is equipped with a third flow regulating valve 151 capable of controlling the flow rate of the third auxiliary agent feeding pipeline 15; the first reaction monomer feeding pipeline 32 is equipped with a fourth flow regulating valve 321 capable of controlling the flow rate of the first reaction monomer feeding pipeline 32, the second reaction monomer feeding pipeline 33 is equipped with a fifth flow regulating valve 331 capable of controlling the flow rate of the second reaction monomer feeding pipeline 33, and the third reaction monomer feeding pipeline 34 is equipped with a sixth flow regulating valve 341 capable of controlling the flow rate of the third reaction monomer feeding pipeline 34. In addition, a flow regulating valve (not shown in the figure) is also provided at the first liquid phase outlet at the bottom of the reflux tank 4 to facilitate control of the ratio of the reflux flow rate and the flow rate entering the feed port.

[0050] In order to facilitate the sufficient mixing of the reaction monomers and the auxiliary agents, the first auxiliary agent feeding pipeline 13 and the first reaction monomer feeding pipeline 32 at least partially share the same pipeline, the second auxiliary agent feeding pipeline 14 and the second reaction monomer feeding pipeline 33 at least partially share the same pipeline, and the third auxiliary agent feeding pipeline 15 and the third reaction monomer feeding pipeline 34 at least partially share the same pipeline.

[0051] In addition, the above-mentioned polymethyl methacrylate production device can also be used as a pre-reactor for products with higher requirements. Accordingly, at least one reactor for continuing the reaction can be connected after the tower reactor 1. For example, to prepare a certain PMMA composite material, a fully mixed kettle reactor with a stirrer can be connected after the tower reactor 1 through a pipeline. After prepolymerization in the tower reactor 1 and removal of impurities such as dimers, the polymethyl methacrylate is extracted from the bottom of the tower and enters the fully mixed kettle reactor. In this reactor, the PMMA copolymer is mixed with other additives for reaction. After the reaction is complete, it enters the devolatilization extruder to remove and recover the remaining unreacted monomers, and finally extrusion granulation is performed to prepare a certain PMMA composite material with special properties.

[0052] The invention also discloses a polymethyl methacrylate production process using the polymethyl methacrylate production device.

[0053] The amount of the additive added is determined by the monomer feed amount at the corresponding feed port and the feed tray temperature. In the following examples, the selected substances and amounts of the reaction monomers, initiators and chain transfer agents are shown in Table 1.

[0054] Table 1:

[0055] Components Selected materials Dosage (kg / hour) Main monomer MMA 3550 Monomers of copolymers MA 187 Initiator Di-tert-Amyl Peroxide 0.71 Chain transfer agent Dodecyl mercaptan 6.0

[0056] Embodiment 1:

[0057] (1) The main monomer and the copolymer monomers are continuously fed into the reflux tank 3, the first flow regulating valve 131 and the fourth flow regulating valve 321 are opened, the monomer flow rate is controlled to be 1550 kg / h, the initiator flow rate is controlled to be 0.71 kg / h, the initiator and the reaction monomer are mixed and fed into the tower reactor 1 through the first feed port 112, and polymerization begins in the first reaction zone 10b;

[0058] (2) When the conversion rate reaches 30-40%, the fifth flow regulating valve 331 is opened to control the monomer flow rate to 1200 kg / h, and the reaction monomer is fed into the tower reactor 1 through the second feed port 113, mixed with the reaction liquid preliminarily polymerized in the first reaction zone 10b, and repolymerized in the second reaction zone 10c;

[0059] (3) When the conversion rate reaches 60-80%, the second flow regulating valve 141 is opened to control the flow rate of the chain transfer agent to 2.0 kg / h, and the chain transfer agent is fed into the tower reactor 1 through the second feed port 113 to control the molecular weight of the polymer in the reaction system;

[0060] (4) When the reaction liquid enters the third reaction zone 10d, the third flow regulating valve 151 and the sixth flow regulating valve 341 are opened to control the monomer flow rate to 800 kg / h and the chain transfer agent flow rate to 4.0 kg / h. The chain transfer agent and the reaction monomer are mixed and fed into the tower reactor 1 through the third feed port 114 to mix with the reaction liquid after repolymerization in the second reaction zone 10c. Final polymerization is carried out in the third reaction zone 10d, and the polymerization rate reaches more than 90%;

[0061] (5) The volatilized monomers in the tower reactor 1 are discharged from the gas phase outlet 115 and condensed by the condenser 2 before entering the reflux tank 3. The recovered monomers after removing the light components are mixed with the monomers continuously fed from the outside, and are drawn out from the bottom of the tank and divided into four streams. One stream is returned to the tower reactor 1 through the reflux inlet 116 as reflux, and the other three streams are respectively fed into the tower reactor 1 through the first feed inlet 112, the second feed inlet 113 and the third feed inlet 114;

[0062] (6) The intermediate product in the tower reactor 1 condenses at the tray 111 near the side line outlet 117 and is discharged through the side line outlet 117 under the action of the first delivery pump 161;

[0063] (7) The PMMA primary product that has completed polymerization in the reactor 12 is continuously pumped out from the reaction liquid outlet 122 under the action of the second delivery pump 41, and is sent to the devolatilization extruder 4 for further devolatilization, and finally extruded into granules.

[0064] The finished product of this embodiment produces 2050 kg per hour, recovers 1630 kg of monomer, and a small amount of impurities are discharged through the side line outlet 117 of the tower body 11. The finished product is clear and transparent granules, and the physical property test results are shown in Table 2 below:

[0065] Table 2:

[0066]

[0067] Embodiment 2:

[0068] The difference from Example 1 is that:

[0069] In step (1), the monomer flow rate is controlled to be 1200 kg / h, and the initiator flow rate is controlled to be 0.5 kg / h;

[0070] In step (2), the monomer flow rate is controlled to be 1600 kg / h;

[0071] In step (3), the chain transfer agent flow rate is controlled to be 4.0 kg / h;

[0072] In step (4), the monomer flow rate is controlled to be 600 kg / h, and the chain transfer agent flow rate is controlled to be 2.0 kg / h.

[0073] The other conditions remain the same as those in Example 1.

[0074] The finished product of this embodiment produces 2060 kg per hour, 1670 kg of monomer is recovered, and a small amount of impurities are discharged through the side line outlet 117 of the tower body 11. The finished product is clear and transparent granules, and its physical properties are shown in Table 3 below:

[0075] Table 3:

[0076]

[0077] Embodiment 3:

[0078] The difference from Example 1 is that:

[0079] In step (1), the monomer flow rate is controlled to be 1000 kg / h, and the initiator flow rate is controlled to be 0.4 kg / h;

[0080] In step (2), the monomer flow rate is controlled to be 800 kg / h;

[0081] In step (3), the chain transfer agent flow rate is controlled to be 4.5 kg / h;

[0082] In step (4), the monomer flow rate is controlled to be 1500 kg / h, and the chain transfer agent flow rate is controlled to be 1.5 kg / h.

[0083] The other conditions remain the same as those in Example 1.

[0084] The finished product of this embodiment produces 2055 kg per hour, 1675 kg of monomer is recovered, and a small amount of impurities are discharged through the side line outlet 117 of the tower body 11. The finished product is clear and transparent granules, and its physical properties are shown in Table 4 below:

[0085] Table 4:

[0086]

[0087] The present invention adopts a tower reactor to replace the traditional process of multi-stage fully mixed kettle reactors in series, which simplifies the process equipment and reduces the energy consumption in the production process. It can be seen from the above test results that the PMMA product prepared in the embodiment of the present invention meets the requirements of optical grade PMMA material, with a molecular weight distribution index of ≤2.0 and a transmittance of ≥90%.

[0088] The working principle of the present invention is as follows:

[0089] (1) The factors that affect the light transmittance of PMMA materials are mainly the molecular weight distribution of the polymer and the purity of the product. PMMA with a narrow molecular weight distribution has a higher molecular weight uniformity and can improve the overall light transmittance. The light transmittance of PMMA with a molecular weight below 10,000 can reach 93%. Optical fibers made of PMMA with a narrow molecular weight distribution have lower light loss during transmission, which can reach 167dB / km. The higher the purity of the product, the better its light transmittance. The refractive index of PMMA products with a purity of more than 95% can reach 1.6;

[0090] The methods for controlling the molecular weight distribution of polymers are mainly temperature gradient control and feeding mode regulation. In view of these two aspects, the present invention adopts the method of combining the reaction zones in the same tower reactor. The tower reactor is divided into four zones from top to bottom according to the temperature distribution and the degree of reaction during the reaction. They are named as the side line extraction zone, the first reaction zone, the second reaction zone and the third reaction zone. The polymerization process is carried out from top to bottom at different plates of the same tower body. The reaction temperature changes gently in a step-like manner. The temperature distribution in the reaction zone is 80°C to 230°C. Specifically, the temperature of the plate at the first feed inlet is 80 to 120°C. The reaction monomers flow downward and Start polymerization. After flowing through 9 to 10 plates, the monomer conversion rate reaches about 40%, and enters the second reaction zone. The reaction temperature of the second reaction zone is set at 140 to 170°C. The reaction monomers and additives are continuously added through the second feed port in this area to control the reaction system to continue polymerization. After flowing through 10 to 12 plates, the system enters the third reaction zone in the tower kettle 12. At this time, the reaction liquid conversion rate reaches 60% to 80%, the system viscosity increases, and the temperature of the third reaction zone 10d is controlled at 180 to 230°C. The reaction liquid completes the polymerization process in this area. Each reaction zone is provided with a cold monomer feed port. The flow rate and mass of the cold monomer entering each reaction zone are controlled by a flow regulating valve. The cold monomer absorbs a large amount of reaction heat after mixing with the reaction system. Combined with the cooling and reflux of the monomer at the top of the tower, a large amount of reaction heat is taken away, so that the reaction temperature remains stable and the temperature in the reactor can be controlled by the amount of cold monomer added;

[0091] The addition of auxiliary agents also has a huge impact on the polymerization process of PMMA: the addition of initiator generates a small amount of chain free radicals, which quickly initiates the polymerization of MMA monomers, and can greatly shorten the polymerization reaction time; the addition of chain transfer agent transfers the active center of PMMA polymerization reaction from the active chain (growth chain) to other compounds, which can effectively control the chain length of the polymer, that is, control the molecular weight distribution of the polymer. The initiator used in the present invention is di-tert-amyl peroxide, which is mixed with the reaction monomer at a ratio of about 1 / 5000 at the feed port of the first reaction zone and enters the reactor. After being heated, the -OO- bond breaks and splits into two corresponding free radicals, thereby initiating the polymerization of MMA monomers. Chain transfer agent needs to be added to the feed ports of the second reaction zone and the third reaction zone, and the amount added is adjusted according to the required polymer molecular weight. The chain transfer agent used in the present invention is 0.3wt% dodecyl mercaptan, which is added continuously by adjusting the flow valve to control the speed and flow of adding dodecyl mercaptan, and the molecular weight of PMMA is regulated to be 80000-100000, and the molecular weight distribution index is 1.8. The PMMA product under this molecular weight distribution has good optical properties.

[0092] (2) Purity is also an important indicator for measuring the optical properties of PMMA. Low-purity PMMA products usually contain some oligomer impurities. These impurities make PMMA yellow or even produce black spots, which greatly affects the optical properties of PMMA.

[0093] In order to obtain PMMA products with higher purity, it is necessary to find a way to remove the dimer impurities generated during the polymerization process and the low-boiling substances such as the unreacted monomers mixed in the polymer. In view of this, the present invention performs bulk polymerization in a tower reactor. The multi-stage tower plates increase the surface area of ​​the materials in the reaction system, so that most of the small molecular oligomers or unreacted monomers in each reaction area are rapidly volatilized and removed from the reaction system. The volatilized monomers are collected from the bottom to the top of the tower body, pass through the reaction area, and enter the side line extraction area at the top of the tower. After condensation by the top condenser, they are condensed in layers at the top of the tower according to their boiling points. Impurities such as oligomers with higher boiling points are condensed and precipitated first, and their boiling points are 5 to 10°C lower than the reaction temperature of the first reaction zone. Therefore, the side line extraction port is set at least three tower plates on the first reaction zone to ensure the removal effect of impurities. The reaction monomers with lower boiling points carry a large amount of reaction heat in the system, exchange heat with the top condenser, and then enter the reflux tank through the pipeline, mix with the continuously added reaction monomers, and participate in the circulation reaction;

[0094] In order to achieve a better removal effect, the present invention sets a supercooler in front of the first feed port pipe at the top of the tower body, so that the monomers entering the reactor through this feed port are supercooled before entering the reactor. This part of the supercooled monomers has a supercooling degree of 6 to 7°C, and its gasification rate is greatly reduced, so that the side line extraction area and the first reaction area have a temperature mutation point. The temperature of the side line extraction area is lower than the polymerization temperature of the monomer and the active temperature of the catalyst, and the feed port is located 3 to 5 plates below the side line extraction port, which ensures that the reaction monomers after entering the reactor basically flow downward to participate in the polymerization reaction; the unidirectional flow of the monomers and the addition of no auxiliary agent in the side line extraction area form a non-reactive zone at the top of the tower, which is the above-mentioned side line extraction area. This measure helps the monomers collected at the top of the tower not to polymerize, and re-participate in the reaction after condensation, while impurities such as dimers with higher boiling points are directly condensed and precipitated in the side line extraction area and removed through the side line extraction port.

Claims

1. A process for producing polymethyl methacrylate, Features: The polymethyl methacrylate production process is applied with a polymethyl methacrylate production device, and the polymethyl methacrylate production device includes: A tower reactor (1), wherein the side line inlet comprises a first feed port (112), a second feed port (113) and a third feed port (114) which are arranged in a spaced manner from top to bottom, wherein the first feed port (112), the second feed port (113) and the third feed port (114) are respectively connected to a first auxiliary agent feeding pipeline (13), a second auxiliary agent feeding pipeline (14) and a third auxiliary agent feeding pipeline (15), and the inner cavity of the tower reactor (1) is divided into a first auxiliary agent feeding pipeline (13), a second auxiliary agent feeding pipeline (14) and a third auxiliary agent feeding pipeline (15). The side-line extraction zone (10a), the first reaction zone (10b), the second reaction zone (10c) and the third reaction zone (10d) are arranged in sequence below, the upper part of the tower reactor (1) has a gas phase outlet (115), a reflux inlet (116) and a side-line extraction outlet (117) which are connected to the side-line extraction zone (10a), and the lower part of the tower reactor (1) has a reaction liquid outlet (122) which is connected to the third reaction zone (10d); A condenser (2), whose gas phase inlet is connected to the gas phase outlet (115) of the tower reactor (1); as well as A reflux tank (3) having a first liquid phase inlet connected to the liquid phase outlet of the condenser (2) and a second liquid phase inlet for feeding reaction monomers, having a first liquid phase outlet for discharging heavy components and a second liquid phase outlet for discharging light components, wherein the first liquid phase outlet is connected to the reflux inlet (116) via a reflux line (31), connected to the first feed port (112) via a first reaction monomer feed line (32), connected to the second feed port (113) via a second reaction monomer feed line (33), and connected to the third feed port (114) via a third reaction monomer feed line (34); The polymethyl methacrylate production process comprises the following steps: (1) continuously feeding the reaction monomers into a reflux tank (3), mixing the initiator and the reaction monomers, and feeding them into a tower reactor (1) through a first feed port (112), and starting polymerization in a first reaction zone (10b); (2) When the conversion rate reaches 30-40%, the reaction monomer is fed into the tower reactor (1) through the second feed port (113), mixed with the reaction liquid preliminarily polymerized in the first reaction zone (10b), and repolymerized in the second reaction zone (10c); (3) When the conversion rate reaches 60-80%, a chain transfer agent is fed into the tower reactor (1) through the second feed port (113) to control the molecular weight of the polymer in the reaction system; (4) When the reaction liquid enters the third reaction zone (10d), the chain transfer agent and the reaction monomer are mixed and fed into the tower reactor (1) through the third feed port (114), mixed with the reaction liquid that has undergone repolymerization in the second reaction zone (10c), and final polymerization is carried out in the third reaction zone (10d); (5) The volatilized monomers in the tower reactor (1) are discharged from the gas phase outlet (115), condensed by the condenser (2), and then enter the reflux tank (3). After stratification in the reflux tank (3), the monomers are recombined into four streams, one of which is returned to the tower reactor (1) through the reflux inlet (116) as reflux, and the other three streams are respectively fed into the tower reactor (1) through the first feed inlet (112), the second feed inlet (113), and the third feed inlet (114); (6) The intermediate product in the tower reactor (1) is discharged through the side line outlet (117).

2. The polymethyl methacrylate production process according to claim 1, Features: The tower reactor (1) comprises a tower body (11) and a tower kettle (12) connected to the bottom of the tower body (11), and a plurality of tower plates (111) arranged alternately from top to bottom are installed in the tower body (11).

3. The polymethyl methacrylate production process according to claim 2, Features: The tower plate (111) is arranged inclined.

4. The polymethyl methacrylate production process according to claim 2, Features: The side line production port (117) is higher than the first feed port (112), and there are at least three tower plates (111) in the area between the side line production port (117) and the first feed port (112).

5. The polymethyl methacrylate production process according to claim 1, Features: The first auxiliary agent feeding pipeline (13) is equipped with a first flow regulating valve (131) capable of controlling the flow of the first auxiliary agent feeding pipeline (13); the second auxiliary agent feeding pipeline (14) is equipped with a second flow regulating valve (141) capable of controlling the flow of the second auxiliary agent feeding pipeline (14); and the third auxiliary agent feeding pipeline (15) is equipped with a third flow regulating valve (151) capable of controlling the flow of the third auxiliary agent feeding pipeline (15); The first reaction monomer feeding pipeline (32) is installed with a fourth flow regulating valve (321) capable of controlling the flow of the first reaction monomer feeding pipeline (32), the second reaction monomer feeding pipeline (33) is installed with a fifth flow regulating valve (331) capable of controlling the flow of the second reaction monomer feeding pipeline (33), and the third reaction monomer feeding pipeline (34) is installed with a sixth flow regulating valve (341) capable of controlling the flow of the third reaction monomer feeding pipeline (34).

6. The polymethyl methacrylate production process according to claim 1, Features: The first auxiliary agent feeding pipeline (13) and the first reaction monomer feeding pipeline (32) at least partially share the same pipeline, the second auxiliary agent feeding pipeline (14) and the second reaction monomer feeding pipeline (33) at least partially share the same pipeline, and the third auxiliary agent feeding pipeline (15) and the third reaction monomer feeding pipeline (34) at least partially share the same pipeline.

7. The polymethyl methacrylate production process according to claim 1, Features: The first reaction monomer feeding pipeline (32) is provided with a subcooler (322) capable of cooling the material in the first reaction monomer feeding pipeline (32).

8. The process for producing polymethyl methacrylate according to any one of claims 1 to 7, Features: It also includes a devolatilization extruder (4) for removing residual monomers in the reaction liquid, and the material inlet of the devolatilization extruder (4) is connected to the reaction liquid outlet (122) of the tower reactor (1).

9. The process for producing polymethyl methacrylate according to any one of claims 1 to 7, Features: In step (1), the monomer flow rate is controlled to be 1000-1550 kg / h, and the initiator flow rate is controlled to be 0.4-0.71 kg / h; In step (2), the monomer flow rate is controlled to be 800-1600 kg / h; In step (3), the chain transfer agent flow rate is controlled to be 2 to 4.5 kg / h; In step (4), the monomer flow rate is controlled to be 600-1500 kg / h, and the chain transfer agent flow rate is controlled to be 1.5-4 kg / h.